Preparation method of super junction device
By replacing wet etching by dry etching and CMP processes, the photoresist layer and hard mask layer are circulated to remove the hard mask layer and etch barrier layer, solving the damage to the trench gate structure in traditional processes The problem is that the yield and electrical performance of the superjunction device are improved.
Patent Information
- Application Number
- CN202411047974.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
AI Technical Summary
In the traditional preparation process of low-voltage superjunction devices, the wet etching process causes the trench gate structure to be destroyed by the wet cleaning solution, affecting the yield of the device.
Use dry etching process and CMP process to remove the hard mask layer and etch barrier layer to avoid the use of wet etching process. By cyclically etching the photoresist layer and hard mask layer, ensure that the thickness of the hard mask layer is smaller than that of The photoresist layer thickness is used, and the remaining hard mask layer and etch barrier layer are removed after the photoresist layer is removed.
The yield and electrical performance of the superjunction device are improved, and the structural damage problems caused by the wet etching process are avoided.
Smart Images

Figure CN118969720A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor manufacturing technology, and in particular to a method for preparing a super junction device. Background Art
[0002] In the traditional preparation process of low-voltage super junction (LV_SJ) devices, after a trench gate structure is formed in the substrate and an etch barrier layer and a hard mask layer are formed on the substrate surface, and after the hard mask layer is etched to form a high aspect ratio trench, a columnar injection region is formed in the substrate at the bottom of the high aspect ratio trench through multiple high-energy IMP (ion implantation), and then the hard mask layer is removed through a wet etching process.
[0003] According to the simulation results, 3400KeV ion implantation energy requires a 5.6μm film layer to block it, and the thickness of the etch barrier layer on the substrate surface directly affects the subsequent IMP implantation depth, thereby directly affecting the device's breakdown voltage (BV). To ensure that BV reaches the ideal value, before the ion implantation process in the columnar implantation area, the thickness of the etch barrier layer on the substrate surface usually needs to be guaranteed to be about.
[0004] However, after the columnar injection area is formed, when the hard mask layer is removed by a wet etching process, it is easy to encounter a series of problems such as the wet etching process time is too long and the etching barrier layer retained on the substrate surface is not enough to block the wet cleaning solution, which allows the wet cleaning solution to enter the trench gate structure from the scribe line and destroy the gate oxide structure in the trench gate structure, thereby affecting the yield of the super junction device product. Summary of the invention
[0005] The present application provides a method for preparing a super junction device, which can solve the problem that in the traditional preparation process of the super junction device, when removing the hard mask layer, the gate oxide structure in the trench gate structure is damaged by the wet cleaning solution, thereby affecting the yield of the super junction device product.
[0006] The present invention provides a method for preparing a super junction device, comprising:
[0007] Step 1: providing a substrate, wherein a trench gate structure is formed in the substrate, and an etching stop layer and a hard mask layer are formed on the surface of the substrate;
[0008] Step 2: etching the hard mask layer to form a plurality of deep trenches;
[0009] Step 3: using the hard mask layer as a mask, forming a columnar implantation region in the substrate at the bottom of the deep trench by an ion implantation process, wherein the columnar implantation region is located between the trench gate structures;
[0010] Step 4: forming a photoresist layer, wherein the photoresist layer fills the deep trench;
[0011] Step 5: etching a portion of the thickness of the photoresist layer located in the deep trench;
[0012] Step 6: etching a partial thickness of the hard mask layer, wherein the remaining thickness of the hard mask layer is less than the remaining thickness of the photoresist layer; wherein steps 5 to 6 are performed at least once;
[0013] Step 7: removing the remaining thickness of the photoresist layer located in the deep trench;
[0014] Step 8: Grinding and removing the remaining thickness of the hard mask layer and a portion of the thickness of the etching stop layer.
[0015] Optionally, in the method for preparing the super junction device, a dry etching process is used to etch a portion of the thickness of the photoresist layer located in the deep trench.
[0016] Optionally, in the method for preparing the super junction device, a dry etching process is used to etch a partial thickness of the hard mask layer.
[0017] Optionally, in the method for preparing the super junction device, the initial thickness of the hard mask layer is at least 5.6 μm.
[0018] Optionally, in the method for preparing the super junction device, in the process of etching the partial thickness of the photoresist layer located in the deep trench, the thickness of the photoresist layer etched and removed does not exceed 1.5 μm.
[0019] Optionally, in the method for preparing the super junction device, before removing the remaining thickness of the photoresist layer located in the deep trench, the remaining thickness of the hard mask layer is less than or equal to 1.3 μm.
[0020] Optionally, in the method for preparing the super junction device, a CMP process is used to grind away the remaining thickness of the hard mask layer and a portion of the thickness of the etch stop layer.
[0021] Optionally, in the method for preparing the super junction device, the initial thickness of the etching stop layer is
[0022] Optionally, in the method for preparing the super junction device, after grinding away the remaining thickness of the hard mask layer and a portion of the thickness of the etch barrier layer, the remaining thickness of the etch barrier layer on the surface of the substrate is no more than
[0023] Optionally, in the method for preparing the super junction device, the material of the etch stop layer is silicon nitride; and the material of the hard mask layer is TEOS.
[0024] The technical solution of this application has at least the following advantages:
[0025] After forming the columnar injection area, the present application fills the deep groove in the hard mask layer with a photoresist layer, and cyclically performs the steps of etching a partial thickness of the photoresist layer + etching a partial thickness of the hard mask layer at least once, and when the thickness of the hard mask layer is etched to a thickness required to meet the grinding process requirements or less, then remove the remaining thickness of the photoresist layer in the deep groove, and finally grind and remove the remaining thickness of the hard mask layer and a partial thickness of the etching barrier layer. In the preparation method of the super junction device of the present application, the removal process of the hard mask layer avoids the traditional wet etching process, thereby avoiding a series of problems such as the trench gate structure being destroyed by the wet etching solution due to the long wet etching process time and the etching barrier layer retained on the substrate surface not being enough to block the wet cleaning solution, thereby improving the yield of the super junction device and improving the electrical performance of the super junction device. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0027] Figure 1 is a flow chart of a method for preparing a super junction device according to an embodiment of the present invention;
[0028] Figure 2-Figure 10 is a schematic diagram of a semiconductor structure in each process step of preparing a super junction device according to an embodiment of the present invention;
[0029] The reference numerals are described as follows:
[0030] 10-substrate, 20-trench gate structure, 11-gate oxide layer, 12-polysilicon gate, 13-column implantation region, 30-etching stop layer, 40-hard mask layer, 41-deep trench, 50-first photoresist layer, 60-second photoresist layer. DETAILED DESCRIPTION
[0031] The following will be combined with the accompanying drawings to clearly and completely describe the technical solutions in this application. Obviously, the described embodiments are part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0032] In the description of the present application, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present application. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.
[0033] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, it can also be the internal connection of two components, it can be a wireless connection, or it can be a wired connection. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0034] In addition, the technical features involved in the different embodiments of the present application described below can be combined with each other as long as they do not conflict with each other.
[0035] The present invention provides a method for preparing a super junction device. Figure 1 , Figure 1 is a flow chart of a method for preparing a super junction device according to an embodiment of the present invention, and Figure 2-Figure 10 , Figure 2-Figure 10 It is a schematic diagram of the semiconductor structure in each process step of preparing a super junction device according to an embodiment of the present invention.
[0036] The method for preparing the super junction device comprises:
[0037] Step 1: Reference Figure 2 , Figure 2 It is a schematic diagram of a semiconductor structure after a hard mask layer is formed according to an embodiment of the present application. A substrate 10 is provided. A trench gate structure 20 is formed in the substrate 10 . An etching stopper layer 30 and a hard mask layer 40 are formed on the surface of the substrate 10 .
[0038] Preferably, the initial thickness of the hard mask layer 40 is at least 5.6 μm.
[0039] Preferably, the initial thickness of the etching stop layer 30 is
[0040] Specifically, the trench gate structure 20 includes a gate oxide layer 11 and a polysilicon gate 12 , wherein the gate oxide layer 11 covers the sidewalls and bottom wall of the trench corresponding to the trench gate structure, and the polysilicon gate 12 covers the gate oxide layer 11 and fills the corresponding trench.
[0041] In this embodiment, the material of the etching stop layer 30 is silicon nitride; the material of the hard mask layer 40 is TEOS.
[0042] The substrate 10 has an epitaxial layer structure on silicon, and the substrate 10 can be N-type highly doped or P-type highly doped.
[0043] This embodiment takes an N-type channel super junction-trench gate as an example, so the substrate 10 is a highly doped N-type substrate.
[0044] Step 2: Reference Figure 3 and Figure 4 , Figure 3 is a schematic diagram of a semiconductor structure after a patterned photoresist layer 1 is formed in an embodiment of the present application, Figure 4 Schematic diagram of a semiconductor structure after forming a plurality of deep trenches according to an embodiment of the present application. Figure 3 As shown, a photoresist layer 50 is first coated on the hard mask layer 40, and a deep groove pattern is defined on the photoresist layer 50 through photolithography processes such as exposure and development, as shown in FIG. Figure 4 As shown, the hard mask layer 40 is then etched and stops at the surface of the etch stop layer 30 to form a plurality of deep trenches 41 .
[0045] In this embodiment, a dry etching process is used to etch the hard mask layer 40 and the etching stops at the surface of the etch stop layer 30 to form a plurality of deep trenches 41 .
[0046] Preferably, the aspect ratio of the deep trench 41 is at least 10:1.
[0047] Step 3: Reference Figure 5 , Figure 5 It is a schematic diagram of the semiconductor structure after the columnar injection region is formed in an embodiment of the present application. With the hard mask layer 40 as a mask, a columnar injection region 13 is formed in the substrate 10 at the bottom of the deep trench 41 through an ion implantation process. The columnar injection region 13 is located between the trench gate structures 20.
[0048] Preferably, in the process of ion implantation to form the columnar implantation region 13, the ion implantation energy is 3400KeV to 4000KeV; the ion implantation dose is 5E11 / cm 2 ~2E13 / cm 2 The columnar implantation region 13 is used to assist the depletion of the N-type substrate (drift region).
[0049] In this embodiment, a P-type pillar implantation region 13 is formed in the substrate 10 at the bottom of the deep trench 41 by a P-type ion implantation process.
[0050] Step 4: Reference Figure 6 , Figure 6 It is a schematic diagram of a semiconductor structure after forming a second photoresist layer according to an embodiment of the present application, wherein a second photoresist layer 60 is formed, and the second photoresist layer 60 fills the deep trench 41 .
[0051] Step 5: Reference Figure 7 , Figure 7 It is a schematic diagram of the semiconductor structure after etching the partial thickness of the second photoresist layer located in the deep trench according to an embodiment of the present application, wherein the partial thickness of the second photoresist layer 60 located in the deep trench 41 is etched.
[0052] Specifically, a dry etching process is used to etch a portion of the thickness of the second photoresist layer 60 located in the deep trench 41 .
[0053] Step 6: Reference Figure 8 , Figure 8 1 is a schematic diagram of a semiconductor structure after etching a portion of the hard mask layer of the embodiment of the present application. The hard mask layer 40 is etched to a portion of the thickness, and the remaining thickness of the hard mask layer 40 is less than the remaining thickness of the photoresist layer 60.
[0054] Specifically, a dry etching process is used to etch a portion of the hard mask layer 40 .
[0055] Preferably, steps 5 to 6 are performed at least once.
[0056] In this embodiment, steps 5 to 6 are performed once.
[0057] In another embodiment, step 5 to step 6 are executed in a loop twice.
[0058] Preferably, after all cycles of step 5 to step 6 are executed and before step 7 is executed, the total thickness of the photoresist layer 60 etched and removed does not exceed 1.5 μm; and the final remaining thickness of the hard mask layer 40 is less than or equal to 1.3 μm.
[0059] Among them, when the number of times that step 5 to step 6 is executed in a cycle is greater than one, the thickness of the photoresist layer 2 60 etched each time can be the same or can decrease gradually; similarly, the thickness of the hard mask layer 40 etched each time can be the same or can decrease gradually. This application only needs to ensure that after all the times that step 5 to step 6 are executed in a cycle and before step 7 is executed, the total thickness of the photoresist layer 2 60 etched and removed does not exceed 1.5μm; the final remaining thickness of the hard mask layer 40 is less than or equal to 1.3μm.
[0060] Step 7: Reference Fig. 9 , Fig. 9 It is a schematic diagram of the semiconductor structure after the remaining thickness of the second photoresist layer located in the deep trench is removed according to an embodiment of the present application, wherein the remaining thickness of the second photoresist layer 60 located in the deep trench 41 is removed.
[0061] Preferably, a dry etching process is used to etch away the remaining thickness of the second photoresist layer 60 located in the deep trench 41 ; or an ashing process is used to remove the remaining thickness of the second photoresist layer 60 located in the deep trench 41 .
[0062] Step 8: Reference Fig.10 , Fig.10 It is a schematic diagram of the semiconductor structure after grinding away the remaining thickness of the hard mask layer and a partial thickness of the etch stop layer according to an embodiment of the present application, wherein the remaining thickness of the hard mask layer 40 and a partial thickness of the etch stop layer 30 are ground away.
[0063] In this embodiment, the CMP process is used to grind away the remaining thickness of the hard mask layer and a portion of the thickness of the etch stop layer.
[0064] It is worth noting that the removal process of the second photoresist layer 60 and the removal process of the hard mask layer 40 do not require a wet etching process and / or a wet cleaning process.
[0065] Preferably, after grinding away the remaining thickness of the hard mask layer 40 and a portion of the thickness of the etch stop layer 30, the remaining thickness of the etch stop layer 30 on the surface of the substrate 10 does not exceed
[0066] In the present application, after forming the columnar injection area, a photoresist layer 2 is filled in the deep groove in the hard mask layer, and the steps of etching a partial thickness of the photoresist layer + etching a partial thickness of the hard mask layer are cyclically performed at least once, and when the thickness of the hard mask layer is etched to a thickness required to meet the grinding process requirements or less (1.3 μm or less in this embodiment), the remaining thickness of the photoresist layer in the deep groove is then removed, and finally the remaining thickness of the hard mask layer and the partial thickness of the etching barrier layer are removed by grinding. The removal process of the hard mask layer and the removal process of the photoresist layer 2 of the present application avoid the traditional wet etching process, thereby avoiding a series of problems such as the trench gate structure being destroyed by the wet etching solution due to the long wet etching process time and the etching barrier layer retained on the substrate surface not being enough to block the wet cleaning solution, thereby improving the yield of the super junction device and improving the electrical performance of the super junction device.
[0067] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection created by this application.
Claims
1. A method for preparing a super junction device, characterized in that: include: Step 1: providing a substrate, wherein a trench gate structure is formed in the substrate, and an etching stop layer and a hard mask layer are formed on the surface of the substrate; Step 2: etching the hard mask layer to form a plurality of deep trenches; Step 3: using the hard mask layer as a mask, forming a columnar implantation region in the substrate at the bottom of the deep trench by an ion implantation process, wherein the columnar implantation region is located between the trench gate structures; Step 4: forming a photoresist layer, wherein the photoresist layer fills the deep trench; Step 5: etching a portion of the thickness of the photoresist layer located in the deep trench; Step 6: etching a partial thickness of the hard mask layer, wherein the remaining thickness of the hard mask layer is less than the remaining thickness of the photoresist layer; wherein steps 5 to 6 are performed at least once; Step 7: removing the remaining thickness of the photoresist layer located in the deep trench; Step 8: Grinding and removing the remaining thickness of the hard mask layer and a portion of the thickness of the etching stop layer.
2. The method for preparing a super junction device according to claim 1, characterized in that: A dry etching process is used to etch a portion of the photoresist layer located in the deep trench.
3. The method for preparing a super junction device according to claim 1, characterized in that: A dry etching process is used to etch a portion of the hard mask layer.
4. The method for preparing a super junction device according to claim 1, characterized in that: The initial thickness of the hard mask layer is at least 5.6 μm.
5. The method for preparing a super junction device according to claim 4, characterized in that: In the process of etching a portion of the photoresist layer located in the deep trench, the thickness of the photoresist layer removed by etching does not exceed 1.5 μm.
6. The method for preparing a super junction device according to claim 5, characterized in that: Before removing the remaining thickness of the photoresist layer in the deep trench, the remaining thickness of the hard mask layer is less than or equal to 1.3 μm.
7. The method for preparing a super junction device according to claim 1, characterized in that: The CMP process is used to grind and remove the remaining thickness of the hard mask layer and a part of the thickness of the etching stop layer.
8. The method for preparing a super junction device according to claim 1, characterized in that: The initial thickness of the etch stop layer is 9. The method for preparing a super junction device according to claim 8, characterized in that: After grinding away the remaining thickness of the hard mask layer and a portion of the thickness of the etch barrier layer, the remaining thickness of the etch barrier layer on the surface of the substrate is no more than 10. The method for preparing a super junction device according to claim 1, characterized in that: The material of the etching stop layer is silicon nitride; the material of the hard mask layer is TEOS.