Nickel-based superalloy and manufacturing method thereof

Through vacuum induction + electroslag remelting and smelting and fine annealing and drawing processes, the grain structure of GH4080A alloy was controlled, and the problem of uneven grain growth of GH4080A material after high temperature solid solution was solved, achieving level 6 to 8 Acquisition of fine-grained structures and excellent mechanical properties of the alloy.

CN118957322APending Publication Date: 2024-11-15SUZHOU JICUI GAOHE MATERIAL TECH CO LTD
View PDF 0 Cites 5 Cited by

Patent Information

Application Number
CN202310541571.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-15
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the GH4080A materials for high-temperature fasteners and valves, it is difficult to control the fine crystal structure after hot or cold processing, especially when the high-temperature solution at 1060-1080℃, the grains are prone to grow unevenly and cannot be thicker than that of the grains. The fine crystal structure requirements of level 6 affect the high temperature mechanical properties and life of the alloy.

Method used

Steel ingots were prepared by vacuum induction + electroslag remelting smelting. After hot processing, the blank is opened and hot rolled into wire rods, softening annealing, cold drawing, stress removal annealing and standard solid solution process are processed to control the Al+Ti content To affect the dissolution temperature and peak temperature of the γ' phase, ensure the fineness and uniformity of the grain structure.

Benefits of technology

Through this method, the grain structure of nickel-based high-temperature alloy reaches 6 to 8 fine crystals after 8 hours of insulation at 1060 to 1080°C. After aging, it has good tensile strength, yield strength and elongation, ensuring that the alloy is at high temperature. Performance stability and lifespan under conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957322A_ABST
    Figure CN118957322A_ABST
Patent Text Reader

Abstract

According to the nickel-based superalloy and the manufacturing method thereof, a vacuum induction (VIM) and electroslag remelting (ESR) smelting mode is adopted for the alloy, the Al + Ti component content is reasonably controlled, the structure is stabilized by combining a special annealing process treatment means before and after cold drawing of a wire and a bar, and after heat preservation is conducted for 8 hours at the temperature of 1060-1080 DEG C, the nickel-based superalloy is subjected to standard solid solution process treatment of discharging and air cooling, the nickel-based superalloy is obtained. And the grain structure is a 6-8-grade fine grain structure, meets the structure requirement, and meets the performance requirement after being subjected to the standard aging process treatment of 845 DEG C heat preservation for 24 h / air cooling and 700 DEG C heat preservation for 16 h / air cooling. The method has the characteristics of low segregation, high purity and low gas content; non-metallic inclusions are less than or equal to grade 1; the oxygen content is smaller than or equal to 10 ppm, the nitrogen content is smaller than or equal to 30 ppm, the tensile strength Rm is larger than or equal to 1300 MPa, the yield strength Rp0.2 is larger than or equal to 800 MPa, the ductility A5 is larger than or equal to 25%, and the area reduction Z is larger than or equal to 35%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of high-temperature alloy material processing and manufacturing, and in particular relates to a method for manufacturing a fine-grained nickel-based high-temperature alloy cold-drawn wire rod. Background Art

[0002] High-temperature alloys have become indispensable materials for key components in aviation, aerospace, nuclear power, petrochemical and other industrial fields that withstand harsh operating environments such as high temperature, corrosion, and long-term loads due to their excellent comprehensive properties. GH4080A alloy is a nickel-based high-temperature alloy strengthened by γ´(Ni3(Al ,Ti)) phase. It has good high-temperature strength at 700℃~800℃ and good oxidation resistance below 850℃. GH4080A materials are widely used in advanced aircraft engines, steam turbines, internal combustion engines and other major equipment, including key components such as high-temperature fasteners and valves. The quality of this alloy determines the safety of the above-mentioned major equipment to a certain extent.

[0003] For GH4080A materials used for high-temperature fasteners and valves, after the standard solution treatment of 1060-1080℃ insulation for 8h / air cooling, it is still required to maintain a fine-grained structure with a grain size not coarser than level 6, and then after the standard aging treatment of 845℃ insulation for 24h / air cooling + 700℃ insulation for 16h / air cooling, the parts can achieve the best comprehensive mechanical properties to ensure their performance stability and life reliability under high-temperature service conditions. However, after hot or cold processing, when the alloy undergoes a solution treatment at a higher temperature for a long time, it is difficult to control the fine grains, especially when the solution temperature is higher than 1060℃, the grains are prone to uneven growth for a long time of insulation, and even abnormal grain coarsening, which significantly deteriorates the performance of the alloy. The raw material bars for high-temperature fasteners and valves are relatively small in size and are mainly formed by cold drawing from hot-rolled bars or coils. Due to the uneven cold deformation of the cross section and the high internal cold deformation storage energy, they are more likely to have mixed crystal / coarse crystal and other structural unevenness problems during high-temperature solution at 1060-1080°C, and cannot meet the fine grain structure requirements of no coarser than level 6.

[0004] Patent CN111187934B discloses a production method for GH4080A wire rods, specifically a manufacturing process for cold-drawn coils, which involves a short-term solid solution heat treatment of 1060°C × 1h / air cooling after cold drawing of the wire rods. In essence, the fineness of the grains is ensured by lowering the solid solution temperature and greatly shortening the holding time. The control level of the grain structure is not mentioned in detail in the invention content, and the influence of holding the solid solution temperature above 1060°C for 8 hours on the grain size and the control method are not included.

[0005] Patents CN112359302B and CN112813292A respectively disclose a method for homogenizing the microstructure of a nickel-based high-temperature alloy flat steel and a method for manufacturing a fine-grained NiCr20TiAl alloy forging material, both of which involve a process for obtaining 3-6-grade and not coarser-than-grade 5-grade grains after hot-rolled or forged hot-processed GH4080A (i.e., NiCr20TiAl) material is subjected to a solid solution treatment at 1050-1080°C for 8 hours / air cooling. Patent CN109985926A discloses a method for producing nickel-based GH4080A alloy wire rods, which involves an online solid solution treatment of 1020-1060°C for 6-10 minutes / water cooling for hot-rolled GH4080A hot-processed coils to effectively control the grain level and range problem. Patent CN113122750A discloses a heat treatment process for a nickel-based high-temperature alloy, which involves adjusting the standard heat treatment system of the GH4080A alloy, especially shortening the high-temperature solution treatment time from 8 hours to 4 to 6 hours, so as to achieve the goal of controlling the grain size within level 3. The above-mentioned processes all involve the control process of the grain structure of the GH4080A hot-processed material after high-temperature solution treatment, and do not involve the fine grain control method of the cold-drawn wire rod material after high-temperature solution treatment, and the control level does not meet the fine grain requirement of not coarser than level 6.

[0006] According to the conventional manufacturing method, the GH4080A wire rod that has been cold drawn before high-temperature solution treatment has large deformation storage energy and internal cold deformation non-uniformity. After a long-term solution treatment at 1060-1080℃ for 8h / air cooling, the grains will grow unevenly and rapidly, and it is impossible to obtain a fine-grained structure not coarser than level 6. By lowering the solution temperature to the lower limit of 1060℃ and significantly shortening the holding time to no more than 1 hour, the grain structure of the cold-drawn wire rod can be controlled to be relatively fine, but this technology cannot fully dissolve the material, and the alloy parts after aging cannot achieve the best comprehensive performance, especially sacrificing the high-temperature mechanical properties of the material, which will seriously affect the safety and life of the alloy during service. Summary of the invention

[0007] In order to overcome the shortcomings of the prior art, the present invention provides a method for manufacturing a fine-grained nickel-based high-temperature alloy, which enables the nickel-based high-temperature alloy to achieve a 6-8 grade fine-grained structure after being treated by a standard solid solution process of 1060-1080°C for 8 hours and air cooling. The specific technical scheme of the present invention is as follows: A method for manufacturing a nickel-based high-temperature alloy comprises the following steps: Step 1: A steel ingot is prepared by a smelting method of vacuum induction + electroslag remelting, wherein at the initial stage and melting period of the vacuum induction furnace, 0.035wt% carbon is laid as the bottom, Ni is added until melting is complete, and then metal Cr is added for melting and refining. After refining, B, Ti and Al are added, and after stirring and clearing, samples are taken to determine the composition, and the composition is adjusted. After the composition is qualified, argon is filled at not less than 30000 Pa, and Ni-Mg alloy is added for complete reaction, and then the steel is tapped and a vacuum ingot is cast; the vacuum ingot is electroslag remelted under argon protection conditions, with a melting rate of 3-5kg / min and an argon flow rate of 10-50L / min; Step 2: hot-processing the steel ingot obtained in step 1 to form a blank, and forging it into a hot-rolled square billet; after the square billet is polished, hot-rolled into a wire rod, and the steel ingot is used to produce a hot-rolled wire rod blank required for manufacturing cold-drawn materials; Step 3: Softening annealing treatment, annealing the hot-rolled wire rod obtained in step 2, the specific annealing process is: T1 insulation 1 to 2 hours / water cooling, furnace loading method: warm loading furnace; where T1 = 950℃ + 30℃ × (wt (Al+Ti) %-3.5%) / 0.8%, there is a specific annealing temperature point in this step, because it is related to the dissolution start temperature of the γ' phase, and the dissolution start temperature of the γ' phase is determined by the Al+Ti composition; Step 4: Lubricate the wire rod blank obtained in step 3, and then pass it through the drawing die of the cold drawing machine to reduce the diameter and cold deform, and the cold drawing deformation is controlled at 10-15%; Step 5: Stress relief annealing treatment, annealing the cold drawn wire rod obtained in step 4, the annealing process is: T2 insulation 3 to 5 hours / water cooling, charging method: charging temperature is lower than 500℃, and the temperature rises with the furnace; where T2=1010℃-30℃×(4.3%-wt (Al+Ti) %) / 0.8%, and there is also a specific annealing temperature point in this step, because it is related to the peak dissolution temperature of the γ' phase, and the peak dissolution temperature of the γ' phase is determined by the Al+Ti composition; Step 6: The wire rod obtained in step 5 is subjected to standard solution heat treatment. The solution heat treatment process is: T3 is kept for 8 hours and then taken out of the furnace for air cooling. The furnace loading method is: the furnace is loaded at the temperature; wherein T3 = 1070℃ + 20℃ × (wt (Al+Ti) %-3.9%) / 0.8%, there is a specific solution temperature point in this step, T3 is in the range of 1060~1080℃.

[0008] Furthermore, the method further comprises step 7: straightening the wire rod obtained in step 6 to meet the straightness requirement of polishing, and the wire rod after straightening is ground by a rough grinding-fine grinding method, and the total grinding allowance is controlled at 0.5-0.8 mm.

[0009] Preferably, the steel ingot obtained in step 1 has the following contents, calculated by mass fraction: C: 0.05-0.07%, Si: ≤0.2%, Mn: ≤0.2%, P: ≤0.008%, S: ≤0.002%, Cr: 19.00-20.5%, Cu: ≤0.1%, Al: 1.2-1.8%, Ti: 2.0-2.7%, Fe: ≤1.0%, Co: ≤0.5%, B: 0.003-0.006% and the balance Ni, and 3.5%≤Al+Ti≤4.3%.

[0010] Furthermore, in step 1, the Mg content added to the Ni-Mg alloy is 0.03wt%.

[0011] A nickel-based high-temperature alloy prepared by the above method has a fine grain structure of level 6 to 8. The alloy material has the characteristics of low segregation, high purity, low gas content, and non-metallic inclusions ≤ level 1.0; oxygen content ≤ 10ppm, and nitrogen content ≤ 30ppm.

[0012] After the alloy is treated by a standard aging process of 845℃ insulation for 24h / air cooling + 700℃ insulation for 16h / air cooling, the tensile strength R m ≥1300MPa, yield strength R p0.2 ≥800MPa, elongation A5≥25%, surface shrinkage Z≥35%.

[0013] The present invention adopts the smelting method of vacuum induction (VIM) + electroslag remelting (ESR), vacuum degassing, refining and atmosphere protection electroslag metallurgy, solidification, to produce low segregation, high purity, low gas content steel ingots; the steel ingots are forged and hot rolled to produce the required hot rolled wire rods through conventional processes. By pre-performing appropriate softening annealing treatment on the hot rolled wire rods, the hardness of the cold drawn blank is reduced by eliminating the hot rolling residual internal stress, and by controlling the cold drawing deformation, the accumulation of internal stress on the surface of the cold drawn wire rods is reduced, so that the cold drawing deformation of the wire rods is moderate and the cross-sectional strain is more uniform, which is conducive to the uniformity of recrystallization of the annealing structure after cold drawing. At the same time, the content of Al+Ti in the alloy is controlled. The content of Al+Ti directly affects the precipitation and dissolution temperature of the γ' phase, and the γ' phase mainly determines the migration of the grain boundary during the annealing process and affects the size of the grains. The Al+Ti content of the alloy composition is controlled at 3.5-4.3%. On the one hand, the starting temperature of γ' phase dissolution is increased to 950~980℃ (the softening annealing temperature before cold drawing is controlled not to exceed the starting temperature of γ' phase dissolution, which is quantitatively determined by the Al+Ti content). The purpose is to soften the alloy at the highest possible temperature before cold drawing to reduce the hardness, and the γ' phase has not yet begun to dissolve to effectively control the grain size; on the other hand, the peak temperature of γ' phase dissolution is increased to 980~1010℃ (the stress relief annealing temperature after cold drawing is controlled not to exceed the peak temperature of γ' phase dissolution, which is quantitatively determined by the Al+Ti content). The purpose is that after cold drawing, the blank obtains a suitable deformation amount, and part of the γ' phase begins to dissolve. Through a longer holding time, the alloy can fully release the internal stress by completing the recrystallization process, while the grain structure will not grow rapidly due to the hindrance of a large amount of undissolved γ' phase. Through the above annealing process and organizational changes of the wire rod before and after cold drawing, the organizational state of the alloy before the standard high-temperature solid solution can be completely stabilized, the grain growth tendency of the alloy during the subsequent high-temperature long-time solid solution treatment of 1060-1080℃ for 8 hours / air cooling can be suppressed, and the occurrence of mixed crystals during abnormal growth can be avoided.

[0014] The beneficial technical effect of the present invention is that after the nickel-based high-temperature alloy is treated by a high-temperature long-time standard solution process of 1060-1080°C insulation for 8 hours / air cooling, and then treated by a standard aging process of 845°C insulation for 24 hours / air cooling + 700°C insulation for 16 hours / air cooling, its grain size can reach level 6-8, and after aging treatment, it also has good toughness and tensile strength R m ≥1300MPa, yield strength R p0.2 ≥800MPa, elongation A5≥ 25%, surface shrinkage Z≥35%. Figure 1 This is a metallographic structure diagram of the nickel-based high-temperature alloy prepared in Example 1 of the present invention; Figure 2This is a metallographic structure diagram of the nickel-based high-temperature alloy prepared in Example 2 of the present invention; Figure 3 This is the metallographic structure diagram of the nickel-based high-temperature alloy prepared in Example 3 of the present invention. Implementation

[0015] The present invention will be further described below with reference to the embodiments.

[0016] The compositions of the electroslag ingots of Examples 1 to 3 of the present invention are shown in Table 1 below.

[0017] element C Si Mn P S Cr Al Ti Fe Cu Co B Ni Al+Ti Requirements (wt%) 0.05-0.07 ≤0.2 ≤0.2 ≤0.008 ≤0.002 19-20.5 1.2-1.8 2.0-2.7 ≤1.0 ≤0.1 ≤0.5 0.003-0.006 Remain 3.5-4.3 Example 1 (wt%) 0.058 0.034 0.082 0.0061 0.001 19.21 1.68 2.54 0.674 0.045 0.042 0.0048 Remain 4.22 Example 2 (wt%) 0.062 0.045 0.078 0.0058 0.001 19.83 1.51 2.42 0.863 0.058 0.023 0.0048 Remain 3.93 Example 3 (wt%) 0.060 0.048 0.097 0.0047 0.001 20.02 1.40 2.23 0.797 0.062 0.054 0.0050 Remain 3.63 Example

[0018] Production of wire rods: First, the steel ingots are produced by the smelting method of vacuum induction (VIM) + electroslag remelting (ESR). GH4080A alloy is melted in a 1-ton vacuum induction furnace, and an electrode rod with a diameter of 290 mm is cast under vacuum conditions. In the second step, the electrode is remelted in an argon-protected electroslag furnace to form an electroslag ingot with a diameter of 400 mm, with a melting rate of 3.5 kg / min and an argon flow rate of 20 L / min. A 5-ton hammer forging machine is then used to forge the electroslag ingot for hot working. The ingot heating temperature is 1160°C, the fire deformation is 30% to 50%, the reheating temperature is 1160°C, and the insulation is 2 hours; the opening forging temperature of the electroslag ingot is ≥1050°C, the final forging temperature is ≥900°C, and a 145×145mm square billet is obtained by forging.

[0019] Billet grinding: 100% of the billets are ground, and then 100% PT inspection is carried out to ensure that there are no defects on the billet surface; at the same time, after the billets are ultrasonically inspected and qualified, the heads and tails are cut off to obtain polished billets for hot rolling with a size of 140×140mm and a single length of about 2500mm.

[0020] Then hot-roll the bars: hot-roll the 140×140mm square billet, the hot-rolling heating temperature is 1170℃±10℃, the start rolling temperature is greater than 1080℃, the hot-rolling specification diameter is 22mm, and the grain size of the bars after hot rolling is grade 8.

[0021] Then, softening annealing: 22mm diameter hot-rolled bars are annealed according to the following process: 977℃ holding for 1 hour / water cooling, charging method: charging the furnace when it reaches temperature.

[0022] Then, cold drawing: the 22mm diameter bar blank is first lubricated, and then reduced to a diameter of 20.6mm through the drawing die of the cold drawing machine, with a cold drawing deformation of 12.3%.

[0023] Stress relief annealing: 20.6mm diameter cold drawn bars are annealed according to the following process: 1007℃ insulation for 3 hours / water cooling, charging method: charging temperature 450℃, heating with the furnace.

[0024] Then carry out solution heat treatment: the annealed cold drawn bars are treated according to the following solution treatment process: 1078℃ insulation for 8 hours / air cooling, charging method: charging the furnace at temperature.

[0025] Finally, straightening / polishing is performed: the 20.6mm diameter cold-drawn bar after solution treatment is straightened and ground to a finished size of 20mm in diameter using a rough grinding + fine grinding method.

[0026] The 20mm diameter cold drawn bar manufactured by the above process is treated by a high temperature long time standard solution treatment of 1078℃ for 8 hours / air cooling. The grain structure is as follows Figure 1 As shown, it is a 6.5-level fine-grained structure. After the standard aging process of 845℃ insulation for 24h / air cooling + 700℃ insulation for 16h / air cooling, the mechanical properties are shown in the following table, and the results of two parallel tests are shown in Table 2, which shows that it has good strength and toughness.

[0027] Table 2: Strength and toughness data of the product obtained in Example 1 after two parallel tests

[0028] Example 2 Production of wire rods: First, the steel ingots are produced by vacuum induction (VIM) + electroslag remelting (ESR) smelting method. GH4080A alloy is melted in a 1-ton vacuum induction furnace, and electrode rods with a diameter of 290 mm are cast under vacuum conditions. In the second step, the electrode is remelted in an argon-protected electroslag furnace to form an electroslag ingot with a diameter of 400 mm, with a melting rate of 4.0 kg / min and an argon flow rate of 30 L / min.

[0029] A 5-ton hammer forging machine is then used to forge the electroslag ingot for hot working. The ingot heating temperature is 1160°C, the deformation amount of the fire is 30% to 50%, the reheating temperature is 1160°C, and the insulation is 2h; the starting forging temperature of the electroslag ingot is ≥1050°C, the final forging temperature is ≥900°C, and a 145×145mm square billet is forged.

[0030] Billet grinding: 100% of the billets are ground, and then 100% PT inspection is carried out to ensure that there are no defects on the billet surface; at the same time, after the billets are ultrasonically inspected and qualified, the heads and tails are cut off to obtain polished billets for hot rolling with a size of 140×140mm and a single length of about 2500mm.

[0031] Then hot rolling the bars: hot rolling the 140×140mm square billet, the hot rolling heating temperature is 1170℃±10℃, the start rolling temperature is greater than 1080℃, the hot rolling specification diameter is 15mm, and the grain size of the bars after hot rolling is level 9.

[0032] Then soften and anneal: 15mm diameter hot-rolled bars are annealed according to the following process: 966℃ insulation for 1.5 hours / water cooling, charging method: charging the furnace when it reaches temperature.

[0033] Next, cold drawing: the 15mm diameter bar blank is first lubricated, and then reduced to 14mm in diameter through the drawing die of the cold drawing machine, with a cold drawing deformation of 12.8%.

[0034] Stress relief annealing: 14mm diameter cold drawn bars are annealed according to the following process: 996℃ insulation for 4 hours / water cooling, charging method: charging temperature 420℃, heating with the furnace.

[0035] Then carry out solution heat treatment: the annealed cold drawn bars are treated according to the following solution treatment process: 1071℃ insulation for 8 hours / air cooling, charging method: charging the furnace at temperature.

[0036] Finally, straightening / polishing: The 14mm diameter cold-drawn bar after solution treatment is straightened and ground to a finished size of 13.5mm in diameter using a rough grinding + fine grinding method.

[0037] The 13.5 mm diameter cold drawn bar manufactured by the above process is treated by a high temperature long time standard solution treatment of 1071℃ for 8 hours / air cooling. The grain structure is as follows Figure 2 As shown, it is a 7.0 grade fine grain structure. After the standard aging process of 845℃ insulation for 24h / air cooling + 700℃ insulation for 16h / air cooling, the mechanical properties of the two parallel tests are shown in Table 3, which has good strength and toughness.

[0038] Table 3: Strength and toughness data of the product obtained in Example 2 after two parallel tests

[0039] Example 3 Production of wire rods: First, the steel ingots are produced by vacuum induction (VIM) + electroslag remelting (ESR) smelting. GH4080A alloy is melted in a 1-ton vacuum induction furnace, and electrode rods with a diameter of 290 mm are cast under vacuum conditions. In the second step, the electrode is remelted in an argon-protected electroslag furnace to form an electroslag ingot with a diameter of 400 mm, with a melting rate of 4.3 kg / min and an argon flow rate of 35 L / min.

[0040] A 5-ton hammer forging machine is then used to forge the electroslag ingot for hot working. The ingot heating temperature is 1160°C, the deformation amount of the fire is 30% to 50%, the reheating temperature is 1160°C, and the insulation is 2h; the starting forging temperature of the electroslag ingot is ≥1050°C, the final forging temperature is ≥900°C, and a 145×145mm square billet is forged.

[0041] Billet grinding: 100% of the billets are ground, and then 100% PT inspection is carried out to ensure that there are no defects on the billet surface; at the same time, after the billets are ultrasonically inspected and qualified, the heads and tails are cut off to obtain polished billets for hot rolling with a size of 140×140mm and a single length of about 2500mm.

[0042] Then hot-roll the bars: hot-roll the 140×140mm square billet, the hot-rolling heating temperature is 1170℃±10℃, the start rolling temperature is greater than 1080℃, the hot-rolling specification diameter is 8mm, and the grain size of the bars after hot rolling is 10 grades.

[0043] Then soften annealing: 8mm diameter hot-rolled bars are annealed according to the following process: 955℃ for 2 hours / water cooling, charging method: charging the furnace when it reaches temperature.

[0044] Then cold drawing: the 8mm diameter bar blank is first lubricated, and then reduced to 7.5mm in diameter through the drawing die of the cold drawing machine, with a cold drawing deformation of 12.1%.

[0045] Stress relief annealing: 7.5mm diameter cold drawn bars are annealed according to the following process: 985℃ insulation for 5 hours / water cooling, furnace charging method: charging temperature 400℃, heating with the furnace.

[0046] Next, solution heat treatment: the annealed cold-drawn bars are treated according to the following solution heat treatment process: 1063℃ insulation for 8 hours / air cooling, charging method: charging the furnace at temperature.

[0047] Finally, straightening / polishing: The 7.5mm diameter cold-drawn bar after solution treatment is straightened and ground to a finished size of 7mm in diameter using a rough grinding + fine grinding method.

[0048] The 7mm diameter cold drawn bar manufactured by the above process is treated by a high temperature long time standard solution treatment of 1063℃ holding for 8 hours / air cooling. The grain structure is as follows Figure 3 As shown, it is a fine-grained structure of level 7.5. After the standard aging process of 845℃ insulation for 24h / air cooling + 700℃ insulation for 16h / air cooling, the two parallel mechanical properties are shown in Table 4, showing good strength and toughness.

[0049] Table 4: Strength and toughness data of the product obtained in Example 3 after two parallel tests

Claims

1. A method for manufacturing a nickel-based high-temperature alloy, characterized in that The following steps are involved: Step 1: A steel ingot is prepared by a smelting method of vacuum induction + electroslag remelting, wherein at the initial stage and melting period of the vacuum induction furnace, 0.035wt% carbon is laid as the bottom, Ni is added until melting is complete, and then metal Cr is added for melting and refining. After refining, B, Ti and Al are added, and after stirring and clearing, samples are taken to determine the composition, and the composition is adjusted. After the composition is qualified, argon is filled at not less than 30000 Pa, and Ni-Mg alloy is added for complete reaction, and then the steel is tapped and a vacuum ingot is cast; the vacuum ingot is electroslag remelted under argon protection conditions, with a melting rate of 3-5kg / min and an argon flow rate of 10-50L / min; Step 2: hot-processing the steel ingot obtained in step 1 to form a blank, and forging it into a hot-rolled square billet; after the square billet is polished, hot-rolled into a wire rod, the steel ingot is used to produce a hot-rolled wire rod blank required for manufacturing cold-drawn materials; Step 3: Softening annealing treatment, annealing the hot-rolled wire rod obtained in step 2, the specific annealing process is: T1 insulation 1 to 2 hours / water cooling, furnace loading method: warm loading furnace; where T1 = 950℃ + 30℃ × (wt (Al+Ti) %-3.5%) / 0.8%; Step 4: Lubricate the wire rod blank obtained in step 3, and then pass it through the drawing die of the cold drawing machine to reduce the diameter and cold deform, and the cold drawing deformation is controlled at 10-15%; Step 5: Stress relief annealing treatment, annealing the cold drawn wire rod obtained in step 4, the annealing process is: T2 insulation 3 to 5 hours / water cooling, charging method: charging temperature is lower than 500℃, and the temperature rises with the furnace; where T2=1010℃-30℃×(4.3%-wt (Al+Ti) %) / 0.8%; Step 6: The wire rod obtained in step 5 is subjected to solution heat treatment. The solution heat treatment process is: T3 is kept at temperature for 8 hours and then taken out of the furnace for air cooling. The furnace loading method is to load the furnace at the temperature; wherein T3 = 1070℃ + 20℃ × (wt (Al+Ti) %-3.9%) / 0.8%.

2. The method for producing a nickel-based high-temperature alloy according to claim 1, characterized in that The method further comprises step 7: straightening the wire rod obtained in step 6 to meet the straightness requirement of polishing, and the wire rod after straightening is ground by a rough grinding-fine grinding method, and the total grinding allowance is controlled within 0.5-0.8 mm.

3. The method for producing a nickel-based high-temperature alloy according to claim 1 or 2, characterized in that The steel ingot prepared in the step 1 has the following contents calculated by mass fraction: C: 0.05-0.07%, Si: ≤0.2%, Mn: ≤0.2%, P: ≤0.008%, S: ≤0.002%, Cr: 19.00-20.5%, Cu: ≤0.1%, Al: 1.2-1.8%, Ti: 2.0-2.7%, Fe: ≤1.0%, Co: ≤0.5%, B: 0.003-0.006% and the balance Ni, and 3.5%≤Al+Ti≤4.3%.

4. The method for producing a nickel-based high-temperature alloy according to claim 3, characterized in that The Mg content added to the Ni-Mg alloy in step 1 is 0.03wt%.

5. A nickel-based high-temperature alloy obtained by the method of claim 1 or 2, characterized in that The obtained alloy grain structure is a fine-grained structure of level 6 to 8.

6. The nickel-based high-temperature alloy according to claim 5, characterized in that It has the characteristics of low segregation, high purity, low gas content, and non-metallic inclusions ≤1 level; oxygen content ≤10ppm, nitrogen content ≤30ppm.

7. The nickel-based high-temperature alloy according to claim 6, characterized in that After the alloy is treated by a standard aging process of 845℃ insulation for 24h / air cooling + 700℃ insulation for 16h / air cooling, the tensile strength R m ≥1300MPa, yield strength R p0.2 ≥800MPa, elongation A5≥25%, surface shrinkage Z≥35%.

Citation Information

Cited By

  • NiCr20TiAl high-temperature alloy rolled material and forming method thereof

    CN120400620A

  • High-performance GH4738 alloy material and preparation method thereof

    CN120758765A

  • Ultrahigh-strength corrosion-resistant high-temperature alloy cold-drawn bar as well as preparation method and application thereof

    CN121272323A

  • High-strength cobalt-nickel-based alloy material and preparation method thereof

    CN121380717A

  • Nicr20tial superalloy rolled product and forming method therefor