High-strength wear-resistant copper alloy and preparation method and application thereof
By regulating the content and proportion of Al, Fe, Ni and Mn in copper alloys, and combining solid solution and aging treatment processes, the shortcomings of existing copper alloys in strength, wear resistance and elongation are solved, and high-performance copper is prepared. Alloys are suitable for mechanical manufacturing, marine and construction fields, achieving high strength, wear resistance and excellent plasticity.
Patent Information
- Application Number
- CN202411020515.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
The existing copper alloys are difficult to meet the high requirements of the machinery manufacturing, marine and construction industries in terms of strength, wear resistance and elongation. The preparation process is complex and the elongation is poor.
By adjusting the content and proportion of Al, Fe, Ni and Mn in the copper alloy, controlling the form and proportion of the alloy's microstructure, combining solid solution and aging treatment processes, a copper alloy with high strength, wear resistance and excellent plasticity was prepared. .
The high tensile strength, yield strength, elongation and hardness of copper alloys are achieved, while reducing wear rate and simplifying the preparation process. It is suitable for mechanical manufacturing, marine and construction fields.
Smart Images

Figure CN118957353A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of copper alloys, and in particular relates to a high-strength wear-resistant copper alloy and a preparation method and application thereof. Background Art
[0002] Aluminum bronze is an important structural material widely used in the field of mechanical industry. Binary aluminum bronze is mainly composed of copper and aluminum elements. Aluminum bronze is widely used in gears, wear-resistant bearings, molds, valves, ships, offshore platform construction materials, etc. due to its high strength, high wear resistance, and high corrosion resistance. It plays a very important role in both civil and military use. In recent years, with the accelerated iteration of product updates and the rapid development of various industries, higher requirements have been placed on the strength, wear resistance and other properties of materials. In order to further improve the strength and wear resistance of the material, scholars in the field usually use microalloying and heat treatment methods to improve it.
[0003] The patent document with the announcement number CN113584343B discloses a corrosion-resistant high-manganese aluminum bronze alloy and its preparation method. The weight percentage composition of the aluminum bronze alloy includes: 7.4-9.4% Al, 0.5-5% Fe, 0.5-5% Ni, 10.1-15% Mn, and the balance is Cu and inevitable impurities. The preparation method is to take each raw material according to the proportion; put the prepared raw materials into a smelting furnace, smelt at 1250-1350°C, and semi-continuously cast at 1150-1270°C after melting to obtain an ingot; hot extrude the obtained ingot to obtain an extruded billet, wherein the extrusion temperature is 700-800°C and the extrusion ratio is 150-350; stretch and anneal the obtained extruded billet online; repeat the hot extrusion process until the desired finished product diameter is reached. The elongation of the alloy prepared by this method is poor, and the wear resistance data of the alloy is not disclosed.
[0004] The patent document with publication number CN114395710A discloses a high-strength corrosion-resistant copper alloy and a preparation method thereof, wherein the alloy composition includes: Al 4.0-10.0wt%, Fe 1.0-4.0wt%, Mn 1.0-4.5wt%, Ni 0.8-3.5wt%, Cr 0.08-0.5wt%, P 0.001-0.05wt%, the sum of inevitable impurities ≤0.15wt%, and the balance is Cu. The preparation method includes casting: casting the raw material into a copper alloy ingot by a semi-continuous casting method; heat treatment: performing perforation hot extrusion, hot extrusion, or hot rolling on the prepared copper alloy ingot; solid solution treatment: performing solid solution treatment on the obtained copper alloy material; cold treatment: performing cold drawing or cold rolling on the copper alloy material after solid solution treatment; straightening: straightening the copper alloy material after cold treatment; finished product annealing: annealing the straightened copper alloy material. This invention improves the mechanical properties, machinability and corrosion resistance of the alloy by adjusting the content of Fe, Ni, Cr and P elements and optimizing the processing technology and heat treatment process. However, the strength of the alloy is relatively low and cannot meet the industry's production requirements for copper alloy performance.
[0005] In summary, it is necessary to find a copper alloy that has high strength, hardness, excellent elongation and low wear rate to meet the needs of machinery manufacturing, shipbuilding and ocean, construction and other industries. Summary of the invention
[0006] The purpose of the present invention is to provide a high-strength wear-resistant copper alloy and a preparation method and application thereof. The high-strength wear-resistant copper alloy of the present invention has high strength, hardness, excellent elongation and low wear rate, and the preparation process is simple, and can be used in machinery manufacturing, shipbuilding, ocean, construction and other fields.
[0007] The first aspect of the present invention provides a high-strength wear-resistant copper alloy, comprising the following components in percentage by mass: Al: 7-11wt%, Fe: 2-5wt%, Ni: 3-6%, Mn: 0.01-2wt%, and the remainder being Cu and unavoidable impurities, wherein the masses of Al, Fe, Ni and Mn satisfy: 0.8≤Al / (Fe+Ni+Mn)≤2 and Ni / (Fe+Mn)≥1.
[0008] The present invention adjusts the content and proportion of Al, Fe, Ni and Mn in the alloy, controls the morphology, distribution and proportion of each phase in the alloy microstructure, thereby obtaining a copper alloy material with high strength, wear resistance, good plasticity and toughness.
[0009] The Al content has an important influence on the performance of aluminum bronze. When the Al content is below 7wt%, the Cu-Al alloy is a single-phase α solid solution structure. At this time, the alloy has good plastic deformation ability, but poor strength and wear resistance. With the increase of Al content, the β phase generated at high temperature will decompose into α+γ2 structure during the cooling process. The γ2 phase has the characteristics of hardness and brittleness, which can significantly improve the strength and wear resistance of the alloy. When the Al content is greater than 11wt%, a large amount of γ2 phase appears in the alloy matrix, the plasticity of the alloy drops sharply, and the application end is limited. Therefore, in order to make the alloy achieve the purpose of high strength, high wear resistance and excellent plasticity in the present invention, the Al content is controlled at 7-11wt%.
[0010] Fe has a certain solid solubility in Cu-Al alloy. When the Fe content is less than 2wt%, a part of Fe is dissolved in the matrix to play a role of solid solution strengthening, and a part of Fe forms Fe-rich phase FeAl3. The Fe-rich phase is first precipitated during solidification, playing the role of heterogeneous nucleation point, thereby refining the grain of the alloy and improving the strength and wear resistance of the alloy, but this effect is relatively small at this time; as the Fe content increases to 2-5wt%, this strengthening effect gradually increases; when the Fe content is greater than 5wt%, a large amount of Fe-rich phase precipitates in needle shape, which seriously reduces the mechanical properties and corrosion resistance of the alloy, and is limited at the application end. Therefore, in order to make the alloy achieve high strength and high wear resistance in the present invention, the Fe content is controlled at 2-5wt%.
[0011] Ni can be solid-dissolved in the aluminum bronze matrix to a limited extent. The addition of Ni element can improve the strength, wear resistance, heat resistance and corrosion resistance of the alloy. By controlling the addition ratio of Ni and Fe, a fine k phase can be formed in the aluminum bronze matrix to improve the mechanical properties of the material. When Ni is less than 3wt%, the less precipitated phase has no significant strengthening effect on the alloy; when the Ni content is greater than 6wt%, the excessive precipitated phase reduces the toughness of the material. Therefore, in order to make the alloy achieve high strength and high wear resistance in the present invention, the Ni content is controlled at 3-6wt%.
[0012] Mn can be dissolved in the α phase of aluminum bronze to improve the alloying degree of the material, and improve the strength, wear resistance and corrosion resistance of the material. However, when the Mn content is greater than 2wt%, the toughness of the material decreases; when the Mn content is less than 0.01wt%, the strength, wear resistance and corrosion resistance of the material are not significantly improved. Therefore, in the present invention, in order to make the alloy achieve high strength and high wear resistance, the Mn content is controlled at 0.01-2wt%.
[0013] In the copper alloy of the present invention, the masses of Al, Fe, Ni and Mn satisfy: 0.8≤Al / (Fe+Ni+Mn)≤2 and Ni / (Fe+Mn)≥1. When the content relationship of Al, Fe, Ni and Mn satisfies 0.8≤Al / (Fe+Ni+Mn)≤2 and Ni / (Fe+Mn)≥1, Al, Fe, Ni and Mn can fully act to generate sufficient quantities of k phase and β+γ2 phase, so that the material has high strength and wear resistance; at the same time, at this ratio, the α phases of the material are connected to each other, and the γ2 phase is precipitated in particles, so that the material has high strength, wear resistance and corresponding plasticity.
[0014] When the content of Al / (Fe+Ni+Mn) is less than 0.8 and Ni / (Fe+Mn) is less than 1, Al, Fe, Ni, and Mn interact to form too much k-phase, and the γ2 phase precipitates in layers. Although the strength and wear resistance are good, the material toughness is poor and difficult to form. When the content of Al / (Fe+Ni+Mn) is greater than 2 and Ni / (Fe+Mn) is less than 1, Al, Fe, Ni, and Mn cannot fully form a k-phase precipitation phase, and the γ2 phase precipitates in layers. Not only is the strength and wear resistance poor, but the plastic deformation ability is also low. Therefore, the present invention limits the content of Al, Fe, Ni, and Mn to 0.8≤Al / (Fe+Ni+Mn)≤2 and Ni / (Fe+Mn)≥1.
[0015] Preferably, the high-strength wear-resistant copper alloy includes at least one of Si and Cr. Si can be dissolved in the α phase in aluminum bronze to improve the strength, wear resistance and corrosion resistance of the material. Cr has a low solubility in aluminum bronze and mainly exists in the alloy in the form of dispersed precipitation phase, which can significantly adjust and refine the grain size and improve the strength and wear resistance of the material.
[0016] Preferably, in the high-strength wear-resistant copper alloy, the mass percentage of Si is 0.01-0.5wt%. When the Si content exceeds 0.5wt%, Si is easy to produce Fe-Si phase, reducing the toughness of the material. When the Si content is lower than 0.01wt%, the strength, wear resistance and corrosion resistance of the material are not significantly improved. Therefore, in the present invention, in order to make the alloy achieve high strength and high wear resistance, the Si content is controlled at 0.01-0.5wt%.
[0017] Preferably, in the high-strength wear-resistant copper alloy, the mass percentage of Cr is 0.01-0.3wt%. When Cr is less than 0.01wt%, the Cr element has an insignificant effect on the grain refinement of the alloy, and the strength and wear resistance of the material are limited. However, when the Cr content is greater than 0.3wt%, the toughness of the material decreases. Therefore, in order to achieve high strength and high wear resistance in the present invention, the Cr content is controlled at 0.01-0.3wt%.
[0018] Preferably, the microstructure of the high-strength wear-resistant copper alloy includes α phase, k phase, β and γ2 phase, wherein the area proportion of each phase is: 87.5%<α phase<96.5%, 0.5%<k phase<2.5%, 3%<β+γ2 phase<10%.
[0019] The α phase is the matrix of the alloy, with high plasticity and easy processing and forming, but low strength and poor wear resistance. The k phase is an intermetallic compound, which is formed by decomposition of a solid solution at high temperature during the cooling process. It is hard and brittle, and can significantly improve the strength and wear resistance of the alloy. The β phase is a residual phase at high temperature, which can improve the strength and wear resistance of the alloy at room temperature. The γ2 phase is the precipitation of the β phase at high temperature during the cooling process. It is hard and brittle, and can significantly improve the strength and wear resistance of the alloy. When 87.5% < α phase < 96.5%, 0.5% < k phase < 2.5%, 3% < β + γ2 phase < 10%, the synergistic effect between the phases ensures that the alloy has high strength and wear resistance, while having a certain toughness.
[0020] Preferably, the tensile strength of the high-strength wear-resistant copper alloy is greater than 850 MPa, the yield strength is greater than 550, the elongation is greater than 8%, the hardness HB is greater than 220, and the wear rate is less than 4.5×10 -6 mm 3 / (N·m).
[0021] The second aspect of the present invention provides a method for preparing the high-strength wear-resistant copper alloy, comprising the following steps: batch smelting + continuous casting → hot extrusion → stretching → solid solution → aging → straightening,
[0022] Wherein, in the aging process, the holding temperature is 420-700°C, the holding time is 1-5h, and after the holding is completed, the furnace is first cooled to 300-350°C and then air-cooled.
[0023] After solution treatment, a supersaturated β-phase solid solution is obtained. The β-phase solid solution undergoes phase transformation through aging treatment to produce α-phase, γ2-phase, and k-phase. By controlling the aging treatment conditions and the proportion of each phase, the strength and wear resistance of the material can be improved.
[0024] During the aging stage, the supersaturated β-phase solid solution is unstable and decomposes to generate α-phase, γ2-phase and K-phase. Since the β-phase has the characteristics of high strength and wear resistance at room temperature, the present invention adopts a step aging process, that is, first furnace cooling to 300-350°C and then air cooling to room temperature, avoiding the complete analysis of the β-phase, so that a part of the β-phase is retained in the copper alloy, thereby further improving the strength and wear resistance of the alloy at room temperature.
[0025] Preferably, in the solutionizing step, the insulation temperature is 750-950° C., the insulation time is 20-90 min, and after the insulation is completed, the mixture is immersed in a sodium chloride aqueous solution to cool.
[0026] The purpose of the solution treatment is to obtain a supersaturated β-phase solid solution. The supersaturated β-phase is an unstable phase. The acquisition of the supersaturated solid solution is related not only to the temperature but also to the cooling intensity. In order to obtain a sufficient supersaturated β-phase, a sodium chloride aqueous solution is used for cooling in the solution treatment process of the present invention.
[0027] Preferably, the concentration of the sodium chloride aqueous solution is 5-10 wt%.
[0028] Preferably, the hot extrusion is as follows: heating the ingot obtained by continuous casting to 650-950° C. and extruding it through an extruder to obtain a billet.
[0029] Preferably, in the stretching step, the processing rate is 5 to 15%.
[0030] The third aspect of the present invention provides the application of the high-strength wear-resistant copper alloy in the fields of machinery manufacturing, shipbuilding, ocean or construction. The copper alloy of the present invention has high strength, wear resistance, good plasticity and toughness, and has broad application prospects in the fields of machinery manufacturing, shipbuilding, ocean, construction and so on.
[0031] Compared with the prior art, the present invention has at least the following beneficial effects:
[0032] The present invention controls the morphology, distribution and proportion of each phase in the alloy microstructure by adjusting the content and proportion of Al, Fe, Ni and Mn in the alloy, and combines the solid solution and aging treatment processes to obtain a copper alloy material with high strength, wear resistance, good plasticity and toughness. The tensile strength of the high-strength wear-resistant copper alloy of the present invention is greater than 850MPa, the yield strength is greater than 550, the elongation is greater than 8%, the hardness HB is greater than 220, and the wear rate is less than 4.5×10 -6 mm 3 / (N·m), can be used in machinery manufacturing, shipbuilding, ocean, construction and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a scanning electron microscope photograph of the copper alloy of Example 2. DETAILED DESCRIPTION
[0034] The present invention is further described in detail below with reference to the embodiments.
[0035] The present invention provides 3 embodiments and 2 comparative examples.
[0036] Example 1
[0037] The copper alloy of this embodiment has the following mass percentage compositions: Al: 7.2wt%, Fe: 2.2wt%, Ni: 3.3wt%, Mn: 1.05%, Cr: 0.27%, and the remainder is Cu and unavoidable impurities.
[0038] 1) Batching and smelting + continuous casting: batching and melting according to the ingredients, and producing ingots through continuous casting.
[0039] 2) Hot extrusion: The ingot is heated to 940°C and extruded into a billet using a horizontal extruder.
[0040] 3) Stretching: The extruded billet is subjected to cold deformation with a processing amount of 6%.
[0041] 4) Solution treatment: The stretched wire blank is subjected to solution treatment at a holding temperature of 770° C. for 90 minutes, and then immersed in a 6 wt % sodium chloride aqueous solution and cooled to room temperature.
[0042] 5) Aging: The wire billet after solid solution is subjected to aging treatment at a holding temperature of 690°C for 4.5 hours, then furnace cooled to 350°C and air cooled to room temperature.
[0043] 6) Straightening: The wire blank after aging treatment is straightened to obtain the finished product.
[0044] Example 2
[0045] The copper alloy has a mass percentage composition of: Al: 10.8wt%, Fe: 2.5wt%, Ni: 3wt%, Mn: 0.02%; Si: 0.45%, and the remainder is Cu and unavoidable impurities.
[0046] 1) Batching and smelting + continuous casting: batching and melting according to the ingredients, and producing ingots through continuous casting.
[0047] 2) Hot extrusion: The ingot is heated to 670°C and extruded into a billet using a horizontal extruder.
[0048] 3) Stretching: The extruded billet is subjected to cold deformation with a processing amount of 14%.
[0049] 4) Solution treatment: The stretched wire blank is solution treated at a temperature of 850° C. for 60 minutes, and then immersed in a 6 wt % sodium chloride aqueous solution and cooled to room temperature.
[0050] 5) Aging: The wire billet after solid solution is subjected to aging treatment at a holding temperature of 580°C for 3 hours, then furnace cooled to 350°C, and then air cooled to room temperature.
[0051] 6) Straightening: The wire blank after aging treatment is straightened to obtain the finished product.
[0052] Example 3
[0053] The copper alloy has a composition in mass percentage of: Al: 9.1wt%, Fe: 4.8wt%, Ni: 5.5%, Mn: 0.15wt%, Si: 0.02wt%, Cr: 0.05wt%, and the remainder is Cu and unavoidable impurities.
[0054] 1) Batching and smelting + continuous casting: batching and melting according to the ingredients, and producing ingots through continuous casting.
[0055] 2) Hot extrusion: The ingot is heated to 850°C and extruded into a billet using a horizontal extruder.
[0056] 3) Stretching: The extruded billet is subjected to cold deformation with a processing amount of 10%.
[0057] 4) Solution treatment: The stretched wire blank is subjected to solution treatment at a holding temperature of 940° C. for 25 minutes, and then immersed in a 6 wt % sodium chloride aqueous solution and cooled to room temperature.
[0058] 5) Aging: The wire billet after solid solution is subjected to aging treatment at a holding temperature of 425°C for 1.5 hours, then furnace cooled to 350°C, and then air cooled to room temperature.
[0059] 6) Straightening: The wire blank after aging treatment is straightened to obtain the finished product.
[0060] Example 4
[0061] The mass percentage composition of the copper alloy is: Al: 10.9wt%, Fe: 3.8wt%, Ni: 5.75%, Mn: 1.85wt%, and the balance is Cu and inevitable impurities.
[0062] 1) Batching and smelting + continuous casting: batching and melting according to the ingredients, and producing ingots through continuous casting.
[0063] 2) Hot extrusion: The ingot is heated to 850°C and extruded in a horizontal extruder to obtain a billet;
[0064] 3) Stretching: cold deformation of the extruded billet by 10%;
[0065] 4) Solution treatment: The stretched wire blank is subjected to solution treatment at a holding temperature of 940° C. for 25 minutes, and then immersed in a 6 wt % sodium chloride aqueous solution and cooled to room temperature.
[0066] 5) Aging: The wire billet after solid solution is subjected to aging treatment, with a holding temperature of 425°C for 1.5 hours, then furnace cooled to 350°C, and then air cooled to room temperature;
[0067] 6) Straightening: The wire blank after aging treatment is straightened to obtain the finished product.
[0068] Comparative Example 1
[0069] The mass percentage composition of the copper alloy is: Al: 11.2wt%, Fe: 3.3wt%, Ni: 2.2wt%, and the balance is Cu and inevitable impurities.
[0070] 1) Batching and smelting + continuous casting: batching and melting according to the ingredients, and producing ingots through continuous casting.
[0071] 2) Hot extrusion: The ingot is heated to 940°C and extruded in a horizontal extruder to obtain a billet;
[0072] 3) Stretching: The extruded billet is subjected to cold deformation with a processing amount of 6%;
[0073] 4) Solution treatment: The stretched wire billet is solution treated at a holding temperature of 770°C for 90 minutes, followed by water cooling.
[0074] 5) Aging: The wire billet after solid solution is subjected to aging treatment, with a holding temperature of 690°C for 4.5 hours, and then furnace cooled to room temperature;
[0075] 6) Straightening: The wire blank after aging treatment is straightened to obtain the finished product.
[0076] Comparative Example 2
[0077] The mass percentage composition of the copper alloy is: Al: 6.8wt%, Fe: 2.5wt%, Ni: 4.9wt%, Mn: 2.5%; Si: 0.45%, and the balance is Cu and inevitable impurities.
[0078] 1) Batching and smelting + continuous casting: batching and melting according to the ingredients, and producing ingots through continuous casting.
[0079] 2) Hot extrusion: The ingot is heated to 850°C and extruded in a horizontal extruder to obtain a billet;
[0080] 3) Stretching: The extruded billet is subjected to cold deformation with a processing amount of 6%;
[0081] 4) Straightening: The wire blank after aging treatment is straightened to obtain the finished product.
[0082] The samples prepared in the comparative examples and the embodiments were subjected to tensile, hardness, scanning electron microscopy, and friction and wear tests, respectively.
[0083] The tensile strength, yield strength and elongation are measured in accordance with GT / T 34505-2017 "Room Temperature Tensile Test Method for Copper and Copper Alloy Materials".
[0084] The hardness is measured according to GB / T231.1-2009 "Brinell hardness test for metal materials".
[0085] The proportion of each phase was obtained by analyzing the scanning electron microscope photos using Pro-Image software.
[0086] Wear test: using hard steel ball reciprocating friction, loading force 20N, sliding length 10mm, frequency 5HZ, test time: 30min.
[0087] Table 1 Performance comparison of examples and comparative examples
[0088]
Claims
1. A high-strength wear-resistant copper alloy, characterized in that: The invention comprises the following components in percentage by weight: Al: 7-11wt%, Fe: 2-5wt%, Ni: 3-6%, Mn: 0.01-2wt%, and the balance is Cu and unavoidable impurities, wherein the weight of Al, Fe, Ni and Mn satisfies: 0.8≤Al / (Fe+Ni+Mn)≤2 and Ni / (Fe+Mn)≥1.
2. The high-strength wear-resistant copper alloy according to claim 1, characterized in that: The high-strength wear-resistant copper alloy comprises Si in a mass percentage of 0.01-0.5wt%.
3. The high-strength wear-resistant copper alloy according to claim 1 or 2, characterized in that: The high-strength wear-resistant copper alloy comprises Cr in a mass percentage of 0.01-0.3wt%.
4. The high-strength wear-resistant copper alloy according to claim 1, characterized in that: The microstructure of the high-strength wear-resistant copper alloy includes α phase, k phase, β and γ2 phase, wherein the area proportion of each phase is: 87.5%<α phase<96.5%, 0.5%<k phase<2.5%, 3%<β+γ2 phase<10%.
5. The high-strength wear-resistant copper alloy according to any one of claims 1 to 4, characterized in that: The tensile strength of the high-strength wear-resistant copper alloy is greater than 850 MPa, the yield strength is greater than 550, and the wear rate is less than 4.5×10 -6 mm 3 / (N·m).
6. The method for preparing a high-strength wear-resistant copper alloy according to any one of claims 1 to 5, characterized in that: The following steps are involved: Ingredient smelting + continuous casting → hot extrusion → stretching → solution treatment → aging → straightening, Wherein, in the aging process, the holding temperature is 420-700°C, the holding time is 1-5h, and after the holding is completed, the furnace is first cooled to 300-350°C and then air-cooled.
7. The preparation method according to claim 6, characterized in that: In the solutionizing process, the holding temperature is 750-950° C., the holding time is 20-90 minutes, and after the holding is completed, the mixture is immersed in a sodium chloride aqueous solution for cooling.
8. The preparation method according to claim 6, characterized in that: The hot extrusion temperature is 650-950°C.
9. The preparation method according to claim 6, characterized in that: In the stretching step, the processing rate is 5 to 15%.
10. Use of the high-strength and wear-resistant copper alloy according to any one of claims 1 to 5 in the fields of machinery manufacturing, shipbuilding, ocean or construction.