Material for laser cladding of nodular iron casting and laser cladding method

By using iron-based alloy powder with specific components for laser cladding, the problem of insufficient cracks and high-temperature oxidation resistance during surface reinforcement and remanufacturing of ductile cast iron is solved, and low-cost, high-quality wear resistance and corrosion resistance are achieved. High temperature resistant cladding.

CN118957573AActive Publication Date: 2024-11-15TAIER (ANHUI) IND TECH SERVICE CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411380035.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-15
Estimated Expiration
2044-09-30

AI Technical Summary

Technical Problem

Ductile cast iron is prone to cracks, white mouths and hardened tissues during surface reinforcement and remanufacturing. The existing laser cladding materials are costly and have insufficient high-temperature oxidation resistance.

Method used

Low-cost iron-based alloy powder is used, with specific components such as C: 0.03-0.05, Si: 1.50-2.00, B: 1.0-1.5, Cr: 17.5-19.5, Mo: 5.0-6.0, Ni: 34-36, Co: 0.3 -0.5, Nb: 1.5-2.0, Ti: 0.5-1.0, Fe margin, surface treatment is carried out by laser cladding method, including cleaning, heating, laser cladding, thermal insulation and cooling and flaw detection detection.

Benefits of technology

The high-quality clad layer of ductile iron parts is achieved, with good wear resistance, corrosion resistance and high temperature resistance, avoiding cracks and white-mouth structure, and significantly reducing material costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957573A_ABST
    Figure CN118957573A_ABST
Patent Text Reader

Abstract

The invention discloses a laser cladding material for a nodular iron casting. The laser cladding material comprises the following specific components in percentage by mass: 0.03 to 0.05 percent of C, 1.50 to 2.00 percent of Si, 1.0 to 1.5 percent of B, 17.5 to 19.5 percent of Cr, 5.0 to 6.0 percent of Mo, 34 to 36 percent of Ni, 0.3 to 0.5 percent of Co, 1.5 to 2.0 percent of Nb, 0.5 to 1.0 percent of Ti and the balance of Fe. Meanwhile, the invention further discloses a laser cladding method which comprises the following steps: 1, cleaning the nodular iron casting, and carrying out PT flaw detection; 2, the nodular iron casting is heated to 100-150 DEG C; 3, the surface of the nodular iron casting is subjected to laser cladding, wherein the thickness of a single layer is 1.2-1.5 mm, and the overlap amount is 2.5 mm; 4, the asbestos-wrapped nodular iron casting is subjected to heat preservation and slow cooling; and 5, performing PT flaw detection on the nodular iron casting subjected to laser cladding. The laser cladding material for the nodular iron casting is low-cost iron-based alloy powder with plasticity, toughness and strength, it is guaranteed that the large nodular iron casting does not crack in laser cladding, meanwhile, a cladding layer has good abrasion resistance, corrosion resistance and high temperature resistance, and the material cost is remarkably reduced compared with a nickel-based material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a material for laser cladding of ductile iron and a laser cladding method. Background Art

[0002] Ductile iron is a high-strength cast iron material. Due to its excellent performance, it has been widely used in some parts with complex loads, such as automobile engine blocks, cylinder heads, crankcases, steering housings, gearbox housings and other parts. The spheroidal graphite obtained by spheroidizing and inoculating ductile iron effectively improves the mechanical properties of cast iron, especially plasticity and toughness, so it has higher strength than carbon steel. However, due to its high carbon content of 3.0% to 4.0%, ductile iron is prone to cracks, chills and hardened structures during surface strengthening and remanufacturing. Therefore, surface strengthening and remanufacturing of ductile iron parts have always been a difficult problem in the industry.

[0003] Most of the existing public technologies use low-hardness nickel-based alloy powder for laser cladding of ductile iron. Although this solves the problem of cracking of ductile iron to a certain extent, it still has problems such as high cost and low hardness of nickel-based alloy.

[0004] Patent CN 109628923 A discloses an iron-based alloy powder for laser cladding remanufacturing of ductile iron castings. The powder has a high C content of 0.8-1.2% and a Cr content of less than 12%. The disadvantages are: first, the high carbon content makes it very easy to have defects such as cracks during the laser cladding process; second, although the corrosion resistance is ensured by a relatively high Ni content, the Cr content is less than 12%, which is not conducive to the performance of the oxide film in a high temperature environment, making its high temperature oxidation resistance insufficient. Summary of the invention

[0005] The problem to be solved by the present invention is to provide a laser cladding material for ductile iron castings, which is a low-cost iron-based alloy powder with both plasticity, toughness and strength, ensuring that large ductile iron castings will not crack during laser cladding. At the same time, the cladding layer has good wear resistance, corrosion resistance and high temperature resistance, and the material cost is significantly reduced compared with nickel-based.

[0006] The invention discloses a laser cladding material for ductile iron castings, wherein the specific components and mass percentages are: C: 0.03-0.05, Si: 1.50-2.00, B: 1.0-1.5, Cr: 17.5-19.5, Mo: 5.0-6.0, Ni: 34-36, Co: 0.3-0.5, Nb: 1.5-2.0, Ti: 0.5-1.0, and Fe as a remainder.

[0007] Furthermore, the composition mass percentages of the laser cladding material are preferably: C: 0.032, Si: 1.85, B: 1.1, Cr: 18, Mo: 5.1, Ni: 36, Co: 0.4, Nb: 1.62, Ti: 0.57, and Fe as a remainder.

[0008] Furthermore, the composition mass percentages of the laser cladding material are preferably: C: 0.038, Si: 1.74, B: 1.3, Cr: 19, Mo: 5.4, Ni: 36, Co: 0.4, Nb: 1.8, Ti: 0.7, and Fe as a remainder.

[0009] Furthermore, the composition mass percentages of the laser cladding material are preferably: C: 0.045, Si: 1.66, B: 1.4, Cr: 17.8, Mo: 5.8, Ni: 35, Co: 0.5, Nb: 1.9, Ti: 0.8, and Fe as a remainder.

[0010] The invention discloses a laser cladding method for materials used for laser cladding of ductile iron parts, which comprises the following steps: 1. cleaning the ductile iron parts and performing PT flaw detection; 2. heating the ductile iron parts to 100-150° C.; 3. laser cladding the surface of the ductile iron parts: the single layer thickness is 1.2-1.5 mm, and the overlap amount is 2.5 mm; 4. wrapping the ductile iron parts with an asbestos blanket to keep them warm and cool slowly; 5. performing PT flaw detection on the ductile iron parts after laser cladding.

[0011] The advantages of the laser cladding material of the present invention are: 1. The C content is relatively low, which improves the plastic toughness, making it difficult for ductile iron parts to have defects such as cracks during the laser cladding process; 2. The Cr content is greater than 12%, which has good high-temperature oxidation resistance; 3. The Ni content is greater than 30%, which has excellent corrosion resistance and can avoid cladding white cast structure; at the same time, the Ni content is greatly reduced compared with nickel-based alloys (Ni≥50), and the cost is greatly reduced; 4. Co is added to improve strength and high-temperature oxidation resistance; 5. Nb and Ti refine the grains, improve strength and plastic toughness. Therefore, the laser cladding material of the present invention is a low-cost iron-based alloy powder with both plastic toughness and strength, which ensures that large ductile iron parts will not crack during laser cladding, and the cladding layer has good wear resistance, corrosion resistance, and high temperature resistance, and the material cost is significantly reduced compared with the nickel-based. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 It is a schematic diagram of the appearance of the cladding layer of the laser cladding material of the present invention.

[0013] Figure 2 It is a PT flaw detection diagram of the cladding layer of the laser cladding material of the present invention.

[0014] Figure 3It is a metallographic diagram of the cladding layer of the laser cladding material of the present invention. DETAILED DESCRIPTION

[0015] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0016] Example 1

[0017] The invention discloses a material for laser cladding of ductile iron castings, wherein the specific components and mass percentages are: C: 0.03-0.05, Si: 1.50-2.00, B: 1.0-1.5, Cr: 17.5-19.5, Mo: 5.0-6.0, Ni: 34-36, Co: 0.3-0.5, Nb: 1.5-2.0, Ti: 0.5-1.0, and Fe as a remainder.

[0018] Among them, the composition mass percentage of the material for laser cladding is preferably:

[0019] C: 0.032, Si: 1.85, B: 1.1, Cr: 18, Mo: 5.1, Ni: 36, Co: 0.4, Nb: 1.62, Ti: 0.57, Fe balance.

[0020] C: 0.038, Si: 1.74, B: 1.3, Cr: 19, Mo: 5.4, Ni: 36, Co: 0.4, Nb: 1.8, Ti: 0.7, Fe balance.

[0021] C: 0.045, Si: 1.66, B: 1.4, Cr: 17.8, Mo: 5.8, Ni: 35, Co: 0.5, Nb: 1.9, Ti: 0.8, Fe balance.

[0022] From the above composition, it can be seen that the advantages of the laser cladding material of the present invention are: 1. The C content is low, which improves the plastic toughness, making it difficult for ductile iron parts to have defects such as cracks during the laser cladding process; 2. The Cr content is greater than 12%, which has good high-temperature oxidation resistance; 3. The Ni content is greater than 30%, and the corrosion resistance is excellent, which can avoid the cladding white structure; at the same time, the Ni content is greatly reduced compared with the nickel-based alloy (Ni≥50), and the cost is greatly reduced; 4. Co is added to improve the strength and high-temperature oxidation resistance; 5. Nb and Ti refine the grains, improve the strength and plastic toughness. Therefore, the laser cladding material of the present invention is a low-cost iron-based alloy powder with both plastic toughness and strength, which ensures that large ductile iron parts will not crack during laser cladding. At the same time, the cladding layer has good wear resistance, corrosion resistance, and high temperature resistance, and the material cost is significantly reduced compared with the nickel-based.

[0023] Example 2

[0024] The invention discloses a laser cladding method for a material used for laser cladding of a ductile iron part, which comprises the following steps: 1. Cleaning the ductile iron part and performing PT flaw detection; 2. Heating the ductile iron part to 100-150° C.; 3. Laser cladding the surface of the ductile iron part: the single layer thickness is 1.2-1.5 mm, and the overlap amount is 2.5 mm; 4. Wrapping the ductile iron part with an asbestos blanket to keep it warm and cool it slowly; 5. Performing PT flaw detection on the ductile iron part after laser cladding.

[0025] Among them, step 2 preheating is to reduce the temperature difference of the ductile iron parts during cladding, thereby preventing the ductile iron parts from cracking; step 4 asbestos wrapping insulation slow cooling is to reduce stress and prevent the ductile iron parts from cracking.

[0026] After laser cladding of the laser cladding material of the present invention: Figure 1 It can be seen that the cladding layer is flat; Figure 2 It can be seen that there are no defects such as cracks on the surface of the cladding layer; Figure 3 It can be seen that the cladding layer has no internal defects and is well bonded to the ductile iron matrix.

[0027] Therefore, the material for laser cladding of ductile iron castings of the present invention can obtain a high-quality cladding layer with good molding, no defects such as cracks, and metallurgical bonding with the substrate through laser cladding: the cladding layer has good wear resistance, corrosion resistance, and high temperature resistance, and the material cost is significantly reduced compared with the nickel base.

Claims

1. A laser cladding material for ductile iron castings, characterized in that: Its specific composition and mass percentage are: C: 0.03-0.05, Si: 1.50-2.00, B: 1.0-1.5, Cr: 17.5-19.5, Mo: 5.0-6.0, Ni: 34-36, Co: 0.3-0.5, Nb: 1.5-2.0, Ti: 0.5-1.0, Fe balance.

2. The laser cladding material for ductile iron castings according to claim 1 is characterized in that: The composition mass percentage of the laser cladding material is preferably: C: 0.032, Si: 1.85, B: 1.1, Cr: 18, Mo: 5.1, Ni: 36, Co: 0.4, Nb: 1.62, Ti: 0.57, and Fe as the balance.

3. The laser cladding material for ductile iron castings according to claim 1 is characterized in that: The composition mass percentage of the laser cladding material is preferably: C: 0.038, Si: 1.74, B: 1.3, Cr: 19, Mo: 5.4, Ni: 36, Co: 0.4, Nb: 1.8, Ti: 0.7, and Fe balance.

4. The laser cladding material for ductile iron castings according to claim 1 is characterized in that: The composition mass percentage of the laser cladding material is preferably: C: 0.045, Si: 1.66, B: 1.4, Cr: 17.8, Mo: 5.8, Ni: 35, Co: 0.5, Nb: 1.9, Ti: 0.8, and Fe as the balance.

5. A laser cladding method for laser cladding material for ductile iron castings, characterized in that: It includes the following steps:

1. Clean the ductile iron parts and perform PT flaw detection; 2. Heat the ductile iron parts to 100-150℃; 3. Laser clad the surface of the ductile iron parts: single layer thickness 1.2-1.5mm, overlap 2.5mm; 4. Wrap the ductile iron parts with asbestos blankets for heat preservation and slow cooling; 5. Perform PT flaw detection on ductile iron parts after laser cladding.

Citation Information

Patent Citations

  • Iron-based alloy powder for nodular iron casting laser cladding remanufacturing

    CN109628923A

  • Iron-based alloy powder for laser cladding, and laser cladding method

    CN111945154A

  • Nodular cast iron bearing cylinder carbon dioxide automatic cladding remanufacturing method

    CN112025224A

  • Iron-based alloy for laser cladding and application thereof

    CN118147524A

  • Wear-resistant and corrosion-resistant iron-based alloy powder for laser cladding and laser cladding layer thereof

    JP6896138B1