Graphene modified UHPC and steel slag epoxy asphalt electric heating integrated combination system for steel bridge deck

Through the integrated electric heating combination system of graphene modified UHPC and steel slag epoxy asphalt, combined with SBS modified asphalt layer and hot melt particle layer, a bridge deck system with low resistivity and high thermal conductivity is formed, which solves the freeze-thawing of the bridge deck in ice and snow The efficiency and intensity of ice and snow melting under conditions have achieved efficient ice and snow melting and stability of the bridge deck under freeze-thawing conditions.

CN118958131AInactive Publication Date: 2024-11-15SUZHOU SANJIATRAFFIC ENG PRESTRESS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411192679.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing bridges are prone to damage during the freeze-thawing process of ice and snow in winter, and conductive blends affect the strength of the road surface, making it difficult to achieve both low resistivity and high freeze-thaw resistance.

Method used

The integrated electric heating combination system of graphene modified UHPC and steel slag epoxy asphalt is adopted. The combination of SBS modified asphalt layer, hot melt particle layer, epoxy resin layer, UHPC structural layer and steel mesh layer is combined with the welding structure to form a low Bridge deck system with resistivity and high thermal conductivity.

Benefits of technology

It realizes efficient ice and snow melting of the bridge deck under freeze-thawing conditions, maintains the strength and stability of the bridge deck, reduces the resistivity, enhances the anti-freeze-thaw damage performance, and solves the problems of both conductivity and strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005015516070000011
    Figure HDA0005015516070000011
  • Figure HDA0005015516070000021
    Figure HDA0005015516070000021
  • Figure HDA0005015516070000031
    Figure HDA0005015516070000031
Patent Text Reader

Abstract

The invention relates to the field of bridge construction, in particular to a graphene modified UHPC and steel slag epoxy asphalt electric heating integrated combined system for a steel bridge deck. The combination system sequentially comprises a styrene-butadiene-styrene block copolymer (SBS) modified asphalt layer, a hot melting particle layer, an epoxy resin layer, an ultra-high performance concrete (UHPC) structure layer, a reinforcing mesh layer and a steel bridge deck slab layer from top to bottom, steel slag is further mixed in the SBS modified asphalt layer, and welding studs are welded between the reinforcing mesh layer and the steel bridge deck slab layer. The ultra-high performance concrete (UHPC) structure layer is modified by graphene, and the steel slag doped in the SBS modified asphalt layer is silane coupling agent modified steel slag. The graphene modified UHPC and steel slag epoxy asphalt electric heating integrated combination system is low in resistivity, high in freeze-thaw damage resistance and suitable for electric heating snow melting and deicing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of bridge construction, and more specifically, it relates to a graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated combination system for steel bridge decks. Background Art

[0002] In order to solve the problem of road icing and snow accumulation in winter, most countries in the world use snow removal equipment or spray industrial salt water / de-snowing agents to clear snow. However, manual snow removal is time-consuming and labor-intensive, and industrial salt water / de-snowing agents will cause environmental pollution and road damage. The technology of adding a certain amount of elastic granular material to the pavement paving material, utilizing the strong local deformation ability of the elastic material, and breaking and melting the ice and snow on the road surface through the self-stress generated by the road surface under load has limited anti-snow and ice melting ability. The technology of adding conductive admixtures to the pavement paving material to heat the pavement to melt snow and ice requires the pavement / bridge deck to experience repeated freezing and thawing, and has high requirements for the mechanical strength of the pavement / bridge deck. Too much conductive admixture is likely to affect the strength of the pavement paving material, while insufficient addition will not effectively generate heat due to the large resistivity of the pavement. How to provide a bridge deck combination system that has both low resistance to achieve high-efficiency temperature rise after power-on and high resistance to freeze-thaw damage, and maintains high strength after repeated freezing and thawing is a problem to be solved. Summary of the invention

[0003] In order to solve the problem of steel bridge decks having both low resistance and high resistance to freeze-thaw damage, the present application provides a graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated combination system for steel bridge decks.

[0004] The present application provides a graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated combination system for steel bridge decks, which includes, from top to bottom: a styrene-butadiene-styrene block copolymer (SBS) modified asphalt layer, a hot-melt particle layer, an epoxy resin layer, an ultra-high performance concrete (UHPC) structural layer, a steel mesh layer and a steel bridge deck layer, wherein steel slag is also mixed in the SBS modified asphalt layer, and welding nails are welded between the steel mesh layer and the steel bridge deck layer.

[0005] By adopting the above technical solution, styrene-butadiene-styrene block copolymer (SBS) modified asphalt has high elasticity and fatigue resistance, does not crack at low temperature, and by using SBS modified asphalt as the surface layer of the composite system, it can withstand the wheel load and wear on the bridge, and the front performance of the steel bridge deck composite system is not easy to deteriorate and damage under ice and snow freeze-thaw and large temperature difference changes. Paving the hot-melt particle layer under the asphalt layer makes the thickness of the composite system more uniform, the stress absorption is more uniform, and the load of the bridge deck is better transmitted to the main structure of the bridge, reducing the damage to the bridge deck, and also reducing the requirements of the composite system for the construction process. The steel bridge deck is not easy to crack due to fatigue or freeze-thaw temperature difference, and the volume is more stable. After the particles are hot-melted, they can form secondary solidification, making the physical and chemical bonding between the asphalt layer and the underlying epoxy resin layer and UHPC structural layer more firm and tight. After the steel bridge deck system is frozen and thawed, snow water is not easy to flow into and stay in the steel bridge deck layer, and it is not easy to produce peeling and base top scouring under repeated loads. By adding the epoxy resin layer, the bonding strength of the SBS modified asphalt layer, the hot melt particle layer and the UHPC structural layer is further improved, the steel bridge deck system is more solid and tight, the capillary water caused by bubbles and pores is reduced, cracking, slipping and delamination are not easy to occur between the pavement layers, and the steel bridge deck system has a lower resistivity. The ultra-low micro-strain performance of UHPC effectively reduces the risk of cracking caused by the inconsistent expansion coefficients of the steel bridge deck and the asphalt system. The volume of the steel bridge deck system is more stable and the anti-freeze-thaw damage performance is better. The steel mesh layer and the steel bridge deck layer are welded by welding nails, the construction process is simple and the connection effect is good. The conductive property of the steel bridge deck can solve the technical problem of pre-embedded conductive electrodes in UHPC. By mixing steel slag into the SBS modified asphalt layer, the resistivity is further reduced, the thermal conductivity of the asphalt layer is improved, and the heat brought by the electric heating UHPC can be effectively utilized to achieve high-efficiency temperature rise, effectively improving the efficiency of road ice and snow melting.

[0006] In a specific embodiment, the steel slag blended in the SBS modified asphalt layer is steel slag modified with a silane coupling agent.

[0007] The stability of steel slag can be improved by water bath treatment, acetic acid treatment, silane coupling agent treatment and natural aging. However, the water bath treatment and natural aging treatment are slow, and the steel slag that has been placed naturally for 6 months has not been fully aged. The acetic acid treatment of steel slag will produce ferrite, and there will be acetic acid residue in the acetic acid treatment liquid, which will affect the mechanical properties of the asphalt layer. Silane-modified steel slag forms a layer of black polysiloxane polymer on the surface of the steel slag, which prevents the steel slag from contacting with water, reduces the water absorption rate of the steel slag, and improves the stability of the steel slag. The steel bridge deck prepared is not easy to crack due to water storage. Since the steel slag itself is alkaline and has high roughness, the bonding strength between the steel slag and the asphalt is high. After the silane coupling agent treatment, the bonding strength between the steel slag and the asphalt is further significantly improved, and the prepared asphalt layer is more compact and not easy to crack, further reducing the bubbles and defects in the combined system, and the resistivity of the prepared combined system is low.

[0008] In a specific embodiment, the ultra-high performance concrete (UHPC) structural layer is modified with graphene, and the modification steps include: S1: Put carbon fiber into sand and stir for 2-4 minutes to obtain carbon fiber sand; S2: Mix cement, graphene, powdered water reducer, defoamer and water evenly, stir for 80-100s, then pour in the carbon fiber sand and methyl cellulose ether prepared in S1 and continue to stir for 80-100s, finally add water and continue to stir for 80-100s to obtain mortar; S3: pour the mortar prepared in S2 evenly and cure it for 3-28 days to obtain a graphene-modified ultra-high performance concrete (UHPC) structural layer.

[0009] Since the raw materials in UHPC are very fine in particle size and difficult to mix evenly, the mixing method is an important factor affecting the performance of the graphene-modified UHPC structural layer. Therefore, in order to give full play to the advantages of UHPC, the above-mentioned mixing method and mixing time are adopted to control the uniform distribution of graphene and carbon fiber in the UHPC structural layer to form a conductive network to ensure that it has good conductivity and low resistivity. A certain amount of powdered water reducer and defoamer are also added to improve the fluidity of concrete and control the generation of foam in the cement mortar system during the mixing process. The obtained graphene-modified ultra-high performance concrete (UHPC) structural layer is uniform and dense, and is tightly coated on the steel mesh layer. Adding a certain amount of methyl cellulose ether further improves the density of the graphene-modified ultra-high performance concrete (UHPC) structural layer and the tightness of the steel mesh layer. The obtained combined system has good anti-freeze-thaw damage performance, low resistivity, and still has high strength after repeated freezing and thawing.

[0010] In a specific embodiment, in a specific embodiment, the melt index (MI) of the hot melt particles is 12-25.

[0011] By adopting the above technical scheme, the melting point of the hot-melt particles is limited, and the obtained hot-melt particle layer has both high strength and good fluidity, which is suitable for the combined system of the present application. The obtained hot-melt particle layer is tightly connected with the asphalt layer and the epoxy resin layer without pores, providing dual guarantees of mechanical bite and chemical bond reaction at high temperature, making it less prone to water penetration, and the resistivity of the combined system is lower, and the anti-freeze and thaw performance is better.

[0012] In a specific embodiment, the thickness of the SBS modified asphalt layer is 35-45 mm, and the amount of hot-melt particles in the hot-melt particle layer is 0.5-0.9 kg / m 2 The epoxy resin dosage of the epoxy resin layer is 0.3-0.7kg / m 2 The thickness of the UHPC structure layer is 55-65mm, the diameter of the steel bars of the steel mesh is 12-20mm, and the center distance between adjacent steel bars is ≤100mm.

[0013] By adopting the above technical scheme, the present application limits the thickness of each surface layer of the combined system, so that the surface layers of the combined system are well matched, tightly combined, not easy to penetrate water, not easy to crack, with low resistivity, and can better conduct heat to the steel bridge deck to resist snow and ice melting.

[0014] In a specific embodiment, the silane coupling agent modified steel slag is epoxy silane coupling agent modified steel slag.

[0015] By adopting the above technical scheme, the epoxysilane coupling agent modified steel slag has higher bonding strength due to its more epoxy groups, and the steel slag is tightly connected to the asphalt layer. The obtained asphalt layer has good strength, is impermeable, has low resistivity, and has good freeze-thaw resistance.

[0016] In a specific possible implementation scheme, the preparation process of the SBS modified asphalt layer includes: mixing SBS modified asphalt and silane coupling agent modified steel slag to obtain a steel slag asphalt mixture, the mixing time is 180-210s, the mixing temperature is 165-175°C, the steel slag asphalt mixture is poured evenly, and then compacted, and cured for 10-20 days to obtain an asphalt layer, the compaction temperature is 150-160°C, and the compaction times are 50-75 times.

[0017] By adopting the above technical solution, SBS modified asphalt and silane coupling agent modified steel slag are mixed evenly, the asphalt layer after curing has high strength and is tightly connected with the hot-melt particle layer.

[0018] In a specific embodiment, the mass percentage of the silane coupling agent modified steel slag in the SBS modified asphalt layer is 40-70%.

[0019] By adopting the above technical solution, the prepared SBS modified asphalt layer has excellent volume stability, high and low temperature performance, fatigue resistance, dynamic modulus and low resistivity.

[0020] In a specific embodiment, the particle size of graphene is 2-6 μm, and the length of carbon fiber is 10-200 μm.

[0021] By adopting the above scheme, graphene and carbon fiber are evenly and stably distributed in the ultra-high performance concrete (UHPC) structural layer, achieving sufficient overlap, and the obtained ultra-high performance concrete (UHPC) structural layer has good conductivity. At the same time, the sizes of the two are limited, probably because the stress is better conducted with the carbon fiber and dispersed around the spherical graphene, the strain performance of the obtained UHPC structural layer is better, and the cracking risk caused by the inconsistent expansion coefficient of the steel bridge deck and the asphalt system is further reduced. The volume of the steel bridge deck system is more stable and the anti-freeze-thaw damage performance is better.

[0022] In a specific embodiment, the mass percentage of graphene in the UHPC structural layer is 10-15%, and the mass percentage of carbon fiber in the UHPC structural layer is 8-12%.

[0023] For the UHPC structural layer used for snow and ice melting, the requirements for resistivity and strength are relatively high. If the resistivity is small, that is, the conductivity is very good, then the conductive phase material added must be large. Excessive addition of graphene will affect the strength of the conductive concrete and increase the manufacturing cost of the conductive concrete; if the resistivity is too large, it cannot generate heat effectively. As the amount of conductive phase filling increases, the resistivity gradually decreases. After repeated experiments, the applicant adopted the above-mentioned technical solution, the graphene particle size is small and evenly distributed in the UHPC structural layer. By limiting the size and dosage of graphene and carbon fiber, at the critical volume fraction, the resistivity drops sharply, the amount of conductive filler in the obtained UHPC structural layer is small, and the conductive network formed has good conductivity, does not affect the strength of the UHPC structural layer, and has low manufacturing cost.

[0024] In summary, this application has the following beneficial effects: 1. The present application adds silane-modified steel slag, especially epoxysilane-modified steel slag, to asphalt to reduce the water absorption of steel slag while significantly improving the bonding strength between steel slag and asphalt. The SBS modified asphalt layer of the obtained combined system exhibits excellent volume stability, resistance to hot water damage, resistance to freeze-thaw damage, and thermal conductivity.

[0025] 2. The present application uses graphene to modify the UHPC structural layer, adopts graphene and carbon fiber as conductive fillers, and forms a better conductive network by limiting the addition ratio and size of the two. Less conductive filler is added to achieve a lower resistivity. The obtained UHPC layer has a lower resistivity and higher strength, and the obtained combined system can effectively melt ice and snow.

[0026] 3. This application reasonably sets the surface layer of the combined system, and limits the thickness of the SBS modified asphalt layer, hot melt particle layer, epoxy resin layer, UHPC structural layer, steel mesh layer and steel bridge deck layer, the size and mass ratio of each component, so that the prepared combined system has high strength and micro-strain performance, effectively reducing the risk of cracking caused by the inconsistent expansion coefficients of each surface layer. Each surface layer is tightly combined and impermeable, and is more resistant to freeze-thaw damage. The tight combination has fewer defects and thus lower resistivity. The conductive properties of the steel box girder system itself solves the technical problem of pre-embedded conductive electrodes in conductive UHPC. The low resistance properties of steel slag SBS modified asphalt and graphene modified UHPC can effectively utilize the heat brought by the electric heating UHPC to achieve high-efficiency temperature rise, effectively improving the efficiency of road ice and snow melting. The prepared graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated combined system is suitable for ice and snow melting on steel bridge decks.

[0027] 4. By limiting the graphene modification steps, the present application makes the distribution of each component more uniform and the modification effect better. By limiting the asphalt layer preparation steps, the asphalt layer prepared in the present application has better performance and is more closely connected with the hot-melt particle layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their description are used to explain the present invention and do not constitute an improper limitation of the present invention. The embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, wherein: Figure 1 :Steel bridge deck-graphene modified UHPC-steel slag epoxy asphalt composite bridge deck system Figure 2 :Graphene modified UHPC mortar preparation process and resistivity detection diagram Figure 3 :Overlapping of graphite and carbon fiber conductive paths in ultra-high performance concrete (UHPC) structural layers DETAILED DESCRIPTION

[0029] The following is a more specific description of the technical solution of the present invention in combination with several specific implementation examples. The embodiments are only partial embodiments of the present invention, not all of them. The following specific embodiments can be combined with each other, and the same or similar concepts or processes therein may not be repeated in some embodiments.

[0030] Unless otherwise specified, the experimental reagents in the preparation examples, embodiments and comparative examples are conventional commercial brands or obtained through conventional preparation processes.

[0031] The carbon fiber length in Preparation Example 3 and Preparation Examples 5-8 is 50 μm, and the particle size of graphene is 4 μm; the carbon fiber length in Preparation Example 4 is 50 μm, and the particle size of graphene is 10 μm; the melt index of the hot-melt particles in Example 12 is 30, and the melt index of the hot-melt particles in Examples 1-11, Example 13, and Comparative Example 2 is 20.

[0032] Preparation Example Preparation Example 1 Silane coupling agent modified steel slag: Pour 100 kg of steel slag into 1000 kg of toluene and stir evenly, then add 12 kg of silane coupling agent KH-560, stir evenly, filter, react at 100 ° C for 6 hours, and dry to obtain epoxy silane coupling agent modified steel slag.

[0033] Preparation Example 2 Acetic acid treatment of steel slag: Pour 100kg of steel slag into a reaction tank containing 4mol / L acetic acid solution, soak for 1 hour, then introduce industrial tail gas with a CO2 concentration of 20vol%, react at 60℃ for 2 hours, and introduce at a speed of 100m / s. 3 / min, to obtain acetic acid treated steel slag.

[0034] Preparation Example 3: Graphene modified UHPC mortar 1: S1: Put 50kg of carbon fiber into 600kg of sand and stir for 3min to obtain carbon fiber sand; S2: 50 kg of cement, 150 kg of graphene, 6 kg of powdered water reducer, 9 kg of defoamer and 50 kg of water were added into a mixer and stirred for 100 s. Then, the carbon fiber sand and 85 kg of methyl cellulose ether prepared in S1 were poured in and stirred for 100 s. Finally, 100 kg of water was added and stirred for 100 s to obtain graphene-modified UHPC mortar 1.

[0035] Preparation Example 4: Graphene modified UHPC mortar 2: The only difference between this preparation example and preparation example 3 is that the graphene particle size is 10 μm.

[0036] Preparation Example 5: Graphene modified UHPC mortar 3: The only difference between this preparation example and preparation example 3 is that the mass percentage of graphene is 14%.

[0037] Preparation Example 6: Graphene modified UHPC mortar 4: The only difference between this preparation example and preparation example 3 is that the mass percentage of graphene is 13%.

[0038] Preparation Example 7: Graphene modified UHPC mortar 5: The only difference between this preparation example and preparation example 3 is that the mass percentage of graphene is 12%.

[0039] Preparation Example 8: Graphene modified UHPC mortar 6: The only difference between this preparation example and preparation example 3 is that the mass percentage of graphene is 18%.

[0040] Preparation Example 9: Steel slag asphalt mixture 1: 100 kg of SBS modified asphalt and 100 kg of steel slag were mixed to obtain steel slag asphalt mixture, with a mixing time of 190 s and a mixing temperature of 170°C.

[0041] Preparation Example 10: Steel slag asphalt mixture 2: 100 kg of SBS modified asphalt and 100 kg of silane coupling agent modified steel slag prepared in Preparation Example 1 were mixed to obtain a steel slag asphalt mixture. The mixing time was 190 s and the mixing temperature was 170° C.

[0042] Preparation Example 11: Steel slag asphalt mixture 3: 100 kg of SBS modified asphalt and 100 kg of acetic acid treated steel slag prepared in Preparation Example 2 were mixed to obtain a steel slag asphalt mixture. The mixing time was 190 s and the mixing temperature was 170° C.

[0043] Preparation Example 12: Steel slag asphalt mixture 4: 100 kg of SBS modified asphalt and 250 kg of silane coupling agent modified steel slag prepared in Preparation Example 1 were mixed to obtain a steel slag asphalt mixture. The mixing time was 190 s and the mixing temperature was 170° C. Example

[0044] Example 1 S1: Clean the steel bridge deck layer, and weld the steel mesh on the steel bridge deck layer with welding nails. The steel mesh steel bar diameter is 16mm, and the center distance between adjacent steel bars is 100mm to obtain the bottom layer of the steel bridge deck; S2: pouring 60 mm ultra-high performance concrete on the bottom layer of the steel bridge deck prepared in S1 and curing for 10 days to obtain a concrete steel bridge deck; S3: On the concrete steel bridge deck made in S2, the pressure is 0.5kg / m 2Spread solvent-free epoxy resin to obtain a resin concrete steel bridge deck; S4: Spread the resin concrete steel bridge deck prepared in S3 at 0.7 kg / m 2 The hot-melt granular resin concrete steel bridge deck is obtained by paving polypropylene (PP); S5: Pour 40 mm of the steel slag asphalt mixture 1 prepared in Preparation Example 9 on the hot-melt granular resin concrete steel bridge deck prepared in S4, compact it, and cure it for 15 days. The compaction temperature is 155°C and the number of compactions is 60 times, thereby obtaining a graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated combination system.

[0045] Example 2 S1: Clean the steel bridge deck layer, and weld the steel mesh on the steel bridge deck layer with welding nails. The steel mesh steel bar diameter is 20mm, and the center distance between adjacent steel bars is 100mm to obtain the bottom layer of the steel bridge deck; S2: pouring 60 mm ultra-high performance concrete on the bottom layer of the steel bridge deck prepared in S1 and curing for 10 days to obtain a concrete steel bridge deck; S3: On the concrete steel bridge deck made in S2, the pressure is 0.5kg / m 2 Spread solvent-free epoxy resin to obtain a resin concrete steel bridge deck; S4: Spread the resin concrete steel bridge deck prepared in S3 at 0.7 kg / m 2 The hot-melt granular resin concrete steel bridge deck is obtained by paving polypropylene (PP); S5: Pour 40 mm of the steel slag asphalt mixture 1 prepared in Preparation Example 9 on the hot-melt granular resin concrete steel bridge deck prepared in S4, compact it, and cure it for 15 days. The compaction temperature is 155°C and the number of compactions is 60 times, thereby obtaining a graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated combination system.

[0046] Example 3 S1: Clean the steel bridge deck layer, and weld the steel mesh on the steel bridge deck layer with welding nails. The steel mesh steel bar diameter is 16mm, and the center distance between adjacent steel bars is 100mm to obtain the bottom layer of the steel bridge deck; S2: pouring 60 mm of graphene-modified UHPC mortar 1 prepared in Preparation Example 3 on the bottom layer of the steel bridge deck prepared in S1, and curing for 10 days to obtain a concrete steel bridge deck; S3: On the concrete steel bridge deck made in S2, the pressure is 0.5kg / m 2 Spread solvent-free epoxy resin to obtain a resin concrete steel bridge deck; S4: Spread the resin concrete steel bridge deck prepared in S3 at 0.7 kg / m 2 The hot-melt granular resin concrete steel bridge deck is obtained by paving polypropylene (PP); S5: Pour 40 mm of the steel slag asphalt mixture 1 prepared in Preparation Example 9 on the hot-melt granular resin concrete steel bridge deck prepared in S4, compact it, and cure it for 15 days. The compaction temperature is 155°C and the number of compactions is 60 times, thereby obtaining a graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated combination system.

[0047] Example 4 S1: Clean the steel bridge deck layer, and weld the steel mesh on the steel bridge deck layer with welding nails. The steel mesh steel bar diameter is 16mm, and the center distance between adjacent steel bars is 100mm to obtain the bottom layer of the steel bridge deck; S2: pouring 60 mm of graphene-modified UHPC mortar 2 prepared in Preparation Example 4 on the bottom layer of the steel bridge deck prepared in S1, and curing for 10 days to obtain a concrete steel bridge deck; S3: On the concrete steel bridge deck made in S2, the pressure is 0.5kg / m 2 Spread solvent-free epoxy resin to obtain a resin concrete steel bridge deck; S4: Spread the resin concrete steel bridge deck prepared in S3 at 0.7 kg / m 2 The hot-melt granular resin concrete steel bridge deck is obtained by paving polypropylene (PP); S5: Pour 40 mm of the steel slag asphalt mixture 1 prepared in Preparation Example 9 on the hot-melt granular resin concrete steel bridge deck prepared in S4, compact it, and cure it for 15 days. The compaction temperature is 155°C and the number of compactions is 60 times, thereby obtaining a graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated combination system.

[0048] Example 5 S1: Clean the steel bridge deck layer, and weld the steel mesh on the steel bridge deck layer with welding nails. The steel mesh steel bar diameter is 16mm, and the center distance between adjacent steel bars is 100mm to obtain the bottom layer of the steel bridge deck; S2: pouring 60 mm of graphene-modified UHPC mortar 3 prepared in Preparation Example 5 on the bottom layer of the steel bridge deck prepared in S1, and curing for 10 days to obtain a concrete steel bridge deck; S3: On the concrete steel bridge deck made in S2, the pressure is 0.5kg / m 2 Spread solvent-free epoxy resin to obtain a resin concrete steel bridge deck; S4: Spread the resin concrete steel bridge deck prepared in S3 at 0.7 kg / m 2 The hot-melt granular resin concrete steel bridge deck is obtained by paving polypropylene (PP); S5: Pour 40 mm of the steel slag asphalt mixture 1 prepared in Preparation Example 9 on the hot-melt granular resin concrete steel bridge deck prepared in S4, compact it, and cure it for 15 days. The compaction temperature is 155°C and the number of compactions is 60 times, thereby obtaining a graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated combination system.

[0049] Example 6 S1: Clean the steel bridge deck layer, and weld the steel mesh on the steel bridge deck layer with welding nails. The steel mesh steel bar diameter is 16mm, and the center distance between adjacent steel bars is 100mm to obtain the bottom layer of the steel bridge deck; S2: pouring 60 mm of graphene-modified UHPC mortar 4 prepared in Preparation Example 6 on the bottom layer of the steel bridge deck prepared in S1, and curing for 10 days to obtain a concrete steel bridge deck; S3: On the concrete steel bridge deck made in S2, the pressure is 0.5kg / m 2 Spread solvent-free epoxy resin to obtain a resin concrete steel bridge deck; S4: Spread the resin concrete steel bridge deck prepared in S3 at 0.7 kg / m 2 The hot-melt granular resin concrete steel bridge deck is obtained by paving polypropylene (PP); S5: Pour 40 mm of the steel slag asphalt mixture 1 prepared in Preparation Example 9 on the hot-melt granular resin concrete steel bridge deck prepared in S4, compact it, and cure it for 15 days. The compaction temperature is 155°C and the number of compactions is 60 times, thereby obtaining a graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated combination system.

[0050] Example 7 S1: Clean the steel bridge deck layer, and weld the steel mesh on the steel bridge deck layer with welding nails. The steel mesh steel bar diameter is 16mm, and the center distance between adjacent steel bars is 100mm to obtain the bottom layer of the steel bridge deck; S2: pouring 60 mm of graphene-modified UHPC mortar 5 prepared in Preparation Example 7 on the bottom layer of the steel bridge deck prepared in S1, and curing for 10 days to obtain a concrete steel bridge deck; S3: On the concrete steel bridge deck made in S2, the pressure is 0.5kg / m 2 Spread solvent-free epoxy resin to obtain a resin concrete steel bridge deck; S4: Spread the resin concrete steel bridge deck prepared in S3 at 0.7 kg / m 2 The hot-melt granular resin concrete steel bridge deck is obtained by paving polypropylene (PP); S5: Pour 40 mm of the steel slag asphalt mixture 1 prepared in Preparation Example 9 on the hot-melt granular resin concrete steel bridge deck prepared in S4, compact it, and cure it for 15 days. The compaction temperature is 155°C and the number of compactions is 60 times, thereby obtaining a graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated combination system.

[0051] Example 8 S1: Clean the steel bridge deck layer, and weld the steel mesh on the steel bridge deck layer with welding nails. The steel mesh steel bar diameter is 16mm, and the center distance between adjacent steel bars is 100mm to obtain the bottom layer of the steel bridge deck; S2: pouring 60 mm of graphene-modified UHPC mortar 6 prepared in Preparation Example 8 on the bottom layer of the steel bridge deck prepared in S1, and curing for 10 days to obtain a concrete steel bridge deck; S3: On the concrete steel bridge deck made in S2, the pressure is 0.5kg / m 2 Spread solvent-free epoxy resin to obtain a resin concrete steel bridge deck; S4: Spread the resin concrete steel bridge deck prepared in S3 at 0.7 kg / m 2 The hot-melt granular resin concrete steel bridge deck is obtained by paving polypropylene (PP); S5: Pour 40 mm of the steel slag asphalt mixture 1 prepared in Preparation Example 9 on the hot-melt granular resin concrete steel bridge deck prepared in S4, compact it, and cure it for 15 days. The compaction temperature is 155°C and the number of compactions is 60 times, thereby obtaining a graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated combination system.

[0052] Example 9 S1: Clean the steel bridge deck layer, and weld the steel mesh on the steel bridge deck layer with welding nails. The steel mesh steel bar diameter is 16mm, and the center distance between adjacent steel bars is 100mm to obtain the bottom layer of the steel bridge deck; S2: pouring 60 mm of graphene-modified UHPC mortar 1 prepared in Preparation Example 3 on the bottom layer of the steel bridge deck prepared in S1, and curing for 10 days to obtain a concrete steel bridge deck; S3: On the concrete steel bridge deck made in S2, the pressure is 0.5kg / m 2 Spread solvent-free epoxy resin to obtain a resin concrete steel bridge deck; S4: Spread the resin concrete steel bridge deck prepared in S3 at 0.7 kg / m 2 The hot-melt granular resin concrete steel bridge deck is obtained by paving polypropylene (PP); S5: Pour 40 mm of the steel slag asphalt mixture 2 prepared in Preparation Example 10 on the hot-melt granular resin concrete steel bridge deck prepared in S4, compact it, and cure it for 15 days. The compaction temperature is 155° C. and the number of compactions is 60 times, thereby obtaining a graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated combination system.

[0053] Example 10 S1: Clean the steel bridge deck layer, and weld the steel mesh on the steel bridge deck layer with welding nails. The steel mesh steel bar diameter is 16mm, and the center distance between adjacent steel bars is 100mm to obtain the bottom layer of the steel bridge deck; S2: pouring 60 mm of graphene-modified UHPC mortar 1 prepared in Preparation Example 3 on the bottom layer of the steel bridge deck prepared in S1, and curing for 10 days to obtain a concrete steel bridge deck; S3: On the concrete steel bridge deck made in S2, the pressure is 0.5kg / m 2 Spread solvent-free epoxy resin to obtain a resin concrete steel bridge deck; S4: Spread the resin concrete steel bridge deck prepared in S3 at 0.7 kg / m 2 The hot-melt granular resin concrete steel bridge deck is obtained by paving polypropylene (PP); S5: Pour 40 mm of the steel slag asphalt mixture 3 prepared in Preparation Example 11 on the hot-melt granular resin concrete steel bridge deck prepared in S4, compact it, and cure it for 15 days. The compaction temperature is 155°C and the number of compactions is 60 times, thereby obtaining a graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated combination system.

[0054] Embodiment 11 S1: Clean the steel bridge deck layer, and weld the steel mesh on the steel bridge deck layer with welding nails. The steel mesh steel bar diameter is 16mm, and the center distance between adjacent steel bars is 100mm to obtain the bottom layer of the steel bridge deck; S2: pouring 60 mm of graphene-modified UHPC mortar 1 prepared in Preparation Example 3 on the bottom layer of the steel bridge deck prepared in S1, and curing for 10 days to obtain a concrete steel bridge deck; S3: On the concrete steel bridge deck made in S2, the pressure is 0.5kg / m 2 Spread solvent-free epoxy resin to obtain a resin concrete steel bridge deck; S4: Spread the resin concrete steel bridge deck prepared in S3 at 0.7 kg / m 2 The hot-melt granular resin concrete steel bridge deck is obtained by paving polypropylene (PP); S5: Pour 40 mm of the steel slag asphalt mixture 4 prepared in Preparation Example 12 on the hot-melt granular resin concrete steel bridge deck prepared in S4, compact it, and cure it for 15 days. The compaction temperature is 155°C and the number of compactions is 60 times, thereby obtaining a graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated combination system.

[0055] Example 12 The difference between the present application and Example 1 is that the melt index of the polypropylene is 30.

[0056] Example 13 S1: Clean the steel bridge deck layer, and weld the steel mesh on the steel bridge deck layer with welding nails. The steel mesh steel bar diameter is 16mm, and the center distance between adjacent steel bars is 100mm to obtain the bottom layer of the steel bridge deck; S2: pouring 60 mm ultra-high performance concrete on the bottom layer of the steel bridge deck prepared in S1 and curing for 10 days to obtain a concrete steel bridge deck; S3: On the concrete steel bridge deck made in S2, the pressure is 0.5kg / m 2 Spread solvent-free epoxy resin to obtain a resin concrete steel bridge deck; S4: Spread the resin concrete steel bridge deck prepared in S3 at 0.7 kg / m 2 The hot-melt granular resin concrete steel bridge deck is obtained by paving polypropylene (PP); S5: Pour 50 mm of the steel slag asphalt mixture 1 prepared in Preparation Example 9 on the hot-melt granular resin concrete steel bridge deck prepared in S4, compact it, and cure it for 15 days. The compaction temperature is 155°C and the number of compactions is 60 times, thereby obtaining a graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated combination system.

[0057] Comparative Example Comparative Example 1 S1: Clean the steel bridge deck layer, and weld the steel mesh on the steel bridge deck layer with welding nails. The steel mesh steel bar diameter is 16mm, and the center distance between adjacent steel bars is 100mm to obtain the bottom layer of the steel bridge deck; S2: pouring 60 mm ultra-high performance concrete on the bottom layer of the steel bridge deck prepared in S1 and curing for 10 days to obtain a concrete steel bridge deck; S3: On the concrete steel bridge deck made in S2, the pressure is 0.5kg / m 2 Spread solvent-free epoxy resin to obtain a resin concrete steel bridge deck; S4: pour 40mm steel slag asphalt mixture 1 obtained in Preparation Example 9 on the resin concrete steel bridge deck obtained in S3, compact it, and cure it for 15 days. The compaction temperature is 155°C and the number of compactions is 60 times to obtain a graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated combination system.

[0058] Comparative Example 2 S1: Clean the steel bridge deck layer, and weld the steel mesh on the steel bridge deck layer with welding nails. The steel mesh steel bar diameter is 16mm, and the center distance between adjacent steel bars is 100mm to obtain the bottom layer of the steel bridge deck; S2: pouring 60 mm ultra-high performance concrete on the bottom layer of the steel bridge deck prepared in S1 and curing for 10 days to obtain a concrete steel bridge deck; S3: On the concrete steel bridge deck made in S2, the pressure is 0.5kg / m 2 Spreading solvent-free epoxy resin to obtain resin concrete steel bridge deck; S4: On the resin concrete steel bridge deck prepared in S3, the 2 The hot-melt granular resin concrete steel bridge deck is obtained by paving polypropylene (PP); S5: Pour 40 mm asphalt on the hot-melt granular resin concrete steel bridge deck prepared in S4, compact it, and maintain it for 15 days. The compaction temperature is 155 ° C and the number of compactions is 60 times, thereby obtaining a graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated combination system.

[0059] Performance test test 1: The graphene modified UHPC and steel slag epoxy asphalt electric heating integrated combination system samples prepared in each embodiment and comparative example were cut into 100mm*100mm test blocks, and freeze-thaw cycles were performed 50 times, cycle time: 24 hours, freezing temperature: -18°C, thawing temperature: 20°C, and then the average strength change of the test blocks before and after freeze-thaw was measured, expressed as a percentage, and the test results are summarized in Table 1.

[0060] Test 2: The samples of the graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated combination system prepared in each embodiment and comparative example were cut into test blocks with a length and width of 100 mm*100 mm, and two test leads were connected to the two end pins of the test block to test the resistivity. The test results are summarized in Table 1.

[0061] Table 1 Strength ratio / % Resistivity / Ω*mm Example 1 89 2.2 Example 2 90 2.0 Example 3 94 1.0 Example 4 92 1.2 Example 5 94 1.2 Example 6 94 1.3 Example 7 93 1.3 Example 8 85 1.3 Example 9 98 0.9 Example 10 90 1.1 Embodiment 11 89 1.0 Example 12 86 2.4 Example 13 88 2.9 Comparative Example 1 86 2.8 Comparative Example 2 88 3.4 This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated system for steel bridge decks, characterized by: The combined system includes, from top to bottom, a styrene-butadiene-styrene block copolymer (SBS) modified asphalt layer, a hot-melt particle layer, an epoxy resin layer, an ultra-high performance concrete (UHPC) structural layer, a steel mesh layer and a steel bridge deck layer. Steel slag is also mixed in the SBS modified asphalt layer. Welding nails are welded between the steel mesh layer and the steel bridge deck layer.

2. The graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated system for steel bridge decks according to claim 1, characterized in that: The steel slag blended in the SBS modified asphalt layer is steel slag modified by a silane coupling agent.

3. The graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated system for steel bridge decks according to claim 1, characterized in that: The ultra high performance concrete (UHPC) structural layer is modified with graphene, and the modification steps include: S1: Put carbon fiber into sand and stir for 2-4 minutes to obtain carbon fiber sand; S2: Mix cement, graphene, powdered water reducer, defoamer and water evenly, stir for 80-100s, then pour in the carbon fiber sand and methyl cellulose ether prepared in S1 and continue to stir for 80-100s, finally add water and continue to stir for 80-100s to obtain mortar; S3: The mortar prepared in S2 is poured evenly and cured for 3-28 days to obtain a graphene-modified ultra-high performance concrete (UHPC) structural layer.

4. The graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated system for steel bridge decks according to claim 1, characterized in that: The melt index (MI) of the hot-melt particles is 12-25.

5. The graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated system for steel bridge decks according to claim 1, characterized in that: The thickness of the SBS modified asphalt layer is 35-45 mm, and the amount of hot-melt particles in the hot-melt particle layer is 0.5-0.9 kg / m 2 The epoxy resin dosage of the epoxy resin layer is 0.3-0.7kg / m 2 The thickness of the UHPC structure layer is 55-65mm, the diameter of the steel bars of the steel mesh is 12-20mm, and the center distance between adjacent steel bars is ≤100mm.

6. The graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated system for steel bridge decks according to claim 2, characterized in that: The silane coupling agent modified steel slag is epoxy silane coupling agent modified steel slag.

7. The graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated system for steel bridge decks according to claim 2, characterized in that: The preparation process of the SBS modified asphalt layer comprises: mixing SBS modified asphalt and silane coupling agent modified steel slag to obtain a steel slag asphalt mixture, the mixing time is 180-210s, the mixing temperature is 165-175°C, the steel slag asphalt mixture is poured evenly, and then compacted, and cured for 10-20 days to obtain an asphalt layer, the compaction temperature is 150-160°C, and the compaction times are 50-75 times.

8. The graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated system for steel bridge decks according to claim 2, characterized in that: The mass percentage of the silane coupling agent modified steel slag in the SBS modified asphalt layer is 40-70%.

9. The graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated system for steel bridge decks according to claim 3, characterized in that: The particle size of the graphene is 2-6 μm, and the length of the carbon fiber is 10-200 μm.

10. The graphene-modified UHPC and steel slag epoxy asphalt electric heating integrated system for steel bridge decks according to claim 3, characterized in that: The mass percentage of the graphene in the UHPC structural layer is 10-15%, and the mass percentage of the carbon fiber in the UHPC structural layer is 8-12%.