Metal ceramic spectrum selective absorbing coating with dual composite nano microstructure and preparation method thereof

By using dual composite nano-microstructure and multi-arc ion plating technology in metal cermet spectral selective absorption coatings, the existing coatings are solved by using double-composite nano-microstructure and multi-arc ion plating technology to form efficient solar spectrum selective absorption coatings, which solves the instability of existing coatings at high temperatures and complex preparation. Problem, high-efficiency spectral selection absorption and thermal stability are achieved, suitable for large-scale production.

CN118957496AInactive Publication Date: 2024-11-15JINZHONG UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411048644.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing metal cermet solar spectral selective absorption coating is unstable under high temperature environments, the spectral absorption mechanism is single, the preparation process is complex, and the multi-layer thickness is required to be precisely controlled.

Method used

The metal cermet spectral selective absorption coating with dual composite nanomicrostructure is composed of metal chromium infrared reflective layer, AlCrNbSiTiON absorbing layer and AlCrO anti-reflective layer. The AlCrNbSiTiON absorbing layer is composed of high entropy nitrogen oxide nanoparticles in the FCC structure and The amorphous ceramic dielectrics are arranged alternately to form a layered composite nanomicrostructure, which is deposited by multi-arc ion plating technology to form a double layered composite nanomicrostructure.

Benefits of technology

It achieves efficient solar light selection absorption performance and thermal stability, with an absorption rate of more than 0.91 and an emissivity of less than 0.15. It can be stable at 500°C atmospheric conditions for more than 400 hours, simplifying the preparation process and suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957496A_ABST
    Figure CN118957496A_ABST
Patent Text Reader

Abstract

The invention discloses a metal ceramic spectrum selective absorbing coating with a dual composite nano microstructure and a preparation method of the metal ceramic spectrum selective absorbing coating, and belongs to the technical field of material preparation, the metal ceramic spectrum selective absorbing coating sequentially comprises a metal chromium infrared reflecting layer, an AlCrNbSiTiON absorbing layer and an AlCrO antireflection layer from a substrate to the outside, the AlCrNbSiTiON absorption layer is formed by a double layered composite nanometer microstructure, and the AlCrNbSiTiON absorption layer is formed by a double layered composite nanometer The layered composite nano microstructure is composed of high-entropy nitrogen oxide nano particles of an FCC (fluid catalytic cracking) structure and an amorphous ceramic dielectric medium. The coating has good spectrum selective absorption performance and thermal stability, the absorptivity of the coating is higher than 0.91, the emissivity of the coating is lower than 0.15, and the coating can be stabilized for more than 400 hours at the temperature of 500 DEG C under the atmospheric condition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material preparation, and in particular relates to a metal ceramic spectrally selective absorption coating with a double composite nano-microstructure and a preparation method thereof. Background Art

[0002] As energy demand grows, the energy crisis is becoming increasingly severe. Traditional fossil energy is non-renewable and pollutes the environment, so the development of new clean energy has become the key. As a clean, pollution-free new energy source, solar energy does not produce pollutants when used, effectively reduces the risk of environmental pollution, and is crucial to protecting the earth's ecology. There are various ways to use solar energy, among which photothermal conversion technology is the most widely used, with the advantages of high efficiency, economy, and strong compatibility. However, since the energy density of solar energy is low and discontinuous after reaching the earth, large-scale development still faces challenges. For a long time, how to convert low-grade solar energy into high-grade thermal energy and enrich solar energy has always been the focus of solar thermal utilization and thermal power generation systems. In order to improve the efficiency of capturing sunlight, the most effective way is to use solar spectrum selective absorption coatings.

[0003] Solar spectrum selective absorption coating is a special coating that efficiently absorbs sunlight in the 0.3-2.5μm band and has a low emissivity in the 2.5-25μm band, which can convert sunlight into heat energy. Because it needs to work in a high temperature environment for a long time, the coating needs to have good thermal stability to resist performance degradation caused by high temperature.

[0004] Metal ceramic coatings, which are composed of metal nanoparticles embedded in ceramic dielectrics, are widely used in solar spectrum selective absorption coatings due to their excellent spectral selective absorption performance and thermal stability. However, existing metal ceramic solar spectrum selective absorption coatings have the following main problems: (1) The spectral absorption mechanism of metal ceramic coatings is single and is severely restricted by the characteristics of nanoparticles; (2) Nanoparticles in the coating are prone to unstable behaviors such as growth and agglomeration in high temperature environments above 500°C, and their thermal stability is insufficient, which induces the attenuation of the coating's spectral selective absorption performance; (3) Existing metal ceramic solar spectrum selective absorption coatings are multi-layer composite structures, and the thickness of each layer needs to be precisely controlled to obtain a good sunlight selective absorption effect, and the preparation process is complicated. Summary of the invention

[0005] The purpose of the present invention is to provide a metal ceramic spectrally selective absorption coating with a double composite nano-microstructure and a preparation method thereof, wherein the coating has good spectrally selective absorption performance and thermal stability.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:

[0007] A metal ceramic spectrally selective absorption coating with a double composite nanostructure, the coating comprising a metal chromium infrared reflection layer, an AlCrNbSiTiON absorption layer and an AlCrO anti-reflection layer in order from the substrate to the outside;

[0008] The AlCrNbSiTiON absorption layer is composed of a double layered composite nano-microstructure;

[0009] The layered composite nanostructure consists of high entropy nitrogen oxide nanoparticles with an FCC structure and an amorphous ceramic dielectric.

[0010] Preferably, the high entropy nitrogen oxide nanoparticles of FCC structure and the amorphous ceramic dielectric are arranged alternately in the layered composite nanostructure to form a layered composite nanostructure, wherein the thickness of a single layer of high entropy nitrogen oxide nanoparticles is 2 to 5 nm, and the thickness of a single layer of amorphous ceramic dielectric is 3 to 7 nm.

[0011] Preferably, in the double layered composite nano-microstructure, the bottom layered composite nano-microstructure is parallel to the substrate, and the top layered composite nano-microstructure is perpendicular to the substrate.

[0012] Preferably, the thickness of the metal ceramic spectrally selective absorption coating is 130 nm. In the AlCrNbSiTiON absorption layer, the thickness of the high entropy nitrogen oxide nanoparticle layer in the lower composite nanostructure parallel to the substrate is 2 to 5 nm, and the thickness of the high entropy nitrogen oxide nanoparticle layer in the upper composite nanostructure perpendicular to the substrate is 3 to 7 nm.

[0013] The present invention also provides a method for preparing a metal ceramic spectrally selective absorption coating having a dual composite nanostructure, comprising the following steps:

[0014] S1, after cleaning and drying the substrate, fix it on the rotating bracket of the furnace chamber, evacuate the furnace chamber, and heat it;

[0015] S2, etching and cleaning the substrate;

[0016] S3, depositing an infrared reflection layer: introducing argon gas, sputtering a chromium target, and forming a metallic chromium infrared reflection layer on the surface of the substrate;

[0017] S4, depositing an absorption layer: introducing a mixed gas of argon, nitrogen and oxygen, sputtering an AlCrNbSiTi high entropy alloy target, and depositing a layer of AlCrNbSiTiON nanocomposite absorption layer on the metal chromium infrared reflection layer in step S3;

[0018] S5, depositing an anti-reflection layer: introducing a mixed gas of argon and oxygen to sputter an AlCr target, and depositing an AlCrO anti-reflection layer on the AlCrNbSiTiON nanocomposite absorption layer in step S4. After the deposition is completed, turn off the arc target power supply, bias power supply, gas valve, and heating power supply in sequence, and after the temperature of the vacuum chamber drops to room temperature, take out the sample to obtain a metal ceramic spectrally selective absorption coating.

[0019] Preferably, in step S1, the substrate is ultrasonically cleaned with deionized water, acetone and anhydrous ethanol for 30 to 40 minutes in sequence, dried with nitrogen, fixed on a rotating bracket in a furnace chamber, and the furnace chamber is vacuumed to 3.0×10 -3 ~6.0×10 -3 Pa, heated to 150-250°C.

[0020] Preferably, in step S2, the etching and cleaning working parameters for the substrate are as follows: after the vacuum degree of the furnace chamber reaches the set value, 80 to 150 sccm of high-purity argon gas is introduced, the spin of the turntable is turned on, the rotation speed is adjusted to 3 to 5 r / min, the bias voltage of the multi-arc ion plating equipment is -500 to -800 V, the furnace chamber pressure is 0.4 to 0.8 Pa, the target power supply is turned on, and the substrate to be deposited is bombarded and cleaned for 10 to 15 minutes.

[0021] Preferably, in step S3, 85 to 95 sccm of argon gas is introduced into the furnace chamber, the gas pressure is 0.4 to 0.8 Pa, the chromium target deposition current is 80 to 110 A, the substrate bias voltage is -100 to -150 V, and the sputtering deposition is performed for 10 to 15 minutes.

[0022] Preferably, in step S4, 30-60 sccm argon, 40-70 sccm nitrogen and 30-60 sccm oxygen are introduced into the furnace chamber, the nitrogen flow rate is adjusted, the gas pressure is 0.5-0.7 Pa, the AlCrNbSiTi high entropy alloy target bias is adjusted to -100-150 V, the deposition current is 60-110 A, the sputtering deposition is performed for 2-3 min, the turntable speed is adjusted to 4-6 r / min, and the sputtering deposition is performed for 2-3 min.

[0023] Preferably, in step S5, 60-100 sccm argon and 120-160 sccm oxygen are introduced into the furnace chamber, the argon flow rate is adjusted, the gas pressure is 0.4-0.8 Pa, the AlCr target bias is adjusted to -100--150 V, the deposition current is 60-90 A, and the sputtering deposition is performed for 2-5 min.

[0024] The present invention also provides application of the metal ceramic spectrally selective absorption coating or the metal ceramic spectrally selective absorption coating prepared by the preparation method in solar thermal utilization.

[0025] The technical principle of forming a double layered composite nano-microstructure in the AlCrNbSiTiON absorption layer of the present invention is as follows: during the deposition process of the multi-arc ion plating technology, the cathode arc plasma is not evenly distributed in the furnace chamber, so that the products formed by the reaction of the target material elements and the gas are not evenly distributed, and the atoms with large mass in the target material tend to be distributed in the space area normal to the target surface, while the atoms with small mass tend to be distributed in the high-angle area normal to the target surface. At the same time, the reaction gas in the central area of ​​the target surface is not enough to react completely with the sputtered atoms, thereby forming a composite structure of nitrogen oxides and metals, while in the high-angle area normal to the target surface, the reaction gas is sufficient to form a ceramic dielectric. During the deposition process, when the substrate passes through different areas continuously, a layered microstructure in which amorphous and crystalline are alternately distributed is formed. In addition, changing the rotation speed of the rotating bracket during the deposition process will change the epitaxial growth relationship of the nanocrystalline / amorphous composite structure, thereby forming a double layered composite nano-microstructure in the AlCrNbSiTiON absorption layer.

[0026] Compared with the prior art, the present invention has the following advantages and technical effects:

[0027] 1. The present invention discloses a metal ceramic spectrally selective absorption coating with a double composite nanostructure, which includes an infrared reflection layer, an absorption layer and an anti-reflection layer in order from the substrate to the outside. The coating includes a metal Cr infrared reflection layer, an AlCrNbSiTiON absorption layer and an AlCrO anti-reflection layer in order from the substrate to the outside, wherein the AlCrNbSiTiON metal ceramic absorption layer has a double composite nanostructure, the bottom layered composite nanostructure is parallel to the substrate, and the top layered composite nanostructure is perpendicular to the substrate. The coating has both good spectrally selective absorption performance and thermal stability, with an absorptivity higher than 0.91 and an emissivity lower than 0.15, and can be stable for more than 400 hours at 500°C and atmospheric conditions.

[0028] 2. The present invention forms a dual composite nano-microstructure inside the AlCrNbSiTiON metal ceramic absorption layer by controlling the deposition process of the multi-arc ion plating process, which can composite dielectric-metal-dielectric and metal ceramic absorbers to achieve the synergistic effect of multiple spectral absorption mechanisms and obtain good sunlight selective absorption performance. At the same time, the dual composite nano-microstructure can use amorphous dielectrics to separate nanoparticles, effectively inhibit the diffusion and fusion of nanoparticles at high temperatures, and significantly improve the thermal stability of the coating. In addition, the multi-arc ion plating technology is used, with high deposition efficiency and low cost, which can enhance the bonding force between the coating and the stainless steel substrate and indirectly improve the thermal stability of the coating.

[0029] 3. The metal ceramic spectrally selective absorption coating of the present invention contains only one absorption layer, which reduces the macroscopic interface in the coating, helps to inhibit the long-range diffusion of atoms, improves the thermal stability of nanoparticles, does not require strict control of the thickness of each layer, has a simple preparation process, and is suitable for large-scale production.

[0030] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a schematic diagram of the structure of the metal ceramic spectrally selective absorption coating of the present invention;

[0032] Figure 2 A reflection spectrum curve of the metal ceramic spectrally selective absorption coating provided in Example 1;

[0033] Figure 3 A reflection spectrum curve of the metal ceramic spectrally selective absorption coating provided in Example 2;

[0034] Figure 4 This is the HADDF diagram of the metal ceramic spectrally selective absorption coating provided in Example 1. DETAILED DESCRIPTION

[0035] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.

[0036] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one having ordinary skills in the field to which the present invention belongs.

[0037] Sources of materials used in the present invention: Unless otherwise specified, the gases, equipment and methods used in the present invention are all commonly used gases, equipment and methods in the technical field. The raw materials used are all conventional commercial products in the field.

[0038] Example 1

[0039] A metal ceramic spectrally selective absorption coating with a double composite nano-microstructure, the coating includes a metal chromium infrared reflection layer, an AlCrNbSiTiON absorption layer and an AlCrO anti-reflection layer in order from a 304 mirror stainless steel substrate to the outside, wherein the AlCrNbSiTiON absorption layer is composed of a double layered composite nano-microstructure; the layered composite nano-microstructure is composed of high entropy nitrogen oxide nanoparticles of FCC structure and amorphous ceramic dielectrics, such as Figure 1 shown.

[0040] Depend on Figure 1 It can be seen that the coating is deposited on a 304 stainless steel substrate, and includes an AlCrNbSiTiON absorption layer and an AlCrO anti-reflection layer from bottom to top.

[0041] In the layered composite nanostructure, high entropy nitrogen oxide nanoparticles of FCC structure and amorphous ceramic dielectrics are arranged alternately to form a layered composite nanostructure, wherein the thickness of a single layer of high entropy nitrogen oxide nanoparticles is 2 nm, and the thickness of a single layer of amorphous ceramic dielectrics is 4 nm.

[0042] In the double-layered composite nanostructure, the bottom layered composite nanostructure is parallel to the substrate, and its high entropy nitrogen oxide nanoparticle layer thickness is 3nm; the top layered composite nanostructure is perpendicular to the substrate, and its high entropy nitrogen oxide nanoparticle layer thickness is 5nm.

[0043] A method for preparing a metal ceramic spectrally selective absorption coating with a dual composite nanostructure comprises the following steps:

[0044] The 304 mirror stainless steel substrate was used as the substrate and the coating was deposited using a cathode multi-arc ion plating device. The metal chromium infrared reflection layer used a Cr target with a purity of 99.95% and was deposited in a pure Ar environment. The AlCrNbSiTiON absorption layer used an AlCrNbSiTi high entropy alloy target and was deposited in an atmosphere of nitrogen and oxygen. The AlCrO anti-reflection layer on the surface used Al 60 Cr 40 (atomic percentage) alloy target for deposition.

[0045] The target size used in the deposition process is Φ110 mm×5 mm, and the size of the 304 mirror stainless steel substrate is 30×40×1 mm.

[0046] S1. The 304 stainless steel substrate was ultrasonically cleaned with deionized water, acetone and anhydrous ethanol for 35 min in sequence to remove the attached matter on the surface, dried with nitrogen, fixed on the rotating bracket in the multi-arc ion plating furnace, and the furnace door was closed. The vacuum in the furnace was evacuated to 4.0×10 -3 Pa, heated to 200°C;

[0047] S2. Etching and cleaning the substrate: After the vacuum degree of the furnace chamber reaches the set value, 80 sccm of high-purity argon gas is introduced, the furnace chamber pressure is 0.5 Pa, the rotating frame is turned on, the speed is adjusted to 4r / min, the bias voltage of the multi-arc ion plating equipment is -600V, the target power supply is turned on, and the substrate to be deposited is bombarded and cleaned for 15 minutes;

[0048] S3, depositing an infrared reflection layer: introducing argon gas, controlling the argon gas flow rate to 85 sccm, keeping the furnace chamber pressure at 0.45 Pa, turning on the chromium metal target power supply in the furnace chamber, setting the deposition current to 90 A, the substrate bias voltage to -120 V, sputtering the chromium target, and depositing for 12 minutes to form a metal chromium infrared reflection layer on the substrate surface;

[0049] S4, deposition of absorption layer: 50 sccm argon, nitrogen and 40 sccm oxygen are introduced into the furnace chamber, the nitrogen flow rate is adjusted to 55 sccm, the furnace chamber pressure is maintained at 0.5 Pa, the AlCrNbSiTi high entropy alloy target power supply is turned on, the deposition current is set to 80A, the bias voltage is set to -120V, the sputtering deposition is performed for 2.5min, the rotating frame speed is adjusted to 5r / min, the sputtering deposition is performed for 2.5min, and a layer of AlCrNbSiTiON nanocomposite absorption layer is deposited on the metal chromium infrared reflection layer in step S3;

[0050] S5, depositing an anti-reflection layer: argon gas and 140 sccm of oxygen are introduced into the furnace chamber, and the argon flow rate is adjusted to 75 sccm to keep the furnace chamber pressure at 0.45 Pa. The AlCr alloy target power supply is turned on, the deposition current is set to 85A, and a substrate bias voltage of -120V is applied. The sputtering deposition is performed for 4 minutes. A layer of AlCrO anti-reflection layer is deposited on the AlCrNbSiTiON nanocomposite absorption layer in step S4. After the deposition is completed, the arc target power supply, bias power supply, gas valve, and heating power supply are turned off in sequence. After the vacuum chamber temperature drops to room temperature, the furnace door is opened and the sample is taken out to obtain a metal ceramic spectrally selective absorption coating.

[0051] Example 2

[0052] The preparation method is the same as that of Example 1, except that the gas flow rates of the AlCrNbSiTiON absorption layer are 40 sccm argon, 50 sccm nitrogen and 45 sccm oxygen respectively introduced into the furnace chamber.

[0053] The effects of the metal ceramic spectrally selective absorption coatings provided in Example 1 and Example 2 were verified by the following experiments:

[0054] 1. The reflectance spectrum curves of the coating close to normal incidence (<10°) in the wavelength range of 300-2500nm and 2500-25000nm were tested using Agilent Cary 5000 UV-Vis-NIR spectrophotometer and Nicolet iS50 FT-IR Fourier transform infrared spectrometer respectively.

[0055] The following formulas are used to calculate the coating's absorptivity α and emissivity ε to sunlight:

[0056]

[0057]

[0058] Where λ is the wavelength, I sol (λ) is the solar radiation power at AM1.5; I b(λ) is the blackbody radiation power at room temperature; R(λ) is the reflectivity of the coating. Figure 2 and Figure 3 shown.

[0059] Depend on Figure 2 It can be seen that the metal ceramic spectrally selective absorption coating provided in Example 1 has an absorptivity α of 0.918 and an emissivity ε of 0.0983 for sunlight, showing excellent spectrally selective absorption performance.

[0060] Depend on Figure 3 It can be seen that the metal ceramic spectrally selective absorption coating provided in Example 2 has an absorptivity α of 0.919 and an emissivity ε of 0.1202 for sunlight, and also exhibits excellent spectrally selective absorption performance and has good repeatability.

[0061] 2. The thermal stability test of the metal ceramic spectrally selective absorption coating provided in Example 1 and Example 2 was carried out. The samples were placed in a muffle furnace, heated to 500°C in an atmospheric environment, and kept warm for 400 hours. The absorptivity α and emissivity ε of the coating to sunlight after annealing were calculated using the same calculation formula as above. The results are as follows: Figure 2 and Figure 3 .

[0062] Depend on Figure 2 It can be seen that the annealed coating provided in Example 1 has an absorptivity α of 0.923 and an emissivity ε of 0.1184 to sunlight, showing excellent high-temperature thermal stability.

[0063] Depend on Figure 3 It can be seen that the absorption rate α of the annealed coating provided in Example 2 to sunlight is 0.923, and the emissivity ε is 0.1190, which indicates that the coating prepared by the present invention has excellent thermal stability at a high temperature of 500°C and in an atmospheric environment.

[0064] 3. The metal ceramic spectrally selective absorption coating provided in Example 1 was subjected to TEM test after annealing. Figure 4 shown.

[0065] Depend on Figure 4 It can be seen that two kinds of nanocomposite microstructures are formed inside the AlCrNbSiTiON absorption layer. The one close to the Cr layer is a layered microstructure parallel to the substrate, in which the thickness of the single-layer high-entropy nitrogen oxide nanoparticle layer is 3nm, and the thickness of the single-layer amorphous ceramic dielectric layer is 4nm. The one close to the AlCrO layer is a layered microstructure perpendicular to the substrate, in which the thickness of the single-layer high-entropy nitrogen oxide nanoparticle layer is 5nm, and the thickness of the single-layer amorphous ceramic dielectric layer is 6nm.

[0066] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A metal ceramic spectrally selective absorption coating with a double composite nanostructure, It is characterized in that The coating includes a metal chromium infrared reflection layer, an AlCrNbSiTiON absorption layer and an AlCrO anti-reflection layer in order from the substrate to the outside; The AlCrNbSiTiON absorption layer is composed of a double layered composite nano-microstructure; The layered composite nano-microstructure consists of high-entropy nitrogen oxide nanoparticles with an FCC structure and an amorphous ceramic dielectric.

2. The metal ceramic spectrally selective absorption coating with a dual composite nanostructure according to claim 1, It is characterized in that In the layered composite nanostructure, high entropy nitrogen oxide nanoparticles of FCC structure and amorphous ceramic dielectrics are arranged alternately, wherein the thickness of a single layer of high entropy nitrogen oxide nanoparticles is 2 to 5 nm, and the thickness of a single layer of amorphous ceramic dielectrics is 3 to 7 nm.

3. The metal ceramic spectrally selective absorption coating with a dual composite nanostructure according to claim 1, It is characterized in that In the double layered composite nanostructure, the bottom layered composite nanostructure is parallel to the substrate, and the top layered composite nanostructure is perpendicular to the substrate.

4. A method for preparing the metal ceramic spectrally selective absorption coating as claimed in claims 1 to 3, It is characterized in that The following steps are involved: S1, after cleaning and drying the substrate, fix it on the rotating bracket of the furnace chamber, evacuate the furnace chamber, and heat it; S2, etching and cleaning the substrate; S3, depositing an infrared reflection layer: introducing argon gas, sputtering a chromium target, and forming a metallic chromium infrared reflection layer on the surface of the substrate; S4, depositing an absorption layer: introducing a mixed gas of argon, nitrogen and oxygen, sputtering an AlCrNbSiTi high entropy alloy target, and depositing a layer of AlCrNbSiTiON nanocomposite absorption layer on the metal chromium infrared reflection layer in step S3; S5, depositing an anti-reflection layer: introducing a mixed gas of argon and oxygen to sputter an AlCr target, and depositing an AlCrO anti-reflection layer on the AlCrNbSiTiON nanocomposite absorption layer in step S4. After the deposition is completed, turn off the arc target power supply, bias power supply, gas valve, and heating power supply in sequence, and after the temperature of the vacuum chamber drops to room temperature, take out the sample to obtain a metal ceramic spectrally selective absorption coating.

5. The preparation method according to claim 4, It is characterized in that In step S1, the substrate is ultrasonically cleaned with deionized water, acetone and anhydrous ethanol for 30 to 40 minutes in sequence, dried with nitrogen, fixed on a rotating bracket in the furnace chamber, and the furnace chamber is vacuumed to 3.0×10 -3 ~6.0×10 -3 Pa, heated to 150-250°C.

6. The preparation method according to claim 4, It is characterized in that In step S2, the etching and cleaning working parameters for the substrate are as follows: after the vacuum degree of the furnace chamber reaches the set value, 80 to 150 sccm of high-purity argon gas is introduced, the spin frame is turned on, the rotation speed is adjusted to 3 to 5 r / min, the bias voltage is -500 to -800 V, the furnace chamber pressure is 0.4 to 0.8 Pa, the target power supply is turned on, and the substrate to be deposited is bombarded and cleaned for 10 to 15 minutes.

7. The preparation method according to claim 4, It is characterized in that In step S3, 85 to 95 sccm of argon gas is introduced into the furnace chamber, the gas pressure is 0.4 to 0.8 Pa, the chromium target deposition current is 80 to 110 A, the substrate bias voltage is -100 to -150 V, and the sputtering deposition is performed for 10 to 15 minutes.

8. The preparation method according to claim 4, It is characterized in that In step S4, 30-60 sccm argon, 40-70 sccm nitrogen and 30-60 sccm oxygen are introduced into the furnace chamber, the nitrogen flow rate is adjusted, the gas pressure is 0.5-0.7 Pa, the AlCrNbSiTi high entropy alloy target bias is adjusted to -100-150 V, the deposition current is 60-110 A, the sputtering deposition is performed for 2-3 min, the rotating frame speed is adjusted to 4-6 r / min, and the sputtering deposition is performed for 2-3 min.

9. The preparation method according to claim 4, It is characterized in that In step S5, 60-100 sccm argon and 120-160 sccm oxygen are introduced into the furnace chamber, the argon flow rate is adjusted, the gas pressure is 0.4-0.8 Pa, the AlCr target bias is adjusted to -100--150 V, the deposition current is 60-90 A, and the sputtering deposition is performed for 2-5 minutes.

10. Use of the metal ceramic spectrally selective absorption coating according to claims 1 to 3 or the metal ceramic spectrally selective absorption coating prepared by the preparation method according to any one of claims 4 to 9 in solar thermal utilization.

Citation Information

Cited By

  • Pure metal / high-entropy amorphous alloy nano multilayer film with three-dimensional interface and preparation method of pure metal / high-entropy amorphous alloy nano multilayer film

    CN119615064A

  • Metal ceramic photothermal conversion coating with inclined microstructure and preparation method of metal ceramic photothermal conversion coating

    CN120719250A