Magnesium alloy micro-arc oxidation composite nanometer electrophoresis coating process
Through the microarc oxidation composite nanoelectrophoresis process of magnesium alloy, a uniform and dense oxide film is formed and the electrophoretic paint is uniformly distributed, which solves the corrosion problem of magnesium alloy materials in humid environments, improves its corrosion resistance and optical properties, and is suitable for high-quality Required optical applications.
Patent Information
- Application Number
- CN202411016411.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-27
- Publication Date
- 2024-11-15
AI Technical Summary
Magnesium alloy materials are prone to oxidation and corrosion in humid and corrosive environments. Traditional coating technology is difficult to meet its corrosion resistance, optical properties and color uniformity requirements, limiting its applications in aerospace, automobile manufacturing and optical fields.
The coating process of magnesium alloy microarc oxidation composite nanoelectrophoresis is adopted to form a uniform and dense oxide film through microarc oxidation treatment, and nanoelectrophoresis technology makes the electrophoretic paint evenly distributed in the micropores of the oxide film layer, forming a flat, smooth and Composite coating with uniform color.
It significantly improves the corrosion resistance and optical properties of magnesium alloys, extends its service life, and improves the adhesion and weather resistance of the coating, and is suitable for high-demand applications in the optical industry.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal surface treatment, in particular to a coating process of magnesium alloy micro-arc oxidation composite nano-electrophoresis. Background Art
[0002] In the field of surface treatment of magnesium alloy materials, although traditional coating technology has made certain progress, it still faces many challenges in practical application. As a lightweight, high-strength metal material, magnesium alloy is widely used in aerospace, automobile manufacturing, electronic communications and other fields. However, due to its active chemical properties, magnesium alloy is prone to oxidation and corrosion in humid and corrosive environments, which seriously limits its service life and application range.
[0003] Traditional magnesium alloy surface treatment methods, such as spraying and electroplating, can improve the corrosion resistance of magnesium alloy to a certain extent, but often have problems such as poor coating uniformity, insufficient adhesion, and difficult to control coating thickness. Especially in terms of the bonding strength between the coating and the substrate, due to the high surface energy of magnesium alloy, the coating is easy to peel off, resulting in unstable coating performance and difficulty in meeting the needs of long-term use. At present, ordinary electrophoretic film layers are generally 15-20 microns, and spray paint is thicker, generally 20 to 50 microns, so it is not suitable for precise size assembly of optical lenses.
[0004] In addition, with the continuous advancement of science and technology and the development of the industry, the requirements for magnesium alloy surface coatings are becoming higher and higher. Especially in the optical industry, there are more stringent requirements for the optical properties, color uniformity, reflectivity, etc. of the coating. Traditional coating technology often finds it difficult to meet these requirements at the same time, which limits the application of magnesium alloys in the optical field.
[0005] Therefore, developing a new magnesium alloy surface treatment technology that can improve the corrosion resistance of magnesium alloys while meeting the requirements for coating optical properties, color uniformity, etc. has become an urgent problem to be solved in the current magnesium alloy surface treatment field. Summary of the invention
[0006] Technical issues solved
[0007] In view of the above-mentioned shortcomings of the prior art, the present invention provides a coating process of micro-arc oxidation composite nano-electrophoresis of magnesium alloy. Through micro-arc oxidation treatment, a uniform and dense micro-arc oxidation film can be formed on the surface of the magnesium alloy substrate. This oxide film has good chemical stability and barrier properties, and can effectively prevent the corrosive medium in the external environment from directly contacting the magnesium alloy substrate, thereby reducing the corrosion rate of the magnesium alloy and significantly improving its corrosion resistance. By utilizing nano-electrophoretic coating technology, the electrophoretic paint can be evenly distributed and penetrated in the micropores of the micro-arc oxidation film layer to form a flat, smooth and uniformly colored composite coating. This coating not only has a good decorative effect and can improve the aesthetics of magnesium alloy products, but also has good adhesion and weather resistance, and can maintain stable surface properties under various environments.
[0008] Technical Solution
[0009] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0010] A coating process of magnesium alloy micro-arc oxidation composite nano-electrophoresis, the process includes three main steps of pretreatment of magnesium alloy substrate, micro-arc oxidation treatment and nano-electrophoresis coating, wherein the magnesium alloy substrate is cleaned and degreased in the pretreatment step to ensure the purity of the substrate surface; the micro-arc oxidation treatment step forms a uniform micro-arc oxidation film on the surface of the magnesium alloy substrate through specific voltage, time, frequency and duty cycle parameters; the nano-electrophoresis coating step uses nano-scale electrophoretic paint, and the electrophoretic paint is uniformly penetrated into the micropores of the micro-arc oxidation film layer through positive and negative pulse power supplies to form a composite coating.
[0011] Furthermore, the micro-arc oxidation treatment step is divided into two stages. The first stage uses a voltage of 350V, a treatment time of 5-10 minutes, a frequency between 600-1200Hz, and a duty cycle controlled at 5%-20% to form an initial micro-arc oxidation film on the surface of the magnesium alloy substrate; the second stage is an activation treatment, the voltage is reduced to 250V, the treatment time is 2-3 minutes, the frequency is maintained at 600-1200Hz, and the duty cycle is set to 5% to further activate the micro-arc oxidation film layer in preparation for subsequent electrophoretic coating.
[0012] Furthermore, the electrophoretic paint used in the nano-electrophoretic coating step is a nano-scale electrophoretic paint, which has excellent permeability and adhesion, and can evenly and effectively penetrate into the micropores of the micro-arc oxidation film layer to form a uniform and dense composite coating.
[0013] Furthermore, the power supply used in the nano-electrophoretic coating step is a positive and negative pulse power supply, which generates alternating positive and negative pulse currents, promoting the uniform distribution and penetration of the electrophoretic paint in the micro-arc oxidation film layer, thereby obtaining a higher quality composite coating.
[0014] Furthermore, the formed composite coating has a black, matte appearance, and its reflectivity is controlled within the range of 3-10%, and has good optical properties, which is suitable for application requirements of the optical industry.
[0015] Furthermore, the thickness of the formed composite coating is in the range of 8-16 microns, and the coating has excellent corrosion resistance, which can significantly improve the corrosion resistance of the magnesium alloy substrate and extend its service life.
[0016] Furthermore, the pretreatment step of the magnesium alloy substrate also includes surface roughening or etching treatment to increase the bonding force between the micro-arc oxidation film layer and the substrate, thereby improving the adhesion and durability of the coating.
[0017] Furthermore, after the nano-electrophoretic coating step, the coating is post-treated, including curing and polishing, to further improve the surface quality and performance of the coating.
[0018] Furthermore, the specific process of the process is:
[0019] S100, pretreatment of magnesium alloy substrate:
[0020] S101, cleaning: thoroughly clean the magnesium alloy substrate to remove oil, dust and other impurities on the surface to ensure the purity of the substrate surface;
[0021] S102, degreasing: degreasing treatment is performed, and appropriate degreasing agents and methods are used to further remove oil stains on the surface of the substrate to provide a clean and dry substrate for subsequent coating processes;
[0022] S103, surface roughening or etching: in the pretreatment step, the surface of the substrate is roughened or etched to increase the bonding force between the micro-arc oxidation film layer and the substrate, thereby improving the adhesion and durability of the coating;
[0023] S200, micro-arc oxidation treatment:
[0024] S201, initial micro-arc oxidation: In the first stage, a voltage of 350V is used, the processing time is 5-10 minutes, the frequency is between 600-1200Hz, and the duty cycle is controlled at 5%-20%. Through this stage of treatment, an initial micro-arc oxidation film is formed on the surface of the magnesium alloy substrate;
[0025] S202, activation treatment: Entering the second stage, namely the activation treatment stage, the voltage is reduced to 250V, the treatment time is 2-3 minutes, the frequency is maintained at 600-1200Hz, and the duty cycle is set to 5%. This stage is to further activate the micro-arc oxidation film layer to prepare for the subsequent electrophoretic coating step;
[0026] S300, nano electrophoretic coating:
[0027] S301, nano-level electrophoretic paint selection: select nano-level electrophoretic paint with excellent permeability and adhesion to ensure that the electrophoretic paint can evenly and effectively penetrate into the micropores of the micro-arc oxidation film layer;
[0028] S302, application of positive and negative pulse power supply: electrophoretic coating is carried out using positive and negative pulse power supply, which generates positive and negative alternating pulse current to promote the uniform distribution and penetration of electrophoretic paint in the micro-arc oxidation film layer, thereby obtaining a higher quality composite coating;
[0029] S400, post-processing:
[0030] S401, curing: after the nano-electrophoretic coating step, the coating is cured to improve the hardness and wear resistance of the coating;
[0031] S402, polishing: polishing the cured coating to further improve the surface quality and appearance of the coating, making it smoother and brighter.
[0032] 10. The coating process of magnesium alloy micro-arc oxidation composite nano-electrophoresis according to claim 8, characterized in that the specific steps of cleaning in step S101 are:
[0033] Preparation: Wear appropriate protective equipment, including gloves and goggles, and ensure that the work area is well ventilated;
[0034] Select cleaning agent: According to the degree of oil, dust and other impurities on the magnesium alloy substrate, select a suitable cleaning agent, including but not limited to neutral cleaning agent and deionized water;
[0035] Cleaning operation:
[0036] Use a soft brush or sponge to dip the cleaning agent and gently scrub the surface of the magnesium alloy substrate to ensure that the oil, dust and other impurities on the surface are removed. For stains that are difficult to clean, the amount of cleaning agent used can be appropriately increased or the cleaning time can be extended. During the cleaning process, the temperature of the cleaning agent and clean water should be kept appropriate, and should not be overheated or overcooled. Rinse the residual cleaning agent on the surface of the magnesium alloy substrate with clean water to ensure that there is no cleaning agent residue on the surface. Use a clean towel or cotton cloth to wipe the moisture on the surface of the magnesium alloy substrate to ensure that the substrate is dry;
[0037] The specific steps of degreasing in step S102 are:
[0038] Preparation: Wear appropriate protective equipment and ensure that the work area is well ventilated;
[0039] Degreasing operation: add 2 / 3 of the prepared solution of water into the tank, then add the required amount of magnesium alloy degreasing agent, stir to dissolve, put the magnesium alloy substrate into the degreasing agent solution, make sure the substrate is completely immersed in the solution, stir or shake the solution to make the degreasing agent fully contact and react with the oil stains on the surface of the substrate;
[0040] Rinse: Rinse the degreaser on the surface of the magnesium alloy substrate with clean water to ensure that there is no degreaser residue on the surface;
[0041] Drying: Use a clean towel or cotton cloth to wipe the moisture off the surface of the magnesium alloy substrate to ensure that the substrate is dry;
[0042] The specific steps of the surface roughening or etching step S103 are as follows:
[0043] Preparation: Wear appropriate protective equipment and ensure that the work area is well ventilated;
[0044] Roughening or etching operations:
[0045] For mechanical roughening, the surface of the magnesium alloy substrate can be polished or sandblasted with sandpaper and a sandblasting machine to make the surface rough; for chemical etching, an appropriate etchant can be selected and the magnesium alloy substrate can be immersed in the etchant for a certain period of time to make the surface chemically react and roughen;
[0046] Cleaning and drying: After roughening or etching, rinse the residue on the surface of the magnesium alloy substrate with clean water and wipe it dry with a clean towel or cotton cloth.
[0047] Beneficial Effects
[0048] Compared with the known public technology, the technical solution provided by the present invention has the following advantages:
[0049] Beneficial effects:
[0050] 1. The present invention can form a uniform and dense micro-arc oxidation film on the surface of the magnesium alloy substrate through micro-arc oxidation treatment. This oxide film has good chemical stability and barrier properties, and can effectively prevent corrosive media (such as moisture, oxygen, acid rain, etc.) in the external environment from directly contacting the magnesium alloy substrate, thereby reducing the corrosion rate of the magnesium alloy and significantly improving its corrosion resistance. In addition, the nano-scale electrophoretic paint used in the nano-electrophoretic coating step can further fill the micropores of the micro-arc oxidation film layer to form a denser composite coating, further enhancing the corrosion resistance of the magnesium alloy.
[0051] 2. The oxide film formed on the surface of the magnesium alloy substrate by micro-arc oxidation treatment in the present invention has high hardness and wear resistance. In the subsequent nano-electrophoretic coating process, the penetration and curing of the nano-level electrophoretic paint can further enhance this characteristic. The nanoparticles in the composite coating can significantly improve the hardness and wear resistance of the coating, making the magnesium alloy material treated by this process less susceptible to scratches or wear when subjected to external mechanical effects, thereby extending its service life.
[0052] 3. By utilizing nano-electrophoretic coating technology, the electrophoretic paint can be evenly distributed and penetrated in the micropores of the micro-arc oxidation film layer to form a flat, smooth and uniformly colored composite coating. This coating not only has a good decorative effect and can improve the aesthetics of magnesium alloy products, but also has good adhesion and weather resistance, and can maintain stable surface properties under various environments. In addition, the selection and application of nano-level electrophoretic paint can also give the coating more functional properties, such as self-cleaning and antibacterial, further expanding the application field of magnesium alloy products. DETAILED DESCRIPTION
[0053] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution in the present invention is described clearly and completely. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0054] The present invention will be further described below in conjunction with the embodiments.
[0055] A coating process of magnesium alloy micro-arc oxidation composite nano-electrophoresis, the specific process of the process is:
[0056] S100, pretreatment of magnesium alloy substrate:
[0057] S101, cleaning: thoroughly clean the magnesium alloy substrate to remove oil, dust and other impurities on the surface to ensure the purity of the substrate surface;
[0058] S102, degreasing: degreasing treatment is performed, and appropriate degreasing agents and methods are used to further remove oil stains on the surface of the substrate to provide a clean and dry substrate for subsequent coating processes;
[0059] S103, surface roughening or etching: in the pretreatment step, the surface of the substrate is roughened or etched to increase the bonding force between the micro-arc oxidation film layer and the substrate, thereby improving the adhesion and durability of the coating;
[0060] S200, micro-arc oxidation treatment:
[0061] S201, initial micro-arc oxidation: In the first stage, a voltage of 350V is used, the processing time is 5-10 minutes, the frequency is between 600-1200Hz, and the duty cycle is controlled at 5%-20%. Through this stage of treatment, an initial micro-arc oxidation film is formed on the surface of the magnesium alloy substrate;
[0062] S202, activation treatment: Entering the second stage, namely the activation treatment stage, the voltage is reduced to 250V, the treatment time is 2-3 minutes, the frequency is maintained at 600-1200Hz, and the duty cycle is set to 5%. This stage is to further activate the micro-arc oxidation film layer to prepare for the subsequent electrophoretic coating step;
[0063] S300, nano electrophoretic coating:
[0064] S301, nano-level electrophoretic paint selection: select nano-level electrophoretic paint with excellent permeability and adhesion to ensure that the electrophoretic paint can evenly and effectively penetrate into the micropores of the micro-arc oxidation film layer;
[0065] S302, application of positive and negative pulse power supply: electrophoretic coating is carried out using positive and negative pulse power supply, which generates positive and negative alternating pulse current to promote the uniform distribution and penetration of electrophoretic paint in the micro-arc oxidation film layer, thereby obtaining a higher quality composite coating;
[0066] S400, post-processing:
[0067] S401, curing: after the nano-electrophoretic coating step, the coating is cured to improve the hardness and wear resistance of the coating;
[0068] S402, polishing: polishing the cured coating to further improve the surface quality and appearance of the coating, making it smoother and brighter.
[0069] Example 1: Magnesium alloy micro-arc oxidation composite nano-electrophoretic coating of optical lenses
[0070] In the optical industry, optical lenses have extremely high requirements on the reflectivity and uniformity of the surface. In order to meet these requirements, a magnesium alloy micro-arc oxidation composite nano-electrophoresis coating process is used to treat the surface of magnesium alloy optical lenses.
[0071] Implementation steps:
[0072] Pretreatment: First, the magnesium alloy optical lens is thoroughly cleaned and degreased to ensure that the lens surface is free of oil, dust and other impurities. Then, the surface is roughened to increase the bonding strength between the micro-arc oxidation film and the substrate.
[0073] Micro-arc oxidation treatment: It is divided into two stages. In the first stage, a voltage of 350V is used, the treatment time is 8 minutes, the frequency is 900Hz, and the duty cycle is 10% to form an initial micro-arc oxidation film. In the second stage, the voltage is reduced to 250V, the treatment time is 2 minutes, the frequency is maintained at 900Hz, and the duty cycle is 5% for activation treatment.
[0074] Nano-electrophoretic coating: Select nano-level electrophoretic paint with excellent permeability and adhesion, and use positive and negative pulse power supplies for electrophoretic coating to ensure that the electrophoretic paint penetrates evenly and effectively into the micropores of the micro-arc oxidation film layer to form a composite coating.
[0075] Post-treatment: The coating is cured to improve its hardness and wear resistance, followed by polishing to make the coating surface smoother and brighter, with the reflectivity controlled at around 5%.
[0076] Results: The optical lens treated by the above process has a uniform surface reflectivity, and the reflectivity is controlled at about 5%, which meets the application requirements of the optical industry. At the same time, the coating has excellent corrosion resistance and can significantly improve the corrosion resistance of the magnesium alloy substrate.
[0077] Example 2: Magnesium alloy shell coating for optical instruments
[0078] In order to improve the appearance quality and corrosion resistance of optical instruments, the shell is treated with magnesium alloy micro-arc oxidation composite nano-electrophoresis coating process.
[0079] Implementation steps:
[0080] Pretreatment: Clean, degrease and roughen the surface of the magnesium alloy shell to ensure the quality of coating.
[0081] Micro-arc oxidation treatment: The same micro-arc oxidation treatment parameters as those in Example 1 were used to form a uniform micro-arc oxidation film.
[0082] Nano-electrophoretic coating: Use black nano-level electrophoretic paint and use positive and negative pulse power to perform electrophoretic coating to form a black, matte composite coating.
[0083] Post-treatment: The coating is cured and then polished to make the coating surface smoother and brighter.
[0084] Results: The coated optical instrument housing has a black, matte surface, and the reflectivity is controlled within the range of 3-10%. It has good optical properties. At the same time, the coating has excellent corrosion resistance and can significantly extend the service life of the optical instrument.
[0085] Example 3: Magnesium alloy substrate coating for optical sensor
[0086] Optical sensors have high requirements on the surface quality and corrosion resistance of the substrate. In order to improve the performance of the sensor, the magnesium alloy micro-arc oxidation composite nano-electrophoresis coating process is used to treat the substrate surface.
[0087] Implementation steps:
[0088] Pretreatment: Clean, degrease and surface etch the magnesium alloy substrate to increase the bonding strength between the micro-arc oxidation film and the substrate.
[0089] Micro-arc oxidation treatment: The same micro-arc oxidation treatment parameters as those in Example 1 were used to form a uniform micro-arc oxidation film.
[0090] Nano-electrophoretic coating: Select nano-level electrophoretic paint with excellent adhesion and corrosion resistance, and use positive and negative pulse power supply for electrophoretic coating to form a composite coating.
[0091] Post-treatment: Curing the coating to improve its hardness and wear resistance.
[0092] Results: The optical sensor substrate after coating has high surface quality, uniform and dense coating. The coating has excellent corrosion resistance and can significantly improve the service life and reliability of the optical sensor.
[0093] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A coating process of magnesium alloy micro-arc oxidation composite nano-electrophoresis, characterized in that: The process includes three main steps: pretreatment of the magnesium alloy substrate, micro-arc oxidation treatment and nano-electrophoretic coating. The magnesium alloy substrate is cleaned and degreased in the pretreatment step to ensure the purity of the substrate surface; the micro-arc oxidation treatment step forms a uniform micro-arc oxidation film on the surface of the magnesium alloy substrate through specific voltage, time, frequency and duty cycle parameters; the nano-electrophoretic coating step uses nano-scale electrophoretic paint, and uses positive and negative pulse power supplies to make the electrophoretic paint evenly penetrate into the micropores of the micro-arc oxidation film layer to form a composite coating.
2. The coating process of magnesium alloy micro-arc oxidation composite nano-electrophoresis according to claim 1 is characterized in that: The micro-arc oxidation treatment step is divided into two stages. The first stage uses a voltage of 350V, a treatment time of 5-10 minutes, a frequency between 600-1200Hz, and a duty cycle controlled at 5%-20% to form an initial micro-arc oxidation film on the surface of the magnesium alloy substrate; the second stage is an activation treatment, the voltage is reduced to 250V, the treatment time is 2-3 minutes, the frequency is maintained at 600-1200Hz, and the duty cycle is set to 5% to further activate the micro-arc oxidation film layer to prepare for subsequent electrophoretic coating.
3. The coating process of magnesium alloy micro-arc oxidation composite nano-electrophoresis according to claim 1 is characterized in that: The electrophoretic paint used in the nano-electrophoretic coating step is a nano-scale electrophoretic paint, which has excellent permeability and adhesion, and can evenly and effectively penetrate into the micropores of the micro-arc oxidation film layer to form a uniform and dense composite coating.
4. The coating process of magnesium alloy micro-arc oxidation composite nano-electrophoresis according to claim 3 is characterized in that: The power supply used in the nano-electrophoretic coating step is a positive and negative pulse power supply, which generates alternating positive and negative pulse currents, promoting the uniform distribution and penetration of the electrophoretic paint in the micro-arc oxidation film layer, thereby obtaining a higher quality composite coating.
5. The coating process of magnesium alloy micro-arc oxidation composite nano-electrophoresis according to claim 1, characterized in that: The formed composite coating has a black, matte appearance, and its reflectivity is controlled within the range of 3-10%. It has good optical properties and is suitable for application requirements in the optical industry.
6. The coating process of magnesium alloy micro-arc oxidation composite nano-electrophoresis according to claim 1 is characterized in that: The thickness of the formed composite coating is in the range of 8-16 microns. The coating has excellent corrosion resistance, can significantly improve the corrosion resistance of the magnesium alloy substrate, and prolong its service life.
7. The coating process of magnesium alloy micro-arc oxidation composite nano-electrophoresis according to claim 1 is characterized in that: The pretreatment step of the magnesium alloy substrate also includes surface roughening or etching treatment to increase the bonding force between the micro-arc oxidation film layer and the substrate, thereby improving the adhesion and durability of the coating.
8. The coating process of magnesium alloy micro-arc oxidation composite nano-electrophoresis according to claim 1 is characterized in that: After the nano-electrophoretic coating step, the coating is also post-processed, including curing and polishing, to further improve the surface quality and performance of the coating.
9. A magnesium alloy micro-arc oxidation composite nano-electrophoresis coating process according to any one of claims 1 to 8, characterized in that: The specific process of this process is: S100, pretreatment of magnesium alloy substrate: S101, cleaning: thoroughly clean the magnesium alloy substrate to remove oil, dust and other impurities on the surface to ensure the purity of the substrate surface; S102, degreasing: degreasing treatment is performed, and appropriate degreasing agents and methods are used to further remove oil stains on the surface of the substrate to provide a clean and dry substrate for subsequent coating processes; S103, surface roughening or etching: in the pretreatment step, the surface of the substrate is roughened or etched to increase the bonding force between the micro-arc oxidation film layer and the substrate, thereby improving the adhesion and durability of the coating; S200, micro-arc oxidation treatment: S201, initial micro-arc oxidation: In the first stage, a voltage of 350V is used, the processing time is 5-10 minutes, the frequency is between 600-1200Hz, and the duty cycle is controlled at 5%-20%. Through this stage of treatment, an initial micro-arc oxidation film is formed on the surface of the magnesium alloy substrate; S202, activation treatment: Entering the second stage, namely the activation treatment stage, the voltage is reduced to 250V, the treatment time is 2-3 minutes, the frequency is maintained at 600-1200Hz, and the duty cycle is set to 5%. This stage is to further activate the micro-arc oxidation film layer to prepare for the subsequent electrophoretic coating step; S300, nano electrophoretic coating: S301, nano-level electrophoretic paint selection: select nano-level electrophoretic paint with excellent permeability and adhesion to ensure that the electrophoretic paint can evenly and effectively penetrate into the micropores of the micro-arc oxidation film layer; S302, application of positive and negative pulse power supply: electrophoretic coating is carried out using positive and negative pulse power supply, which generates positive and negative alternating pulse current to promote the uniform distribution and penetration of electrophoretic paint in the micro-arc oxidation film layer, thereby obtaining a higher quality composite coating; S400, post-processing: S401, curing: after the nano-electrophoretic coating step, the coating is cured to improve the hardness and wear resistance of the coating; S402, polishing: polishing the cured coating to further improve the surface quality and appearance of the coating, making it smoother and brighter.
10. The coating process of magnesium alloy micro-arc oxidation composite nano-electrophoresis according to claim 8, characterized in that: The specific steps of cleaning in step S101 are: Preparation: Wear appropriate protective equipment, including gloves and goggles, and ensure that the work area is well ventilated; Select cleaning agent: According to the degree of oil, dust and other impurities on the magnesium alloy substrate, select a suitable cleaning agent, including but not limited to neutral cleaning agent and deionized water; Cleaning operation: Use a soft brush or sponge to dip the cleaning agent and gently scrub the surface of the magnesium alloy substrate to ensure that the oil, dust and other impurities on the surface are removed. For stains that are difficult to clean, the amount of cleaning agent used can be appropriately increased or the cleaning time can be extended. During the cleaning process, the temperature of the cleaning agent and clean water should be kept appropriate, and should not be overheated or overcooled. Rinse the residual cleaning agent on the surface of the magnesium alloy substrate with clean water to ensure that there is no cleaning agent residue on the surface. Use a clean towel or cotton cloth to wipe the moisture on the surface of the magnesium alloy substrate to ensure that the substrate is dry; The specific steps of degreasing in step S102 are: Preparation: Wear appropriate protective equipment and ensure that the work area is well ventilated; Degreasing operation: add 2 / 3 of the prepared solution of water into the tank, then add the required amount of magnesium alloy degreasing agent, stir to dissolve, put the magnesium alloy substrate into the degreasing agent solution, make sure the substrate is completely immersed in the solution, stir or shake the solution to make the degreasing agent fully contact and react with the oil stains on the surface of the substrate; Rinse: Rinse the degreaser on the surface of the magnesium alloy substrate with clean water to ensure that there is no degreaser residue on the surface; Drying: Use a clean towel or cotton cloth to wipe the moisture off the surface of the magnesium alloy substrate to ensure that the substrate is dry; The specific steps of the surface roughening or etching step S103 are as follows: Preparation: Wear appropriate protective equipment and ensure that the work area is well ventilated; Roughening or etching operations: For mechanical roughening, the surface of the magnesium alloy substrate can be polished or sandblasted with sandpaper and a sandblasting machine to make the surface rough; for chemical etching, an appropriate etchant can be selected and the magnesium alloy substrate can be immersed in the etchant for a certain period of time to make the surface chemically react and roughen; Cleaning and drying: After roughening or etching, rinse the residue on the surface of the magnesium alloy substrate with clean water and wipe it dry with a clean towel or cotton cloth.
Citation Information
Cited By
Ceramization composite process applied to metal substrate
WO2026129408A1