355MPa-strength-grade high-straightness steel plate and manufacturing method thereof
By introducing B elements into hot-rolled materials and controlling chemical composition, combined with the open-flat cutting board treatment process, the problems of poor quality stability and high production cost of steel plates of 355MPa strength grade high flatness are solved, and low internal stress and plate-shaped flattening are achieved The production of high straightness and high efficiency meets the high-quality requirements of steel plates during processing.
Patent Information
- Application Number
- CN202410887822.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-03
AI Technical Summary
When manufacturing 355MPa strength grade high-standard steel plates, the quality stability is poor and the production cost is high, making it difficult to meet the high-quality dimensional requirements such as cutting without warping and welding dimensional accuracy during the processing process.
By introducing B elements into hot-rolled materials and controlling the chemical composition quality, combining the open-flat cutting board treatment process, the straightness and internal stress are controlled, and the 355MPa strength level and good plate straightness are achieved. Production of steel plates.
It achieves efficient and stable production of steel plates, improves the processing stability and aesthetics of materials, and the pass rate of laser cutting pattern reaches more than 95%, reducing production costs, and is suitable for large-scale promotion and application.
Smart Images

Figure CN118957435A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of metal casting, and in particular to a 355MPa strength level high flatness steel plate and a manufacturing method thereof. Background Art
[0002] 355MPa strength grade high flatness steel plate belongs to low alloy structural steel, with relatively low material grade, mainly used for ordinary structural components, etc., and the quality requirements for the material are not high. However, with the popularization of automation such as laser cutting and automatic welding in downstream processing and supporting plants, steel plates need to meet high quality dimensional requirements such as cutting without warping and high dimensional accuracy of welding during use. In order to meet the use requirements of steel plates, the steel plates need to have the characteristics of low internal stress, good flatness and good stability of mechanical properties, so that the steel plates can reflect the processing ability and aesthetics of the materials. Therefore, it is necessary to have a comprehensive quality requirement of high quality and low price for this material.
[0003] However, due to the particularity of the production process, the existing technology for manufacturing coiled flat steel plates is not as good as the single-rolling steel plate rolling production line for controlling the internal stress quality of the product. Nb and Ti micro-alloy control is used in production control, resulting in high production costs and poor quality stability of the steel plates. Summary of the invention
[0004] The main purpose of the present invention is to provide a 355MPa strength level high flatness steel plate and a manufacturing method thereof, aiming to solve the problems of poor quality stability and high production cost of the 355MPa strength level high flatness steel plate produced by the prior art.
[0005] To achieve the above object, the present invention provides a 355MPa strength level high flatness steel plate, wherein the chemical composition mass percentage of the 355MPa strength level high flatness steel plate is 0.13wt%≤C≤0.15wt%, 0.15wt%≤Si≤0.30wt%, 0.50wt%≤Mn≤0.80wt%, P≤0.02wt%, S≤0.005wt%, 0.018wt%≤Als≤0.045wt% t%, 0.03wt%≤Ti≤0.04wt%, N≤0.0055wt%, 0.0012wt%≤B≤0.0020wt%, and the rest are iron and other inevitable impurities; and the average internal stress of the 355MPa strength level high flatness steel plate is <70MPa; the metallographic surface layer of the 355MPa strength level high flatness steel plate has a 30μm decarburized layer structure, and the grain boundaries are distributed with a F+B+P structure of cementite.
[0006] The present invention also provides a method for manufacturing a 355MPa strength level high flatness steel plate, comprising the steps of: providing a hot-rolled material; the chemical composition mass percentage of the hot-rolled material is 0.13wt%≤C≤0.15wt%, 0.15wt%≤Si≤0.30wt%, 0.50wt%≤Mn≤0.80wt%, P≤0.02wt%, S≤0.005wt%, 0.018wt%≤Als≤0.045wt%, 0.03wt%≤Ti≤0.04wt%, N≤0.0055wt%, 0.0012wt%≤B≤0.0020wt%, and the rest is iron and other inevitable impurities.
[0007] When the hot-rolled material is cooled to below 60°C, it is cut into plates according to the order specifications and thickness to obtain high-flatness steel plates with a strength level of 355MPa.
[0008] When the order specification thickness a≤12mm, the straightness ≤2mm / m; when the order specification thickness is 12mm<a≤18mm, the straightness ≤4mm / 2m; when the order specification thickness is 18mm<a≤25mm, the straightness ≤5mm / 2m; wherein, the order specification width b is 1800~2000mm.
[0009] Furthermore, the amount of pressure reduction at the entrance of the rough straightening process of the flattened plate processing is -5mm to -10mm.
[0010] Furthermore, when the straightness does not meet the requirements, it also includes tempering heat treatment of the steel plate and re-using it as the hot-rolled material for subsequent operation steps; the temperature of the tempering heat treatment is 550°C; the insulation time of the tempering heat treatment is 1.8amin; wherein a is the order specification thickness, in mm.
[0011] Furthermore, the thickness of the hot-rolled material is 230 mm; and the center segregation and center porosity of the slab of the hot-rolled material do not exceed C1.5.
[0012] Furthermore, before the hot rolled material is cooled, the hot rolled material is sequentially subjected to dephosphorization treatment, rough rolling treatment, finishing rolling treatment and coiling treatment; wherein the finishing rolling treatment temperature is 840-870°C; and the coiling treatment temperature is 560-630°C.
[0013] Furthermore, the rough rolling process uses a rough rolling mill with flat rolls; and the finish rolling process uses a finish rolling mill with CVC rolls.
[0014] Furthermore, after the finish rolling treatment, the finished product is subjected to laminar cooling to be cooled to the temperature of the coiling treatment; wherein the upper and lower water ratio of the laminar cooling is set to 1:1.1.
[0015] Furthermore, the hot-rolled material is obtained by sequentially performing top and bottom combined blowing converter primary refining, LF refining and CC casting on the raw materials to obtain the hot-rolled material.
[0016] Furthermore, the process of cooling to below 60° C. is specifically to take the hot-rolled material out of the warehouse for 24 hours to be cooled, and then naturally cool it to below 60° C.
[0017] The beneficial effects achieved by the present invention are:
[0018] The metallographic structure of the 355MPa strength grade high flatness steel plate provided by the present invention has a 30μm decarburized layer structure on the surface, and the F+B+P structure (ferrite+bainite+pearlite structure) of cementite is distributed at the grain boundary, the grains are uniform, the average internal stress of the steel plate is <70MPa, the plate shape is flat, the quality stability is high, and it has high processing stability and aesthetics. The qualified rate of laser cutting templates reaches more than 95%.
[0019] The method for manufacturing a 355MPa strength level high-flatness steel plate provided by the present invention enhances the hardenability and mechanical property stability of the 355MPa strength level high-flatness steel plate by introducing B element into the hot-rolled material and controlling 0.13wt%≤C≤0.15wt%, 0.03wt%≤Ti≤0.04wt%, and 0.0012wt%≤B≤0.0020wt%. Combined with a flattening plate processing process for controlling flatness according to order specification thickness, the 355MPa strength level high-flatness steel plate with low internal stress, good plate flatness, and high quality stability is produced efficiently and stably, and the quality problem of no warping or side bending of the material after laser cutting is met. Moreover, the manufacturing method has low cost and is suitable for large-scale promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0021] Figure 1 This is a comparison diagram of the residual stress of the products obtained in Example 1 and Comparative Example 1;
[0022] Figure 2 The material microstructure diagram of the product obtained in Example 1;
[0023] Figure 3 This is the material microstructure diagram of the product prepared in Comparative Example 1.
[0024] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with the implementation methods and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] It should be noted that, in the absence of conflict, the following embodiments and features in the embodiments can be combined with each other. It should also be understood that the terms used in the embodiments of the present invention are intended to describe specific embodiments rather than to limit the scope of protection of the present invention.
[0027] Unless otherwise defined, all technical and scientific terms used in the present invention are consistent with the prior art knowledge of those skilled in the art and the description of the present invention. The present invention can also be implemented using any methods, devices and materials in the prior art that are similar or equivalent to the methods, devices and materials described in the embodiments of the present invention.
[0028] When the embodiments give numerical ranges, it should be understood that unless otherwise specified in the present invention, both endpoints of each numerical range and any value between the two endpoints can be selected. The test methods in the following embodiments without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturers. The materials or reagents required in the following embodiments are commercially available unless otherwise specified.
[0029] In order to solve the problems of poor quality stability and high production cost of 355MPa strength level high flatness steel plates produced by the prior art, the present invention provides a 355MPa strength level high flatness steel plate, the chemical composition mass percentage of the 355MPa strength level high flatness steel plate is 0.13wt%≤C≤0.15wt%, 0.15wt%≤Si≤0.30wt%, 0.50wt%≤Mn≤0.80wt%, P≤0.02wt%, S≤0.005wt%, 0.018wt%≤Als≤0.045wt%, 0.03wt%≤Ti≤0.04wt%, N≤0.0055wt%, 0.0012wt%≤B≤0.0020wt%, and the rest are iron and other inevitable impurities; and the average internal stress of the 355MPa strength level high flatness steel plate is <70MPa; the metallographic structure surface layer of the 355MPa strength level high flatness steel plate has a 30μm decarburized layer structure, and the grain boundaries are distributed with a F+B+P structure of cementite.
[0030] The surface of the 355MPa strength grade high flatness steel plate provided by the present invention has a 30μm decarburized layer structure, and its grain boundaries are distributed with cementite F+B+P structure (ferrite+bainite+pearlite structure), the grains are uniform, the average internal stress of the steel plate is <70MPa, the plate shape is flat, the quality stability is high, and it has high processing stability and aesthetics. The qualified rate of laser cutting templates reaches more than 95%.
[0031] The present invention also provides a method for manufacturing a 355MPa strength level high flatness steel plate, comprising the steps of: providing a hot-rolled material; the chemical composition mass percentage of the hot-rolled material is 0.13wt%≤C≤0.15wt%, 0.15wt%≤Si≤0.30wt%, 0.50wt%≤Mn≤0.80wt%, P≤0.02wt%, S≤0.005wt%, 0.018wt%≤Als≤0.045wt%, 0.03wt%≤Ti≤0.04wt%, N≤0.0055wt%, 0.0012wt%≤B≤0.0020wt%, and the rest is iron and other inevitable impurities. Specifically, when 0.13wt%≤C≤0.15wt%, 0.03wt%≤Ti≤0.04wt%, 0.0012wt%≤B≤0.0020wt%, the yield strength is about 400Mpa, the content of Ti element is reduced to control the precipitation strengthening effect, and the performance is better stabilized. At the same time, the B element has good hardenability, which improves the effect of solid solution strengthening of the material and reduces the fluctuation of the mechanical properties of the material. The relatively low mechanical properties and surface decarburization layer organization are conducive to the control of flatness by the material cutting + straightening process.
[0032] When the hot-rolled material is cooled to below 60°C, it is cut into plates according to the order specifications and thickness to obtain high-flatness steel plates with a strength level of 355MPa.
[0033] When the order specification thickness a≤12mm, the straightness ≤2mm / m; when the order specification thickness is 12mm<a≤18mm, the straightness ≤4mm / 2m; when the order specification thickness is 18mm<a≤25mm, the straightness ≤5mm / 2m; wherein, the order specification width b is 1800~2000mm.
[0034] The method for manufacturing a 355MPa strength level high-flatness steel plate provided by the present invention enhances the hardenability and mechanical property stability of the 355MPa strength level high-flatness steel plate by introducing B element into the hot-rolled material and controlling 0.13wt%≤C≤0.15wt%, 0.03wt%≤Ti≤0.04wt%, and 0.0012wt%≤B≤0.0020wt%. Combined with a flattening plate processing process for controlling flatness according to order specification thickness, the 355MPa strength level high-flatness steel plate with low internal stress, good plate flatness, and high quality stability is produced efficiently and stably, and the quality problem of no warping or side bending of the material after laser cutting is met. Moreover, the manufacturing method has low cost and is suitable for large-scale promotion and application.
[0035] Furthermore, the pressure reduction of the rough straightening entrance of the flattening process is -5mm to -10mm. When the pressure reduction of the rough straightening entrance of the flattening process is -5mm to -10mm, the internal stress of the steel plate can be effectively released to improve the stability of the 355MPa strength grade high flatness steel plate.
[0036] Furthermore, when the flatness does not meet the requirements, it also includes tempering heat treatment of the steel plate and reusing it as hot-rolled material for subsequent operation steps; the temperature of the tempering heat treatment is 550°C; the holding time of the tempering heat treatment is 1.8amin; where a is the order specification thickness, in mm. Specifically, when the flatness of the steel plate does not meet the above requirements, the steel plate that does not meet the flatness requirements should be tempered heat treated at 550°C for 1.8amin, and after being tempered out of the furnace, it should be rolled on the cooling bed and naturally cooled to below 60°C, and then it should be cut and flattened according to the order specification thickness.
[0037] Furthermore, the thickness of the hot-rolled material is 230 mm, and the center segregation and center porosity of the hot-rolled material slab do not exceed C1.5. Specifically, it is beneficial to control the grain size of the material, and the hot-rolled material at this time has good surface quality and internal quality.
[0038] Furthermore, before the hot rolled material is cooled, the hot rolled material is subjected to dephosphorization treatment, rough rolling treatment, finishing rolling treatment and coiling treatment in sequence; wherein the temperature of the finishing rolling treatment is 840-870°C; and the temperature of the coiling treatment is 560-630°C.
[0039] Furthermore, the rough rolling process uses a rough rolling mill with flat rolls; and the finishing rolling process uses a finishing mill with CVC rolls.
[0040] Furthermore, after the finishing rolling process, the finished rolled material is subjected to laminar cooling to be cooled to the temperature of the coiling process; wherein the upper and lower water ratio of the laminar cooling is set to 1:1.1. When the upper and lower water ratio of the laminar cooling is set to 1:1.1, it can ensure that the upper and lower surfaces of the rolled material are cooled uniformly.
[0041] Furthermore, the hot-rolled material is obtained by sequentially performing top and bottom combined blowing converter primary refining, LF refining and CC casting on the raw materials to obtain the hot-rolled material. Specifically, LF refining is slag deoxidation, adjusting the composition of molten steel and controlling the temperature of molten steel, and finally forming molten steel with qualified composition, high cleanliness and appropriate temperature, and CC casting is to form a slab (hot-rolled material) with good surface and internal quality.
[0042] Furthermore, the process of cooling to below 60°C is specifically to take the hot-rolled material out of the warehouse for cooling for 24 hours, and then naturally cool it to below 60°C.
[0043] For further understanding of the present invention, examples are given below:
[0044] Example 1
[0045] (1) Composition of molten steel in the tundish: C: 0.143wt%, Si: 0.203wt%, Mn: 0.556wt%, P: 0.0152wt%, S: 0.0032wt%, Als: 0.0256wt%, Ti: 0.0325wt%, N: 0.0045wt%, B: 0.0012wt%, and the rest are iron and unavoidable elements.
[0046] (2) Rolling process: Finishing rolling temperature is 820℃~870℃, coiling temperature is 600~630℃, laminar water ratio is 1:1.1 and laminar water height is set. The thickness of the ingot is 230mm, the temperature of the continuous casting ingot heating furnace is 1195℃, and the total heating time is 242min. After the slab is heated, controlled rolling is carried out, and two-stage rolling is adopted. The rough rolling mill adopts flat rolls and the finishing mill adopts CVC rolls.
[0047] (3) According to the hot rolling process, the rolled steel coil is shipped out for 24 hours to be cooled. After the steel coil is naturally cooled to below 60°C, it is processed for flattening and cutting. The production specification of the order thickness is 8mm, and the pressure reduction at the entrance of the rough straightening is reduced to -4mm. The straightness of the steel plate does not exceed 3mm / 2m.
[0048] Example 2
[0049] (1) Composition of molten steel in the tundish: C: 0.135wt%, Si: 0.223wt%, Mn: 0.526wt%, P: 0.0122wt%, S: 0.0022wt%, Als: 0.0326wt%, Ti: 0.0355wt%, N: 0.0052wt%, B: 0.0018wt%, Cr: 0.20%, and the rest are iron and unavoidable elements.
[0050] (2) Rolling process: Finishing rolling temperature is 820℃~870℃, coiling temperature is 560~600℃, laminar water ratio is 1:1.1 and laminar water height is set. The thickness of the ingot is 230mm, the temperature of the continuous casting ingot out of the furnace is 1215℃, and the total heating time is 256min. After the slab is heated, controlled rolling is carried out, and two-stage rolling is adopted. The rough rolling mill adopts flat rolls and the finishing mill adopts CVC rolls.
[0051] (3) According to the hot rolling process, the rolled steel coil is shipped out for 24 hours to be cooled. After the steel coil is naturally cooled to below 60°C, it is processed for flattening and cutting. The production specification of the order thickness is 20mm, and the pressure reduction at the entrance of the rough straightening is reduced to -8mm. The straightness of the steel plate does not exceed 5mm / 2m, and the straightness of some steel plates at the end of the coil is 10-15mm / 2m.
[0052] (4) The steel plate is tempered at a temperature of 550°C and a holding time of 36 min. The steel plate is then rolled on a cooling bed and naturally cooled to room temperature. The straightness is 2 mm / 2 m.
[0053] Comparative Example 1
[0054] (1) Composition of molten steel in the tundish: C: 0.075wt%, Si: 0.153wt%, Mn: 0.80wt%, P: 0.0132wt%, S: 0.0042wt%, Als: 0.0226wt%, Ti: 0.0425wt%, Nb: 0.0115wt%, N: 0.0062wt%, and the rest are iron and unavoidable elements.
[0055] (2) Rolling process: Finishing rolling temperature is 850℃~870℃, coiling temperature is 610~630℃, laminar water ratio is 1:1.1 and laminar water height is set. The thickness of the ingot is 230mm, the temperature of the continuous casting ingot out of the furnace is 1205℃, and the total heating time is 256min. After the slab is heated, controlled rolling is carried out, and two-stage rolling is adopted. The rough rolling mill adopts flat rolls and the finishing mill adopts CVC rolls.
[0056] (3) Rolling is controlled according to the hot rolling process. The rolled steel coil is placed in the hot coil warehouse for more than 48 hours. The steel coil is naturally cooled to below 60°C for flattening and cutting. The pressure reduction at the entrance of the rough straightening is reduced to -5mm, and the straightness of the steel plate is 5mm / 2m.
[0057] Comparative Example 2
[0058] (1) Composition of molten steel in the tundish: C: 0.065wt%, Si: 0.183wt%, Mn: 0.967wt%, P: 0.0102wt%, S: 0.003wt%, Als: 0.0286wt%, Ti: 0.0455wt%, N: 0.0056wt%, Nb: 0.0215wt%, and the rest are iron and unavoidable elements.
[0059] (2) Rolling process: Finishing rolling temperature is 840℃~860℃, coiling temperature is 560~580℃, laminar water ratio is 1:1.1 and laminar water height is set. The thickness of the ingot is 230mm, the temperature of the continuous casting ingot out of the furnace is 1220℃, and the total heating time is 302 minutes. After the slab is heated, controlled rolling is carried out, and two-stage rolling is adopted. The rough rolling mill adopts flat rolls and the finishing mill adopts CVC rolls.
[0060] (3) According to the hot rolling process, the rolled steel coil is shipped out for 24 hours to be cooled. After the steel coil is naturally cooled to below 60°C, it is processed for flattening and cutting. The production specification of the order thickness is 20mm, and the pressure reduction at the entrance of the rough straightening is reduced to -5mm. The straightness of the steel plate is 7-15mm / 2m, and the straightness of the steel plate does not meet the requirements.
[0061] Analysis example 1
[0062] (1) The mechanical properties of the products obtained in Examples 1 to 2 and Comparative Examples 1 to 2 were compared and analyzed; the mechanical properties of the products obtained in Examples 1 to 2 and Comparative Examples 1 to 2 are shown in Table 1.
[0063] Table 1 Comparative analysis of mechanical properties of products obtained from Examples 1-2 and Comparative Examples 1-2
[0064]
[0065] According to Table 1, the yield of the materials in Examples 1 and 2 is relatively lower by about 30 MPa than that in Comparative Examples 1 and 2, and the elongation is increased by 7-10%, and the materials have good processing characteristics.
[0066] (2) The residual stress of Example 1 and Comparative Example 1 was tested. The specific results were compared as follows: Figure 1 .
[0067] from Figure 1 It can be seen that the internal stress detection data of Example 1 and Comparative Example 1 show that the internal stress of the embodiment is low and the stability is better.
[0068] (3) The metallographic structures of Example 1 and Comparative Example 1 were observed microscopically, and the microstructure diagrams of the materials were as follows: Figure 2 , Figure 3 shown.
[0069] from Figure 2 It can be seen from the figure that the decarburized layer is 30-50um on the surface; the B structure content gradually increases from the decarburized layer to 1 / 4 of the thickness. The metallographic structure shows that the addition of B element and the reduction of Ti element have achieved structural strengthening instead of precipitation strengthening; Figure 3 It can be seen that there is basically no decarburized layer on the surface, and the main structure is ferrite and pearlite. Figure 2 and Figure 3 It can be seen that the material microstructure of the 355MPa strength grade steel shows a 30-50μm decarburized layer on the surface. The decarburized layer has a good effect on stress conduction during straightening, and does not affect the mechanical properties. That is, the concentrated stress area is more likely to conduct stress to the ferrite tissue area through the deformation caused by straightening. This decarburized layer is beneficial to the stress uniformity of customers during straightening. By using the hardenability characteristics of B and Cr elements and reducing the precipitation effect of Ti elements, the addition of B element achieves the goal of organizational strengthening instead of partial precipitation strengthening.
[0070] In summary, the above technical solutions of the present invention are only preferred embodiments of the present invention, and the patent scope of the present invention is not limited thereto. All equivalent structural changes made by using the contents of the present invention specification and drawings under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A 355MPa strength grade high flatness steel plate, characterized in that: The chemical composition of the 355MPa strength grade high flatness steel plate is 0.13wt%≤C≤0.15wt%, 0.15wt%≤Si≤0.30wt%, 0.50wt%≤Mn≤0.80wt%, P≤0.02wt%, S≤0.005wt%, 0.018wt%≤Als≤0.045wt%, 0.03wt%≤Ti≤0.04wt%, N≤0.0055wt%, 0.0012wt%≤B≤0.0020wt%, and the rest is iron and other unavoidable impurities; The average internal stress of the 355MPa strength grade high flatness steel plate is <70MPa; the metallographic surface layer of the 355MPa strength grade high flatness steel plate has a 30μm decarburized layer structure, and the F+B+P structure of cementite is distributed at its grain boundaries.
2. A method for manufacturing a 355MPa strength grade high flatness steel plate, characterized in that: Includes steps: A hot-rolled material is provided; the chemical composition of the hot-rolled material is 0.13wt%≤C≤0.15wt%, 0.15wt%≤Si≤0.30wt%, 0.50wt%≤Mn≤0.80wt%, P≤0.02wt%, S≤0.005wt%, 0.018wt%≤Als≤0.045wt%, 0.03wt%≤Ti≤0.04wt%, N≤0.0055wt%, 0.0012wt%≤B≤0.0020wt%, and the rest is iron and other inevitable impurities; When the hot-rolled material is cooled to below 60°C, it is cut into plates according to the order specifications and thickness to obtain 355MPa strength grade high flatness steel plates; When the order specification thickness a≤12mm, the straightness ≤2mm / m; when the order specification thickness is 12mm<a≤18mm, the straightness ≤4mm / 2m; when the order specification thickness is 18mm<a≤25mm, the straightness ≤5mm / 2m; wherein, the order specification width b is 1800~2000mm.
3. The manufacturing method according to claim 2, characterized in that: The rough straightening entrance pressure reduction amount of the flattened plate processing is -5mm to -10mm.
4. The manufacturing method according to claim 2, characterized in that: When the straightness does not meet the requirement, the steel plate is subjected to tempering heat treatment and used as the hot-rolled material for subsequent operation steps; The temperature of the tempering heat treatment is 550°C; the insulation time of the tempering heat treatment is 1.8amin; wherein a is the order specification thickness, in mm.
5. The manufacturing method according to claim 2, characterized in that: The thickness of the hot-rolled material is 230 mm; and the center segregation and center porosity of the slab of the hot-rolled material do not exceed C1.
5.
6. The manufacturing method according to claim 2, characterized in that: The hot rolled material is subjected to dephosphorization treatment, rough rolling treatment, finish rolling treatment and coiling treatment in sequence before the hot rolled material is cooled; Wherein, the temperature of the finish rolling process is 840-870°C; the temperature of the coiling process is 560-630°C.
7. The manufacturing method according to claim 6, characterized in that: The rough rolling process uses a rough rolling mill with flat rolls; the finish rolling process uses a finish rolling mill with CVC rolls.
8. The manufacturing method according to claim 6, characterized in that: After the finishing rolling process, the finished product is subjected to laminar cooling to a temperature of the coiling process; Wherein, the upper and lower water ratio of the laminar cooling is set to 1:1.
1.
9. The manufacturing method according to claim 2, characterized in that: The hot-rolled material is obtained by sequentially performing top-bottom combined blowing converter primary refining, LF refining and CC casting on the raw materials to obtain the hot-rolled material.
10. The manufacturing method according to claim 2, characterized in that: The process of cooling to below 60° C. specifically includes taking the hot-rolled material out of the warehouse for cooling for 24 hours, and then naturally cooling it to below 60° C.
Citation Information
Patent Citations
Low-cost hot-rolled steel plate with yield strength of 345 MPa, and manufacturing method thereof
CN107419078A
High-carbon steel plate with high plastic toughness and high straightness and manufacturing method of same
CN109321830A
Thin, wide, extremely long and high-straightness steel plate and preparation method thereof
CN116463558A
Hot-dip aluminum-zinc-plated steel plate with yield strength of 350MPa and manufacturing method thereof
CN117327970A
High-strength steel sheet excellent in seam weldability
KR1020180125936A