Preparation method of semiconductor structure

By nitriding the substrate of the semiconductor structure and oxidizing the in-situ water vapor growth process, the oxidation of the substrate is solved, and the yield and performance of the semiconductor structure are improved.

CN118973254AActive Publication Date: 2024-11-15CHANGXIN MEMORY TECH INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310515691.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-11-15
Estimated Expiration
2043-05-08

AI Technical Summary

Technical Problem

In the process of semiconductor structure, oxidation of the substrate causes substrate loss when forming the gate dielectric layer, reducing the yield of the semiconductor structure.

Method used

By nitriding the substrate exposed in the trench, a barrier layer with nitrogen ions is formed, and the precursor layer is oxidized through the in-situ water vapor growth process to prevent the bonding of oxygen atoms and substrate silicon atoms, avoid oxidation of the substrate and improve deposition precursor The uniformity of the body layer prevents the formation of holes in the dielectric layer.

Benefits of technology

It reduces substrate loss, improves the yield of the semiconductor structure, reduces leakage risk, enhances the breakdown resistance of the dielectric layer, and improves the performance of the semiconductor structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118973254A_ABST
    Figure CN118973254A_ABST
Patent Text Reader

Abstract

The embodiment of the invention provides a preparation method of a semiconductor structure, relates to the technical field of semiconductors, and is used for solving the technical problem that a substrate is lost. The preparation method of the semiconductor structure comprises the steps of providing a substrate, wherein a groove is formed in the substrate; carrying out nitriding treatment on the substrate exposed in the groove; and forming a precursor layer covering the inner wall of the groove, and oxidizing the precursor layer through an in-situ water vapor growth process to form a dielectric layer. The semiconductor structure is used for preventing oxygen atoms from being combined with silicon atoms in the substrate, the substrate is prevented from being oxidized, the loss of the substrate is reduced, and the yield of the semiconductor structure is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The disclosed embodiments relate to the field of semiconductor technology, and in particular, to a method for preparing a semiconductor structure. Background Art

[0002] In the process of manufacturing semiconductor structures, it is usually necessary to form a groove in the substrate by a patterning process, and then form a dielectric layer covering the inner wall of the groove by an oxidation process. For example, a gate groove is formed in the active area of ​​the substrate by a patterning process, and then a gate dielectric layer is formed in the gate groove. However, in the process of forming the gate dielectric layer, a part of the thickness of the substrate will be oxidized, resulting in loss of the substrate and reducing the yield of the semiconductor structure. Summary of the invention

[0003] In view of the above problems, an embodiment of the present disclosure provides a method for preparing a semiconductor structure, which is used to reduce the loss of the substrate and improve the yield of the semiconductor structure.

[0004] The present disclosure provides a method for preparing a semiconductor structure, which comprises the following steps:

[0005] Providing a substrate having a groove therein;

[0006] performing a nitridation process on the substrate exposed in the groove;

[0007] A precursor layer covering the inner wall of the groove is formed, and the precursor layer is oxidized by an in-situ water vapor growth process to form a dielectric layer.

[0008] In some embodiments, a nitrogen-containing gas is introduced into the trench at a preset temperature, and then a plasma process is used to perform a nitridation treatment on the substrate exposed in the trench.

[0009] In some embodiments, the nitrogen ion concentration in the surface of the substrate close to the precursor layer is greater than the nitrogen ion concentration in the interior of the substrate.

[0010] In some embodiments, the step of performing a nitridation treatment on the substrate exposed in the trench further includes:

[0011] A barrier layer is formed, wherein the barrier layer covers the inner wall of the groove.

[0012] In some embodiments, the nitrogen-containing gas includes at least one of ammonia, nitrogen, and nitrous oxide.

[0013] In some embodiments, the flow rate of the nitrogen-containing gas is 0.5 L / min-5 L / min.

[0014] In some embodiments, the pressure of the nitrogen-containing gas is 3 torr-10 torr.

[0015] In some embodiments, the preset temperature is 700°C-800°C.

[0016] In some embodiments, the step of forming a precursor layer covering the inner wall of the trench includes: forming a precursor layer on the inner wall of the trench by a deposition process, and the material of the precursor layer includes amorphous silicon.

[0017] In some embodiments, the step coverage of the precursor layer is less than 40%.

[0018] In the method for preparing the semiconductor structure provided in the embodiment of the present disclosure, the substrate exposed in the groove is nitrided so that nitrogen ions are present in the substrate; when the precursor layer is subsequently oxidized through an in-situ water vapor growth process, the nitrogen ions have a blocking function and can block the oxygen atoms from combining with the silicon atoms in the substrate, thereby avoiding oxidation of the substrate, reducing the loss of the substrate, and thereby improving the yield of the semiconductor structure.

[0019] In addition, nitriding the substrate exposed in the grooves can also improve the uniformity of the deposited precursor layer, reduce or even avoid the formation of pinholes in the precursor layer. When the precursor layer is oxidized in the subsequent in-situ water vapor growth process to form a dielectric layer, it can prevent the formation of holes in the dielectric layer, thereby reducing the risk of leakage and improving the yield of the semiconductor structure.

[0020] In addition to the technical problems solved by the embodiments of the present disclosure, the technical features that constitute the technical solutions, and the beneficial effects brought about by the technical features of the technical solutions described above, other technical problems that can be solved by the method for preparing the semiconductor structure provided by the embodiments of the present disclosure, other technical features included in the technical solutions, and the beneficial effects brought about by these technical features will be further described in detail in the specific implementation methods. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the embodiments of the present disclosure or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0022] Figure 1 A process flow chart of a method for preparing a semiconductor structure provided by an embodiment of the present disclosure;

[0023] Figure 2 A schematic diagram of forming a trench in a method for preparing a semiconductor structure provided by an embodiment of the present disclosure;

[0024] Figure 3Schematic diagram of forming a nitridation treated substrate in the method for preparing a semiconductor structure provided in an embodiment of the present invention Figure 1 ;

[0025] Figure 4 Schematic diagram of forming a nitridation treated substrate in the method for preparing a semiconductor structure provided in an embodiment of the present invention Figure 2 ;

[0026] Figure 5 Schematic diagram of forming a barrier layer in the method for preparing a semiconductor structure provided in the present embodiment Figure 1 ;

[0027] Figure 6 Schematic diagram of forming a barrier layer in the method for preparing a semiconductor structure provided in an embodiment of the present disclosure Figure 2 ;

[0028] Figure 7 Schematic diagram of forming a precursor layer in the method for preparing a semiconductor structure provided in the present embodiment Figure 1 ;

[0029] Figure 8 Schematic diagram of forming a precursor layer in the method for preparing a semiconductor structure provided in an embodiment of the present disclosure Figure 2 ;

[0030] Fig. 9 Schematic diagram of forming a dielectric layer in a method for preparing a semiconductor structure provided in an embodiment of the present invention Figure 1 ;

[0031] Fig.10 Schematic diagram of forming a dielectric layer in a method for preparing a semiconductor structure provided in an embodiment of the present disclosure Figure 2 ;

[0032] Fig.11 A schematic diagram of forming a gate structure in a method for preparing a semiconductor structure provided in an embodiment of the present disclosure.

[0033] Reference numerals:

[0034] 100: substrate; 110: trench; 200: barrier layer; 300: precursor layer; 400: dielectric layer; 500: gate structure; 510: barrier layer; 520: conductive layer. DETAILED DESCRIPTION

[0035] As described in the background art, in the related art, when a dielectric layer is formed on the inner wall of the groove, part of the substrate will be oxidized, causing damage to the substrate. The inventors have found that the reason for this problem is that the process of forming the dielectric layer mainly includes the following steps: first, a precursor layer of a certain thickness is formed on the inner wall of the groove, and then the precursor layer is oxidized by an oxidation process to form a dielectric layer. However, when the precursor layer is introduced, the silicon atoms in the precursor layer will form an epitaxial layer of a certain thickness on the surface of the substrate; or, in the oxidation process, not only the precursor layer is oxidized, but also the substrate is oxidized, which will increase the damage to the substrate, for example, shorten the distance between adjacent active areas, increase the risk of leakage in adjacent active areas, and reduce the yield of the semiconductor structure.

[0036] In response to the above technical problems, an embodiment of the present disclosure provides a method for preparing a semiconductor structure, by nitriding the substrate exposed in the groove so that nitrogen ions are present in the substrate; when the precursor layer is subsequently oxidized through an in-situ water vapor growth process, the nitrogen ions have a blocking function, which can prevent oxygen atoms from combining with silicon atoms in the substrate, avoid oxidation of the substrate, reduce the loss of the substrate, and thereby improve the yield of the semiconductor structure.

[0037] In addition, nitriding the substrate exposed in the grooves can also improve the uniformity of the deposited precursor layer, reduce or even avoid the formation of pinholes in the precursor layer. When the precursor layer is oxidized in the subsequent in-situ water vapor growth process to form a dielectric layer, it can prevent the formation of holes in the dielectric layer, thereby reducing the risk of leakage and improving the yield of the semiconductor structure.

[0038] In order to make the above-mentioned purposes, features and advantages of the embodiments of the present disclosure more obvious and understandable, the technical solutions in the embodiments of the present disclosure will be clearly and completely described below in conjunction with the drawings in the embodiments of the present disclosure. Obviously, the described embodiments are only part of the embodiments of the present disclosure, not all of the embodiments. Based on the embodiments in the present disclosure, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present disclosure.

[0039] The present embodiment does not limit the semiconductor structure. The semiconductor structure will be described below by taking a dynamic random access memory (DRAM) as an example, but the present embodiment is not limited thereto. The semiconductor structure in the present embodiment may also be other structures.

[0040] Please refer to the attached Figure 1 , a method for preparing a semiconductor structure provided by an embodiment of the present disclosure includes the following steps:

[0041] Step S100: providing a substrate having a groove therein.

[0042] Please refer to the attached Figure 2 The substrate 100 is used to support the semiconductor device disposed thereon. The substrate 100 may be a silicon (Si) substrate, a germanium (Ge) substrate, a silicon germanium (GeSi) substrate, a silicon carbide (SiC) substrate, a silicon on insulator (SOI) substrate, or a germanium on insulator (GOI) substrate.

[0043] In the present embodiment, the substrate 100 may include an array area and a peripheral area, wherein the array area is used to set a plurality of storage cells and data lines (e.g., a bit line structure and a word line structure). Each storage cell may include a transistor and a capacitor connected to the transistor, and the capacitor is used to store data. Exemplarily, the transistor includes a gate, a source and a drain, and the source and the drain are respectively located on both sides of the gate. Among them, the gate of the transistor is connected to the word line structure, one of the source and the drain is connected to the bit line structure, and the other of the source and the drain is connected to the capacitor, for example, the source is connected to the bit line structure, and correspondingly, the drain is connected to the capacitor. The voltage signal on the word line structure can control the opening or closing of the transistor, and then read the data information stored in the capacitor through the bit line structure, or write the data information into the capacitor for storage through the bit line structure.

[0044] In addition, a logic circuit is disposed in the peripheral area, and the logic circuit is used to be electrically connected to the data line in the array area to implement storage or reading of data information.

[0045] The substrate 100 has a groove 110 in its interior, and the depth direction of the groove 110 is perpendicular to the substrate 100. In the present embodiment, the groove 110 can be used as an isolation groove, and is used to form a shallow trench isolation structure in the isolation groove, so as to divide the substrate 100 into independent active areas. It should be noted that in the present embodiment, the shallow trench isolation structure can be an "ONO" structure, that is, the shallow trench isolation structure includes a stacked silicon oxide layer, a silicon nitride layer and a silicon oxide layer. In addition, the shallow trench isolation structure can also be a single silicon oxide layer, or a single silicon nitride layer.

[0046] The trench 110 can also be used as a gate trench, wherein the gate trench can be formed in the active region, and then a gate structure or a word line structure is formed in the trench 110. In order to facilitate the description of the method for preparing the semiconductor structure, the following embodiment will be described in detail by taking the trench 110 as a gate trench as an example.

[0047] Exemplarily, a mask layer (not shown in the figure) is formed on the substrate 100, and a portion of the thickness of the substrate 100 is removed through a patterning process to form a groove 110 in the substrate 100. The depth direction of the groove 110 is perpendicular to the substrate 100. It should be noted that the mask layer in this embodiment can be a photoresist layer, or a combination of a photoresist layer and a hard mask layer. Among them, the hard mask layer can be a single film layer, or a laminated structure. For example, the hard mask layer can include a spin on hard mask layer (Spin on Hardmask, SOH for short) and a silicon oxynitride layer that are stacked. When the hard mask layer is a laminated structure, the accuracy of the pattern transfer process can be improved, thereby improving the accuracy of the groove 110.

[0048] After the hard mask layer is formed, an anti-reflection layer (not shown) is formed on the surface of the hard mask layer away from the substrate 100. The material of the anti-reflection layer may include nitride. For example, the material of the anti-reflection layer includes silicon nitride or silicon oxynitride, but is not limited thereto. The anti-reflection layer can alleviate or eliminate the standing wave effect of the photoresist layer, thereby increasing the accuracy of the mask pattern transferred from the mask to the photoresist layer, thereby improving the accuracy of the pattern transfer process.

[0049] In this embodiment, the patterning process may be a self-aligned double patterning (SADP) process or a self-aligned quadruple patterning (SAQP) process.

[0050] Step S200: performing nitridation treatment on the substrate exposed in the trench.

[0051] Please refer to the attached Figure 3 and attached Figure 4 , a nitrogen-containing gas is introduced into the groove 110 at a preset temperature, and then a plasma treatment process is used to perform a nitridation treatment on at least the substrate 100 exposed in the groove 110 .

[0052] It should be noted that the attached Figure 3 The structure shown is a cross-sectional view along the direction perpendicular to the extension of the groove 110; Figure 4 The structure shown is a cross-sectional view along the extending direction of the groove 110 .

[0053] Exemplarily, a nitrogen-containing gas is introduced into the reaction chamber, and the nitrogen-containing gas is plasmatized or dissociated under the action of radio frequency power (power of the plasma source) to form nitrogen-containing plasma or nitrogen ions. The nitrogen-containing plasma or nitrogen ions move toward the exposed substrate 100, and the substrate 100 exposed at least in the groove 110 is nitrided. The nitrogen-containing plasma or nitrogen ions can penetrate into the interior of the substrate 100, or react with the silicon in the substrate 100 to form a barrier layer. In this way, the capture ability of the top surface of the substrate 100 can be increased by using nitrogen-containing plasma or nitrogen ions. For example, nitrogen ions or nitrogen-containing plasma can capture oxygen ions, prevent oxygen ions from penetrating into the substrate 100, avoid oxidation of the substrate 100, and thus avoid damage to the substrate 100.

[0054] In one example, nitrogen-containing plasma or nitrogen ions can penetrate into the substrate 100, so that nitrogen ions are present in the substrate 100. Nitrogen ions can increase the capture capability of the surface of the substrate 100. For example, nitrogen ions can capture oxygen ions, prevent oxygen ions from penetrating into the substrate 100, avoid oxidation of the substrate 100, and thus avoid damage to the substrate 100.

[0055] The nitrogen ion concentration in the substrate 100 may be the same everywhere, or other options may be used. For example, the nitrogen ion concentration on the surface of the substrate 100 exposed in the groove 110 is greater than the nitrogen ion concentration inside the substrate 100. Figure 3 Taking the orientation shown as an example, in the area corresponding to the bottom wall of the groove 110, the nitrogen ion concentration in the substrate 100 gradually decreases from the top surface of the substrate 100 to the bottom surface, that is, from the bottom wall of the groove 110 to the bottom surface of the substrate 100. It can be ensured that the nitrogen ion concentration on the surface of the substrate 100 is large enough, thereby ensuring the surface capture ability of the substrate 100. For example, the nitrogen ions can capture oxygen ions, prevent the oxygen ions from penetrating into the substrate 100, avoid oxidation of the substrate 100, and thus avoid damage to the substrate 100.

[0056] At the same time, in the area corresponding to the sidewall of the groove 110, the nitrogen ion concentration in the substrate 100 gradually decreases from one groove 110 to another groove 110. In other words, whether in the direction perpendicular to the substrate 100 or in the horizontal direction, the nitrogen ion concentration in the substrate 100 gradually decreases. In this way, the nitrogen ion concentration on the surface of the substrate 100 can be ensured to be large enough as much as possible, thereby ensuring the surface capture ability of the substrate 100. For example, nitrogen ions can capture oxygen ions, prevent oxygen ions from penetrating into the substrate 100, avoid oxidation of the substrate 100, and thus avoid damage to the substrate 100.

[0057] In addition, it can also prevent excessive nitrogen ions from penetrating into the substrate 100, thereby improving the conductivity of the active region of the substrate 100 and further improving the performance of the semiconductor structure.

[0058] Please refer to the attached Figure 5 and attached Figure 6 In another example, a barrier layer is formed, and the barrier layer covers the inner wall of the groove.

[0059] Exemplarily, nitrogen ions react with silicon in the substrate 100 to form a barrier layer 200, and the barrier layer 200 covers the inner wall of the trench 110. The material of the barrier layer 200 may include any one of silicon nitride and silicon oxynitride. The material of the barrier layer 200 may also be a mixture of silicon nitride and silicon oxynitride.

[0060] In this embodiment, a barrier layer 200 is formed on the inner wall of the groove 110. The barrier layer 200 covers the inner wall of the groove 110, and the barrier layer 200 is used to shield and protect the exposed substrate 100 to prevent the interface between the barrier layer 200 and the substrate 100 from being oxidized, thereby improving the breakdown voltage of the active area and improving the yield of the semiconductor structure.

[0061] In this embodiment, the thickness of the barrier layer 200 is 1 nm-10 nm, and illustratively, the thickness of the barrier layer 200 is 5 nm. This configuration can not only ensure the barrier capability of the barrier layer 200, but also prevent excessive nitrogen ions from reacting with silicon in the substrate 100, avoid excessive loss of the substrate 100, and improve the yield of the semiconductor structure.

[0062] Step S300: forming a precursor layer covering the inner wall of the trench, and oxidizing the precursor layer through an in-situ water vapor growth process to form a dielectric layer.

[0063] Please refer to the attached Figure 7 and attached Figure 8 Exemplarily, the precursor layer 300 is formed by a deposition process, for example, by a process such as chemical vapor deposition (CVD), physical vapor deposition (PVD), or atomic layer deposition (ALD), to form the precursor layer 300 on the inner wall of the trench 110. The material of the precursor layer 300 includes amorphous silicon.

[0064] It should be noted that when the barrier layer 200 is present on the inner wall of the groove 110 , the precursor layer 300 is conformally covered on the barrier layer 200 , that is, the precursor layer 300 and the barrier layer 200 are stacked, and the precursor layer 300 is disposed on the side of the barrier layer 200 facing away from the substrate 100 .

[0065] The precursor layer 300 has a step coverage of less than 40%, for example, less than 10%. In this embodiment, since the surface of the substrate 100 is nitrided and the precursor layer 300 is deposited, the precursor layer 300 is not easy to crystallize. On the one hand, the thickness of each region of the precursor layer 300 can be made substantially the same, with a higher step coverage, so as to prevent the formation of pinholes in the precursor layer 300; on the other hand, the gap between adjacent crystals is reduced, and in subsequent etching or other processes, the gap between adjacent crystals can be prevented from expanding, and the formation of pinholes in the precursor layer 300 can be reduced or even avoided. In this way, the risk of leakage of the semiconductor structure can be reduced, thereby improving the yield of the semiconductor structure.

[0066] After the precursor layer 300 is formed, please refer to the attached Fig. 9 and attached Fig.10 The precursor layer 300 is oxidized by an in-situ water vapor growth process to form a dielectric layer 400. The dielectric layer 400 is made of silicon oxide, but is not limited thereto.

[0067] Exemplarily, a reaction gas is introduced into the reaction chamber, and the reaction gas generates a large number of gas-phase active free radicals with oxidizing properties. These gas-phase active free radicals react with the precursor layer 300 to form the dielectric layer 400 .

[0068] When the material of the dielectric layer 400 is silicon oxide, the reaction gas may be a mixed gas of oxygen and hydrogen. When the mixed gas of hydrogen and oxygen as the reaction gas is transmitted into the reaction chamber, as the temperature rises, the hydrogen and oxygen react to produce a large number of gas-phase active free radicals with oxidative properties, and these free radicals include active oxygen atoms, atomic oxygen, water molecules, and hydroxyl groups. Subsequently, these free radicals participate in the oxidation process of the silicon material of the precursor layer 300.

[0069] In this embodiment, the temperature in the reaction chamber is first raised to a relatively low temperature, for example, a temperature less than 600° C., so that the generation rate of oxygen free radicals on the surface of the precursor layer 300 can be reduced to a certain extent, thereby reducing the reaction rate of oxygen free radicals with silicon materials, providing sufficient reaction time for oxygen free radicals and silicon materials, and thus ensuring that the entire precursor layer 300 is completely oxidized to form the dielectric layer 400. The dielectric layer 400 has a high thickness uniformity, so that the structure of the dielectric layer 400 is compact, and the dielectric layer 400 has improved anti-breakdown capability, for example, the breakdown field strength is increased to 13MV / cm, which greatly improves the performance of the semiconductor structure.

[0070] Please refer to the attached Figure 8 After the precursor layer 300 is formed, the thickness of the area of ​​the substrate 100 corresponding to the bottom wall of the groove 110 can be recorded as D1. Fig.10 After the precursor layer 300 is oxidized by an in-situ water vapor growth process to form the dielectric layer 400 , the thickness of the area of ​​the substrate 100 corresponding to the bottom wall of the trench 110 may be recorded as D2 .

[0071] After the surface of the substrate 100 exposed in the groove 110 is nitrided, the surface of the substrate 100 has nitrogen ions, which have a blocking function and can block the interface state electrons in the substrate 100 from being captured, preventing oxygen atoms from combining with silicon atoms in the substrate 100, so that D1 and D2 are substantially equal. In this way, oxidation of the substrate 100 can be avoided and the loss of the substrate 100 can be reduced, and the step coverage of the dielectric layer 400 can be improved, and the breakdown voltage of the dielectric layer 400 can be improved, thereby ensuring the stability of the electrical parameters of the semiconductor structure, for example, ensuring the stability of the threshold voltage and reducing the leakage rate to improve TTDB, thereby improving the service life and reliability of the semiconductor structure.

[0072] It should be noted that, in this embodiment, D1 and D2 are substantially equal, which can be understood as D1 and D2 being strictly equal; it can also mean that D1 and D2 are approximately equal, for example, the difference between D1 and D2 is within the process error, for example, the difference between the two is within 5%.

[0073] The dielectric layer 400 is not pure silicon oxide, but may be doped with nitrogen. For example, nitrogen accounts for 20% of all elements in the dielectric layer 400. At this time, nitrogen ions can prevent boron ions and phosphorus ions from diffusing into the channel region during the subsequent heat treatment process, thereby improving the conductivity of the gate structure formed subsequently.

[0074] Nitrogen ions can also increase the dielectric constant of the dielectric layer 400. The dielectric layer 400 with a high dielectric constant can increase the physical thickness of the dielectric layer 400 while maintaining the gate capacitance unchanged, thereby reducing the risk of leakage current in the dielectric layer 400 and further improving the reliability of the semiconductor structure. In this embodiment, by nitriding the substrate 100 exposed in the groove 110, the breakdown strength of the dielectric layer 400 can be increased to 13Mv / cm.

[0075] In a possible implementation, the nitrogen-containing gas includes at least one of ammonia, nitrogen and nitrous oxide. That is, the nitrogen-containing gas may be one of the above gases alone, or a mixed gas of ammonia, nitrogen and nitrous oxide. As for the proportion of each gas in ammonia, nitrogen and nitrous oxide, it can be designed according to actual needs, and this embodiment will not be described in detail here.

[0076] Exemplarily, at a preset temperature of 700°C-800°C, for example, at 750°C, at least one of ammonia, nitrogen and nitrous oxide is introduced into the reaction chamber to ensure that the reaction chamber is at a suitable temperature. Such a setting can ensure that as many nitrogen ions as possible penetrate into the substrate 100, or form the barrier layer 200 as evenly as possible, thereby improving the substrate 100's ability to capture interface state electrons, preventing oxygen atoms from combining with silicon atoms in the substrate 100, and making D1 and D2 substantially equal. In this way, it is possible to avoid oxidation of the substrate 100 and reduce excessive loss of the substrate 100, and it is also possible to improve the step coverage of the dielectric layer 400, improve the breakdown voltage of the dielectric layer 400, and thereby ensure the stability of the electrical parameters of the semiconductor structure.

[0077] In one possible implementation, when the pressure of the reaction chamber or the pressure of the nitrogen-containing gas is 3 torr-10 torr, nitrogen-containing gas is continuously introduced into the reaction chamber at a flow rate of 0.5 L / min-5 L / min to form a precursor layer 300 of a preset thickness on the inner wall of the groove 110 to ensure that the thickness of the subsequently formed dielectric layer 400 can be controlled, thereby allowing the width of the groove to be maintained at a maximum, the device turn-on power also increases due to the increase in the groove width, and the signal resolution is greater, thereby improving the performance of the semiconductor structure.

[0078] It should be noted that in this embodiment, the substrate 100 exposed in the groove 110 can be nitrided for about two hours, so that as many nitrogen ions as possible can penetrate into the substrate 100, or the barrier layer 200 can be formed as uniformly as possible, thereby improving the substrate 100's ability to capture interface state electrons, preventing oxygen atoms from combining with silicon atoms in the substrate 100, and making D1 and D2 substantially equal.

[0079] In a possible implementation manner, after the steps of forming a precursor layer covering the inner wall of the trench and oxidizing the precursor layer by an in-situ water vapor growth process to form a dielectric layer, the method for preparing a semiconductor structure further includes:

[0080] Please refer to the attached Fig.11 , a gate structure 500 is formed in the trench 110 , and a top surface of the gate structure 500 is lower than a top surface of the substrate 100 .

[0081] The regions located on both sides of the trench 110 are source regions and drain regions. The source region and the drain region can be formed by ion doping or ion diffusion processes so that the transistor formed is an NMOS transistor or a PMOS transistor. In one example, the conductivity type of the source region and the conductivity type of the drain region are both P-type. Exemplarily, P-type doping ions can be doped into the source region and the drain region, respectively, for example, boron B or gallium Ga and other group III element ions are doped into the source region and the drain region, respectively, so that the transistor formed is a PMOS transistor. In another example, the conductivity type of the source region and the conductivity type of the drain region are both N-type. Exemplarily, N-type doping ions can be doped into the source region and the drain region, respectively, for example, phosphorus P or arsenic As and other group V element ions are doped into the source region and the drain region, respectively, so that the transistor formed is an NMOS transistor.

[0082] In the present embodiment, the top surface of the gate structure 500 is lower than the top surface of the substrate 100, which can reduce the area of ​​the overlapping region between the gate structure 500 and the source region and the drain region. This can not only generate a smaller gate-induced drain leakage current at the junction of the gate structure and the source region and the drain region, but also increase the turn-on current of the semiconductor structure, thereby improving the sensitivity of the semiconductor structure and improving the performance of the semiconductor structure.

[0083] In a possible implementation, the gate structure 500 includes a barrier layer 510 and a conductive layer 520 that are stacked, and the conductive layer 520 completely fills the area surrounded by the barrier layer 510 .

[0084] For example, an atomic layer deposition process may be used to form a barrier material layer and a conductive material layer on the surface of the dielectric layer 400, and the top surface of the barrier material layer is flush with the top surface of the conductive material layer and is higher than the top surface of the dielectric layer 400. In this embodiment, the barrier material layer and the conductive material layer are formed using an atomic layer deposition process, which can ensure the uniformity of the thickness of the barrier material layer and the conductive material layer.

[0085] Afterwards, a chemical mechanical polishing (CMP) process may be used to planarize the top surfaces of the barrier material layer and the conductive material layer, so that the top surfaces of the barrier material layer and the conductive material layer are flush with the top surface of the dielectric layer 400 .

[0086] Then, an etching process, such as a dry etching process or a wet etching process, is used to remove part of the barrier material layer and the conductive material layer located in the groove 110, and the remaining barrier material layer constitutes a barrier layer 510, and the remaining conductive material layer constitutes a conductive layer 520. The barrier layer 510 and the conductive layer 520 constitute a gate structure 500. The top surface of the gate structure 500 is lower than the upper surface of the substrate 100, so that a groove is formed between the gate structure 500 and the top surface of the substrate 100, so as to facilitate the subsequent formation of a gate protection layer in the groove. Among them, the material of the gate protection layer may include silicon nitride, but is not limited thereto.

[0087] In this embodiment, the material of the barrier layer 510 may include a conductive material such as titanium nitride, which prevents the conductive material in the conductive layer 520 from penetrating into the substrate 100 while also having conductivity, thereby ensuring the performance of the semiconductor structure. The material of the conductive layer 520 may include metal tungsten.

[0088] It should be noted that the gate structure 500 is not limited to the above structure, but may also include a first conductive layer, a barrier layer, and a second conductive layer stacked together, wherein the material of the first conductive layer includes polysilicon, and the material of the second conductive layer includes tungsten.

[0089] Please refer to the attached Fig.11 The present disclosure also provides a semiconductor structure according to an embodiment of the present disclosure. The semiconductor structure is manufactured by the method for manufacturing the semiconductor structure in any of the above embodiments.

[0090] When forming the dielectric layer 400 of the semiconductor structure, the surface of the substrate 100 exposed in the groove 110 by nitridation treatment in advance has nitrogen ions on the surface of the substrate 100, and the nitrogen ions have a blocking function, which can prevent the interface state electrons in the substrate 100 from being captured, and prevent the oxygen atoms from combining with the silicon atoms in the substrate 100, so that D1 and D2 are basically equal. In this way, it is possible to avoid oxidation of the substrate 100 and reduce excessive loss of the substrate 100, and it is also possible to improve the step coverage of the dielectric layer 400 and improve the breakdown voltage of the dielectric layer 400, thereby ensuring the stability of the electrical parameters of the semiconductor structure, for example, ensuring the stability of the threshold voltage and reducing the leakage rate to improve TTDB, thereby increasing the service life of the semiconductor structure.

[0091] The various embodiments or implementation methods in this specification are described in a progressive manner. Each embodiment focuses on the differences from other embodiments, and the same or similar parts between the various embodiments can be referenced to each other.

[0092] In the description of this specification, the description with reference to terms such as "one embodiment", "some embodiments", "illustrative embodiment", "example", "specific example", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present disclosure.

[0093] In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0094] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present disclosure, rather than to limit them. Although the present disclosure has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present disclosure.

Claims

1. A method for preparing a semiconductor structure, It is characterized in that The steps include: Providing a substrate having a groove therein; performing a nitridation process on the substrate exposed in the groove; A precursor layer covering the inner wall of the groove is formed, and the precursor layer is oxidized by an in-situ water vapor growth process to form a dielectric layer.

2. The method for preparing a semiconductor structure according to claim 1, It is characterized in that At a preset temperature, nitrogen-containing gas is introduced into the groove, and then a plasma process is used to perform nitridation treatment on the substrate exposed in the groove.

3. The method for preparing a semiconductor structure according to claim 2, It is characterized in that The nitrogen ion concentration in the surface of the substrate close to the precursor layer is greater than the nitrogen ion concentration in the interior of the substrate.

4. The method for preparing a semiconductor structure according to claim 2, It is characterized in that The step of performing a nitridation treatment on the substrate exposed in the groove further includes: A barrier layer is formed, wherein the barrier layer covers the inner wall of the groove.

5. The method for preparing a semiconductor structure according to claim 2, It is characterized in that The nitrogen-containing gas includes at least one of ammonia, nitrogen and nitrous oxide.

6. The method for preparing a semiconductor structure according to any one of claims 2 to 5, It is characterized in that The flow rate of the nitrogen-containing gas is 0.5 L / min-5 L / min.

7. The method for preparing a semiconductor structure according to any one of claims 2 to 5, It is characterized in that The pressure of the nitrogen-containing gas is 3 torr-10 torr.

8. The method for preparing a semiconductor structure according to any one of claims 2 to 5, It is characterized in that The preset temperature is 700°C-800°C.

9. The method for preparing a semiconductor structure according to any one of claims 1 to 5, It is characterized in that The step of forming a precursor layer covering the inner wall of the groove comprises: A precursor layer is formed on the inner wall of the groove by a deposition process, and the material of the precursor layer includes amorphous silicon.

10. The method for preparing a semiconductor structure according to claim 9, It is characterized in that The step coverage of the precursor layer is less than 40%.

Citation Information

Patent Citations

  • Preparation method for shallow trench isolation structure

    CN104157602A

  • Preparation method of shallow trench isolation structure

    CN104779195A

  • Semiconductor structure and forming method thereof

    CN105448914A

  • Manufacturing method of semiconductor structure and semiconductor structure

    CN115084031A

  • Trench-capacitor dram device and manufacture method thereof

    US20070238244A1