Method for recycling plastic film

By contacting the laminate with an acid aqueous solution or an alkali aqueous solution, the resin cured layer of the epoxy resin composition interacts with the inorganic layer, the problems of insufficient gas barrier properties and limited recovery conditions in the laminate are solved, and high-efficiency plastics are achieved Film recycling.

CN118973782APending Publication Date: 2024-11-15MITSUBISHI GAS CHEM CO INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380031107.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-08
Filing Date
2023-03-27
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, the laminated body containing the layer formed of resin is insufficient in gas barrier properties, and the degree of freedom of recovery conditions of the plastic film is low, especially in the laminated form of two or more plastic films, it is difficult to be effective. Recycled plastic film.

Method used

By contacting the laminate with an acid aqueous solution or an alkali aqueous solution, the resin cured layer with an epoxy resin composition interacts with the inorganic layer, thereby promoting dissolution of the inorganic layer and peeling of the resin layer, thereby achieving efficient recovery of the plastic film.

Benefits of technology

The recovery efficiency and freedom of the plastic film are improved, and the plastic film can be easily recovered from a laminated body with two or more pieces of plastic film, and the method is suitable for aqueous acid solutions and aqueous alkali solutions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005063449090000081
    Figure BDA0005063449090000081
  • Figure BDA0005063449090000082
    Figure BDA0005063449090000082
  • Figure BDA0005063449090000121
    Figure BDA0005063449090000121
Patent Text Reader

Abstract

A method for recovering a plastic film from a laminate wherein the laminate comprises: a plastic film (I); at least one inorganic layer (II) selected from the group consisting of silicon oxides, aluminum, and aluminum oxides; and a cured resin layer (III) which is a cured product of an epoxy resin composition containing an epoxy resin and an epoxy resin curing agent containing an amine-based curing agent, the method having a step of bringing the laminate into contact with an aqueous acid solution or an aqueous alkali solution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for recovering plastic film from a laminate. Background Art

[0002] Inorganic vapor-deposited films formed by vapor-depositing inorganic substances such as aluminum oxide and silicon dioxide on thermoplastic plastic films have high gas barrier properties and are therefore used in gas barrier packaging materials. Gas barrier packaging materials have a printed layer in addition to the inorganic vapor-deposited film. In addition, packaging materials in the form of laminated films formed by laminating an inorganic vapor-deposited film and a plastic film via an adhesive layer are also known.

[0003] However, in recent years, considering the effective use of resources and energy and environmental pollution issues, countries around the world have gradually enacted laws to promote the recycling of plastic materials. In response, methods for recycling plastic films from packaging materials containing plastic films have been studied.

[0004] For example, Patent Document 1 discloses a method for manufacturing a recycling substrate, comprising the step of immersing a stacked body in an alkaline aqueous solution, wherein the stacked body has, in sequence, a plastic substrate; a release layer containing at least one selected from the group consisting of aluminum, aluminum oxide and silicon dioxide; and a printed layer, and the concentration of the alkaline compound and the water temperature of the alkaline aqueous solution are within a specified range. The manufacturing method can efficiently and simply obtain the plastic substrate constituting the stacked body as a recycling substrate from a printed material or a laminated stacked body.

[0005] Patent document 2 discloses a packaging material, which comprises a first substrate, a first release layer for detaching the first substrate to recover the first substrate, a second substrate, and a second release layer for detaching the second substrate to recover the second substrate, wherein the first release layer forming composition contains at least one inorganic substance selected from the group consisting of aluminum, aluminum oxide and silicon dioxide and is contained in a specified amount, and the second release layer forming composition is an adhesive composition containing a specified polyol component and a polyisocyanate component. It is also recorded that the packaging material has excellent adhesion to the substrate necessary for the packaging material, and not only the printed layer on the outside of the packaging body but also the printed layer on the inside can be removed, and the two substrates on both sides constituting the packaging material have excellent releasability and are suitable for plastic recycling.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2020-175620

[0009] Patent Document 2: Japanese Patent Application Publication No. 2021-107159 Summary of the invention

[0010] Problem that the invention aims to solve

[0011] In the technology disclosed in Patent Document 1, examples of the binder resin contained in the release layer include a resin selected from polyurethane resin, acrylic resin, polyester resin and polyvinyl alcohol, and examples of the adhesive layer include an anchor layer, a resin layer formed of a molten polyolefin resin, a urethane adhesive layer, an acrylic adhesive, etc. In addition, the second release layer forming composition disclosed in Patent Document 2 is an adhesive composition containing a polyol component and a polyisocyanate component.

[0012] However, laminates including layers formed of these resins have problems such as insufficient gas barrier properties and low flexibility in recycling conditions for plastic films. It is desired to have a technology that can easily recycle plastic films, especially from laminates having a laminated form of two or more plastic films.

[0013] An object of the present invention is to provide a method for efficiently recovering a plastic film from a laminate containing the plastic film.

[0014] Solutions for solving problems

[0015] The present inventors have found that the above-mentioned problems can be solved by a method comprising the step of bringing a laminate comprising a plastic film and a predetermined layer into contact with an aqueous acid solution or an aqueous alkali solution.

[0016] That is, the present invention relates to a method for recovering a plastic film from a laminate, wherein the laminate comprises:

[0017] Plastic film (I);

[0018] an inorganic layer (II) of at least one selected from the group consisting of silicon oxide, aluminum, and aluminum oxide; and

[0019] Resin cured layer (III);

[0020] The resin cured layer (III) is a cured product of an epoxy resin composition, wherein the epoxy resin composition contains an epoxy resin and an epoxy resin curing agent including an amine curing agent.

[0021] The method comprises the step of bringing the laminate into contact with an acid aqueous solution or an alkali aqueous solution.

[0022] Effects of the Invention

[0023] According to the method of the present invention, the plastic film can be efficiently recovered from a laminate containing the plastic film. In the method of the present invention, the degree of freedom of the recovery conditions of the plastic film is high, and in particular, the plastic film can be easily recovered from a laminate having a laminated form of two or more plastic films. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a photograph of the laminated body after being pulverized by a dry pulverizer in Example 32. DETAILED DESCRIPTION

[0025] [Methods for recycling plastic film]

[0026] The present invention is a method for recovering a plastic film from a laminate (hereinafter also referred to as "the method of the present invention"), wherein the laminate comprises:

[0027] Plastic film (I);

[0028] an inorganic layer (II) of at least one selected from the group consisting of silicon oxide, aluminum, and aluminum oxide; and

[0029] The resin cured layer (III) is a cured product of an epoxy resin composition, wherein the epoxy resin composition contains an epoxy resin and an epoxy resin curing agent including an amine curing agent, and the method comprises the step of contacting the laminate with an acid aqueous solution or an alkali aqueous solution.

[0030] The method of the present invention can efficiently recover the plastic film from the laminate containing the plastic film by having the above-mentioned configuration. The reason for this is not clear, but it is considered as follows.

[0031] The inorganic layer (II) of at least one selected from the group consisting of silicon oxide, aluminum and aluminum oxide (hereinafter referred to as "inorganic layer (II)") will dissolve when in contact with an acid aqueous solution or an alkaline aqueous solution. Therefore, it is easy to recover the plastic film from the laminate having the inorganic layer (II). However, the laminate having a laminated form of two or more plastic films has a problem that the acid or alkaline aqueous solution does not easily penetrate between the layers, making it difficult to recover the plastic film.

[0032] In a laminate having two or more plastic films, the films are usually laminated via a resin cured layer such as an adhesive layer. In addition, when the laminate is a packaging material, it may include a primer layer, an anchor coating layer, a coloring layer formed of a coloring ink, a medium layer formed of an ink containing no colorant, and an outer coating layer for surface protection.

[0033] According to the research conducted by the present inventors, it was found that when recycling a plastic film from a laminate containing multiple layers as described above, not only whether or not the laminate contains an inorganic layer (II) affects the ease of recycling of the plastic film, but also the type of other layers, especially the type of the resin cured layer, affects the ease of recycling of the plastic film. In other words, it was found that even if the laminate contains the same inorganic layer (II) and has the same layer structure, the ease of recycling of the plastic film still varies depending on the type of the resin cured layer.

[0034] The laminated body specified in the present invention has a resin cured layer (III), which is a cured product of an epoxy resin composition, and the epoxy resin composition contains an epoxy resin and an epoxy resin curing agent containing an amine curing agent. The resin cured layer (III) is a cured product of an epoxy resin composition, and is therefore different from a resin layer that can be dissolved in an acid or alkaline aqueous solution, a solvent, etc. However, it is believed that if an epoxy resin curing agent containing an amine curing agent is used in an epoxy resin composition, an acid aqueous solution and an alkaline aqueous solution easily penetrate into the interlayer of the formed resin cured layer (III), promote the dissolution of the inorganic layer (II), and the interlayer peeling of the resin cured layer (III) also becomes easy. Different from the technology disclosed in patent documents 1 and 2, the present invention has the following benefits: not only can the plastic film be recycled when the laminated body is in contact with an alkaline aqueous solution, but also when the laminated body is in contact with an acid aqueous solution, the plastic film can be recycled.

[0035] It is presumed that when the inorganic layer (II) is adjacent to or close to the resin cured layer (III), the presence of the resin cured layer (III) makes it easier for the acid or alkali aqueous solution to penetrate between the layers of the laminate, resulting in easier recycling of the plastic film. Here, "the inorganic layer (II) is close to the resin cured layer (III)" means that the inorganic layer (II) and the resin cured layer (III) are present with one or two layers between them.

[0036] Hereinafter, the method of the present invention will be described.

[0037] <Laminated body>

[0038] The laminate specified in the present invention comprises: a plastic film (I); an inorganic layer (II) of at least one selected from the group consisting of silicon oxide, aluminum and aluminum oxide; and a resin cured layer (III), and the resin cured layer (III) is a cured product of an epoxy resin composition, wherein the epoxy resin composition contains an epoxy resin and an epoxy resin curing agent containing an amine-based curing agent.

[0039] (Plastic film (I))

[0040] The plastic film (I) may be any plastic film commonly used for packaging materials, and examples thereof include: polyolefin films such as low-density polyethylene, high-density polyethylene, linear low-density polyethylene, and polypropylene; polyester films such as polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate; polyamide films such as nylon 6, nylon 6,6, and poly(m-phenylenediamine adipamide) (N-MXD6); polyimide films; biodegradable films such as polylactic acid; polyacrylonitrile films; poly(meth)acrylic acid films; polystyrene films; polycarbonate films; ethylene-vinyl acetate copolymer saponified (EVOH) films, polyvinyl alcohol films, and the like.

[0041] Among them, from the viewpoint of transparency, strength, heat resistance, and resistance to acid or alkali aqueous solutions of the laminate, the plastic film is preferably at least one selected from the group consisting of polyolefin films, polyester films, polyamide films, and polyimide films, more preferably at least one selected from the group consisting of polyolefin films and polyester films, and further preferably at least one selected from the group consisting of polypropylene films and polyethylene terephthalate (PET) films.

[0042] The film may be unstretched or stretched in a uniaxial or biaxial direction.

[0043] The thickness of the plastic film (I) is not particularly limited, but is preferably 5 to 300 μm, more preferably 5 to 100 μm, and even more preferably 5 to 50 μm from the viewpoint of transparency, strength, heat resistance, and resistance to acid or alkali aqueous solutions used in the recovery of the plastic film (I). The above thickness is the thickness per sheet of the plastic film (I).

[0044] (Inorganic layer (II))

[0045] The inorganic layer (II) is a layer composed of at least one selected from the group consisting of silicon oxide, aluminum and aluminum oxide. Since the laminate has the inorganic layer (II), the plastic film (I) can be easily recovered by contacting the laminate with an acid aqueous solution or an alkali aqueous solution.

[0046] Examples of silicon oxides include silicon dioxide (SiO x ); Aluminum oxides can be exemplified by aluminum oxide (Al2O x ).

[0047] From the viewpoint of the ease of recycling of the plastic film (I) based on an acidic aqueous solution, the inorganic layer (II) is preferably a layer consisting of at least one selected from the group consisting of aluminum and aluminum oxide (alumina), and more preferably a layer consisting of aluminum. In addition, from the viewpoint of the ease of recycling of the plastic film (I) based on an alkaline aqueous solution, the inorganic layer (II) is preferably a layer containing silicon dioxide. Examples of the layer containing silicon dioxide include a layer consisting of silicon dioxide and a layer consisting of silicon dioxide-alumina.

[0048] The inorganic layer (II) may be composed of a metal foil, formed by a vapor deposition method, etc., and is preferably an inorganic vapor-deposited layer formed by a vapor deposition method from the viewpoint of being able to impart gas barrier properties to the laminate. That is, the inorganic layer (II) is more preferably at least one selected from the group consisting of a silica vapor-deposited layer, an aluminum vapor-deposited layer, and an aluminum oxide vapor-deposited layer, and from the viewpoint of the ease of recycling of the plastic film (I) based on an acidic aqueous solution, it is further preferably at least one selected from the group consisting of an aluminum vapor-deposited layer and an aluminum oxide vapor-deposited layer, and it is further preferably an aluminum vapor-deposited layer. From the viewpoint of the ease of recycling of the plastic film (I) based on an alkaline aqueous solution, the inorganic layer (II) is preferably a vapor-deposited layer containing silica, and more preferably at least one selected from the group consisting of a silica vapor-deposited layer and a silica-alumina binary vapor-deposited layer.

[0049] The thickness of the inorganic layer (II) is not particularly limited, but is preferably 5 nm or more from the viewpoint of the ease of recycling of the plastic film (I) and the viewpoint of imparting gas barrier properties. In addition, when the inorganic layer (II) is an inorganic vapor-deposited layer, it is preferably 100 nm or less, and more preferably 50 nm or less from the viewpoint of improving the transparency and bending resistance of the laminate and the viewpoint of economic efficiency. The above thickness is the thickness of each layer of the inorganic layer (II).

[0050] The method for forming the inorganic layer (II) is not particularly limited, and examples of the evaporation method include physical vapor deposition methods such as vacuum evaporation, sputtering, and ion plating; or chemical vapor deposition methods such as plasma chemical vapor deposition, thermal chemical vapor deposition, and photochemical vapor deposition, and other known evaporation methods. In addition, the inorganic layer (II) may be formed by laminating a metal foil such as aluminum foil with other layers.

[0051] (Resin Cured Layer (III))

[0052] The cured resin layer (III) is a cured product of an epoxy resin composition containing an epoxy resin and an epoxy resin curing agent including an amine-based curing agent. Components contained in the epoxy resin composition will be described below.

[0053] 〔Epoxy resin〕

[0054] The epoxy resin used in the epoxy resin composition may be any of a saturated or unsaturated aliphatic compound, an alicyclic compound, an aromatic compound, or a heterocyclic compound. In view of imparting gas barrier properties, an epoxy resin containing an aromatic ring or an alicyclic structure in the molecule is preferred.

[0055] Specific examples of the epoxy resin include at least one resin selected from an epoxy resin having a glycidylamino group derived from m-xylylenediamine, an epoxy resin having a glycidylamino group derived from p-xylylenediamine, an epoxy resin having a glycidylamino group derived from 1,3-bis(aminomethyl)cyclohexane, an epoxy resin having a glycidylamino group derived from 1,4-bis(aminomethyl)cyclohexane, an epoxy resin having a glycidylamino group derived from diaminodiphenylmethane, an epoxy resin having a glycidylamino group and / or a glycidyloxy group derived from p-aminophenol, an epoxy resin having a glycidyloxy group derived from bisphenol A, an epoxy resin having a glycidyloxy group derived from bisphenol F, an epoxy resin having a glycidyloxy group derived from phenol novolac, and an epoxy resin having a glycidyloxy group derived from resorcinol. In order to improve various properties such as flexibility, impact resistance, and moisture and heat resistance, two or more of the above epoxy resins may be mixed in an appropriate ratio and used.

[0056] Among the above, from the viewpoint of imparting gas barrier properties, the epoxy resin preferably contains as a main component at least one selected from the group consisting of an epoxy resin having a glycidyl amino group derived from m-xylylenediamine, an epoxy resin having a glycidyl amino group derived from p-xylylenediamine, and an epoxy resin having a glycidyloxy group derived from bisphenol F, and more preferably contains as a main component an epoxy resin having a glycidyl amino group derived from m-xylylenediamine.

[0057] It should be noted that the “main component” referred to herein may contain other components within the scope of the present invention, and is preferably 50 to 100% by mass, more preferably 70 to 100% by mass, and even more preferably 90 to 100% by mass of the whole.

[0058] [Epoxy resin curing agent including amine curing agent]

[0059] The epoxy resin curing agent used in the epoxy resin composition contains an amine curing agent from the viewpoint of easily recovering the plastic film (I) from the laminate and from the viewpoint of imparting gas barrier properties.

[0060] The amine curing agent may be a polyamine or a modified product thereof which has been used as a curing agent for epoxy resins. From the viewpoint of being able to easily recover the plastic film (I) from the laminate, from the viewpoint of improving adhesion, and from the viewpoint of imparting gas barrier properties, the amine curing agent is preferably a modified product of a polyamine, more preferably at least one selected from the group consisting of the following amine curing agents (i) and amine curing agents (ii), and further preferably contains the following amine curing agent (i).

[0061] (i) a reaction product of the following component (A) and component (B):

[0062] (A) at least one selected from the group consisting of m-xylylenediamine and p-xylylenediamine

[0063] (B) at least one selected from the group consisting of unsaturated carboxylic acids represented by the following general formula (1) and their derivatives

[0064]

[0065] (In formula (1), R 1 , R 2 Each independently represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aralkyl group having 7 to 13 carbon atoms.)

[0066] (ii) a reaction product of epichlorohydrin and at least one selected from the group consisting of m-xylylenediamine and p-xylylenediamine

[0067] 《Amine curing agent (i)》

[0068] The amine curing agent (i) is a reaction product of the following components (A) and (B). In this specification, "reaction product of X and Y" refers to the reaction product (adduct) of X and Y, and also includes byproducts other than the reaction product, unreacted raw materials X, Y, etc.

[0069] (A) at least one selected from the group consisting of m-xylylenediamine and p-xylylenediamine

[0070] (B) at least one selected from the group consisting of unsaturated carboxylic acids represented by the following general formula (1) and their derivatives

[0071]

[0072] (In formula (1), R 1 , R 2 Each independently represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aralkyl group having 7 to 13 carbon atoms.)

[0073] The component (A) is used from the viewpoint of being able to easily recover the plastic film (I) from the laminate, improving the adhesion to other layers and improving the gas barrier properties. From the viewpoint of gas barrier properties, meta-xylylenediamine is preferred. The component (A) may be used alone or in combination of two.

[0074] The component (B) is at least one selected from the group consisting of unsaturated carboxylic acids represented by the general formula (1) and derivatives thereof. In order to facilitate the recovery of the plastic film (I) from the laminate, improve the adhesion to other layers and improve the gas barrier properties, R in the general formula (1) is preferably 1It is preferably a hydrogen atom or an alkyl group having 1 to 8 carbon atoms, more preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, further preferably a hydrogen atom or a methyl group, and still more preferably a hydrogen atom.

[0075] In addition, from the same viewpoint as above, R in the above general formula (1) 2 It is preferably a hydrogen atom or an alkyl group having 1 to 8 carbon atoms, more preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, further preferably a hydrogen atom or a methyl group, and still more preferably a hydrogen atom.

[0076] Examples of the derivatives of the unsaturated carboxylic acid represented by the general formula (1) include esters, amides, anhydrides and acid chlorides of the unsaturated carboxylic acid. The esters of the unsaturated carboxylic acid are preferably alkyl esters, and the alkyl group preferably has 1 to 6 carbon atoms, more preferably 1 to 3 carbon atoms, and still more preferably 1 to 2 carbon atoms, from the viewpoint of obtaining good reactivity.

[0077] Examples of the unsaturated carboxylic acid represented by the general formula (1) and its derivatives include unsaturated carboxylic acids such as acrylic acid, methacrylic acid, α-ethylacrylic acid, α-propylacrylic acid, α-isopropylacrylic acid, α-n-butylacrylic acid, α-tert-butylacrylic acid, α-pentylacrylic acid, α-phenylacrylic acid, α-benzylacrylic acid, crotonic acid, 2-pentenoic acid, 2-hexenoic acid, 4-methyl-2-pentenoic acid, 2-heptenoic acid, 4-methyl-2-hexenoic acid, 5-methyl-2-hexenoic acid, 4,4-dimethyl-2-pentenoic acid, 4-phenyl-2-butenoic acid, cinnamic acid, o-methylcinnamic acid, m-methylcinnamic acid, p-methylcinnamic acid, and 2-octenic acid, and their esters, amides, anhydrides, acid chlorides, and the like.

[0078] Among the above, from the viewpoint of easily recovering the plastic film (I) from the laminate, improving the adhesion to other layers and improving the gas barrier properties, the aforementioned (B) component is preferably at least one selected from the group consisting of acrylic acid, methacrylic acid, crotonic acid and their derivatives, more preferably at least one selected from the group consisting of acrylic acid, methacrylic acid, crotonic acid and their alkyl esters, further preferably at least one selected from the group consisting of acrylic acid, methacrylic acid and their alkyl esters, further preferably an alkyl ester of acrylic acid, and still more preferably methyl acrylate.

[0079] (B) The component may be used alone or in combination of two or more.

[0080] The reaction between the component (A) and the component (B) is carried out by mixing the component (A) and the component (B) at 0 to 100° C., more preferably 0 to 70° C., and performing a Michael addition reaction and an amide group formation reaction based on dehydration, dealcoholization or deamination at 100 to 300° C., preferably 130 to 250° C., when an unsaturated carboxylic acid, ester or amide is used as the component (B).

[0081] At this time, when the amide group forms the reaction, in order to terminate the reaction, the reaction unit may be subjected to a decompression treatment in the final stage of the reaction as required. In addition, a non-reactive solvent may be used for dilution as required. Furthermore, a catalyst such as phosphite may be added as a dehydrating agent or a dealcoholizing agent.

[0082] On the other hand, when an anhydride or an acid chloride of an unsaturated carboxylic acid is used as the component (B), the Michael addition reaction and the amide group formation reaction are carried out by mixing at 0 to 150°C, preferably 0 to 100°C. At this time, in order to terminate the amide group formation reaction, the reaction apparatus may be decompressed in the final stage of the reaction as required. In addition, a non-reactive solvent may be used for dilution as required. Furthermore, a tertiary amine such as pyridine, picoline, lutidine, or a trialkylamine may be added.

[0083] Since the amide group site formed by the reaction of the aforementioned component (A) and the aforementioned component (B) has high cohesive force, the resin cured layer (III) formed using an epoxy resin composition containing an epoxy resin curing agent which is a reaction product of the components (A) and (B) has high gas barrier properties and good adhesion.

[0084] The reaction molar ratio of the component (B) to the component (A) [(B) / (A)] is preferably in the range of 0.3 to 1.0. If the reaction molar ratio is 0.3 or more, a sufficient amount of amide groups will be generated in the epoxy resin curing agent, and a high level of gas barrier properties will be exhibited. On the other hand, if the reaction molar ratio is in the range of 1.0 or less, the amount of amino groups required for the reaction with the epoxy group in the epoxy resin is sufficient, and the heat resistance and solubility in organic solvents or water are excellent.

[0085] In particular, in consideration of improvement in gas barrier properties, the reaction molar ratio [(B) / (A)] of the component (B) to the component (A) is more preferably in the range of 0.6 to 1.0.

[0086] The amine curing agent may be a reaction product of the above-mentioned components (A) and (B) and at least one compound selected from the group consisting of the following components (C), (D) and (E).

[0087] (C) Select from R 3 At least one of the group consisting of monocarboxylic acids represented by -COOH and derivatives thereof (R 3 represents a hydrogen atom, an alkyl group having 1 to 7 carbon atoms or an aryl group having 6 to 12 carbon atoms which may have a hydroxyl group)

[0088] (D) Cyclic carbonate

[0089] (E) Monoepoxy compounds having 2 to 20 carbon atoms

[0090] The aforementioned component (C) is R 3 The monocarboxylic acid represented by -COOH and its derivatives are used, if necessary, from the viewpoint of reducing the reactivity between the epoxy resin curing agent and the epoxy resin and improving workability.

[0091] R 3 represents a hydrogen atom, an alkyl group having 1 to 7 carbon atoms or an aryl group having 6 to 12 carbon atoms which may have a hydroxyl group, and R 3 An alkyl group having 1 to 3 carbon atoms or a phenyl group is preferred.

[0092] In addition, as R 3 Derivatives of monocarboxylic acids represented by -COOH include, for example, esters, amides, anhydrides and chlorides of the carboxylic acids. The esters of the carboxylic acids are preferably alkyl esters, and the alkyl group preferably has 1 to 6 carbon atoms, more preferably 1 to 3 carbon atoms, and even more preferably 1 to 2 carbon atoms.

[0093] Examples of the component (C) include monocarboxylic acids such as formic acid, acetic acid, propionic acid, butyric acid, lactic acid, glycolic acid, and benzoic acid, and derivatives thereof.

[0094] The component (C) may be used alone or in combination of two or more.

[0095] From the viewpoint of reducing the reactivity of epoxy resin curing agent and epoxy resin and improving workability, the aforementioned (D) component, i.e., cyclic carbonate, is used as required, and from the viewpoint of reactivity with the aforementioned (A) component, it is preferably a cyclic carbonate below a six-membered ring. For example, it can be listed: ethylene carbonate, propylene carbonate, glyceryl carbonate, carbonate-1,2-butylene ester, vinylene carbonate, 4-vinyl-1,3-dioxolane-2-one, 4-methoxymethyl-1,3-dioxolane-2-one, 1,3-dioxane-2-one, etc. Among them, from the viewpoint of improving gas barrier properties, it is preferably selected from at least one of the group consisting of ethylene carbonate, propylene carbonate and glyceryl carbonate.

[0096] The component (D) may be used alone or in combination of two or more.

[0097] The monoepoxy compound of the component (E) is a monoepoxy compound having 2 to 20 carbon atoms, and is used as required to reduce the reactivity between the epoxy resin curing agent and the epoxy resin and improve workability. From the viewpoint of gas barrier properties, a monoepoxy compound having 2 to 10 carbon atoms is preferred, and a compound represented by the following formula (2) is more preferred.

[0098]

[0099] (In formula (2), R 4 represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, an aryl group, or R 5 -O-CH2-, R 5 represents phenyl or benzyl. )

[0100] Examples of the monoepoxy compound represented by the formula (2) include ethylene oxide, propylene oxide, 1,2-butylene oxide, styrene oxide, phenyl glycidyl ether, and benzyl glycidyl ether. The component (E) may be used alone or in combination of two or more.

[0101] When the component (C), component (D) or component (E) is used in the amine curing agent, any one compound selected from the group consisting of the components (C), (D) and (E) may be used alone or in combination of two or more.

[0102] It should be noted that the amine curing agent may be a reaction product obtained by reacting the components (A) to (E) as well as other components within a range that does not impair the effects of the present invention. Examples of the other components include aromatic dicarboxylic acids or derivatives thereof.

[0103] However, the amount of the "other components" used is preferably 30% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less, of the total amount of the reactive components constituting the amine-based curing agent.

[0104] The reaction product of the aforementioned component (A) and component (B) and at least one compound selected from the group consisting of the aforementioned component (C), component (D) and component (E) can be obtained by combining at least one compound selected from the group consisting of the aforementioned component (C), component (D) and component (E) with the aforementioned component (B) and reacting the combination with the polyamine compound, i.e., the aforementioned component (A). In this reaction, the aforementioned components (B) to (E) can be added in any order and reacted with the aforementioned component (A), or the aforementioned components (B) to (E) can be mixed and reacted with the aforementioned component (A).

[0105] The reaction of the component (A) with the component (C) can be carried out under the same conditions as the reaction of the component (A) with the component (B). When the component (C) is used, the components (B) and (C) may be mixed and then reacted with the component (A), or the components (A) and (B) may be reacted first and then reacted with the component (C).

[0106] On the other hand, when the component (D) and / or the component (E) is used, it is preferred that the component (A) and the component (B) are reacted first and then reacted with the component (D) and / or the component (E).

[0107] The reaction of the component (A) with the component (D) and / or the component (E) is carried out by mixing the component (A) with the component (D) and / or the component (E) at 25 to 200° C. and performing an addition reaction at 30 to 180° C., preferably 40 to 170° C. In addition, a catalyst such as sodium methoxide, sodium ethoxide, potassium tert-butoxide, etc. may be used as necessary.

[0108] In the above reaction, in order to promote the reaction, the component (D) and / or the component (E) may be melted or diluted with a non-reactive solvent before use, as required.

[0109] When the amine curing agent is a reaction product of the components (A) and (B) and at least one compound selected from the group consisting of the components (C), (D) and (E), the reaction molar ratio of the component (B) to the component (A) [(B) / (A)] is preferably in the range of 0.3 to 1.0, and more preferably in the range of 0.6 to 1.0, for the same reasons as above. On the other hand, the reaction molar ratio of the components (C), (D) and (E) to the component (A) {[(C)+(D)+(E)] / (A)} is preferably in the range of 0.05 to 3.1, more preferably in the range of 0.07 to 2.5, and even more preferably in the range of 0.1 to 2.0.

[0110] However, from the viewpoint of improving gas barrier properties, the reaction molar ratio of the components (B) to (E) to the component (A) {[(B)+(C)+(D)+(E)] / (A)} is preferably in the range of 0.35 to 2.5, more preferably in the range of 0.35 to 2.0.

[0111] From the viewpoint of easily recovering the plastic film (I) from the laminate and imparting gas barrier properties, the amine curing agent (i) is more preferably a reaction product obtained by reacting only the component (A) and the component (B).

[0112] (Amine curing agent (ii))

[0113] The amine curing agent (ii) is a reaction product of epichlorohydrin and at least one selected from the group consisting of m-xylylenediamine and p-xylylenediamine.

[0114] The amine curing agent (ii) preferably contains a compound represented by the following formula (3) as a main component. The "main component" herein refers to a component whose content is 50% by mass or more when all the components in the amine curing agent (ii) are taken as 100% by mass.

[0115]

[0116] (In formula (3), A is 1,3-phenylene or 1,4-phenylene. n is a number from 1 to 12.)

[0117] A is more preferably 1,3-phenylene.

[0118] The content of the compound represented by the general formula (3) in the amine curing agent (ii) is preferably 60% by mass or more, more preferably 70% by mass or more, further preferably 75% by mass or more, and further preferably 85% by mass or more. The upper limit is 100% by mass.

[0119] From the viewpoint of obtaining good curing performance as a curing agent, the compound represented by the general formula (3) preferably has a high proportion of compounds in which n=1. In the amine curing agent (ii), the content of the compound in which n=1 represented by the general formula (3) is preferably 15% by mass or more, more preferably 20% by mass or more, and further preferably 25% by mass or more. In addition, the upper limit is 100% by mass.

[0120] The content of the compound represented by the general formula (3) in the amine curing agent (ii) and the composition of the compound represented by the general formula (3) can be determined by GC analysis and gel permeation chromatography (GPC) analysis.

[0121] The amine curing agent (ii) can be obtained by subjecting epichlorohydrin to an addition reaction with at least one selected from the group consisting of m-xylylenediamine and p-xylylenediamine by a conventional method.

[0122] From the viewpoint of easily recovering the plastic film (I) from the laminate and from the viewpoint of imparting gas barrier properties, the total content of the amine curing agent (i) and the amine curing agent (ii) in the amine curing agent is preferably 50% by mass or more, more preferably 70% by mass or more, further preferably 80% by mass or more, further preferably 90% by mass or more, and is 100% by mass or less.

[0123] The epoxy resin curing agent may also contain a curing agent component other than the amine curing agent. From the viewpoint of being able to easily recover the plastic film (I) from the laminate, improving the adhesion to other layers and improving the gas barrier properties, it is preferred that the content of the amine curing agent is high. From the above viewpoints, the content of the amine curing agent in the epoxy resin curing agent is preferably 50% by mass or more, more preferably 70% by mass or more, further preferably 80% by mass or more, further preferably 90% by mass or more, and is 100% by mass or less.

[0124] In the epoxy resin composition, the content ratio of the epoxy resin to the epoxy resin curing agent is preferably in the range of 0.2 to 12.0, more preferably in the range of 0.2 to 10.0, from the viewpoint of easily recovering the plastic film (I) from the laminate, improving the adhesion to other layers and improving the gas barrier properties, and the ratio of the number of active hydrogens in the epoxy resin curing agent to the number of epoxy groups in the epoxy resin (number of active hydrogens in the epoxy resin curing agent / number of epoxy groups in the epoxy resin). From the viewpoint of easily peeling the resin cured layer (III) from the laminate when it comes into contact with an acid or alkaline aqueous solution and more easily recovering the plastic film (I), it is further preferably in the range of 0.2 to 8.0, further preferably 0.2 to 5.0, further preferably 0.5 to 5.0, further preferably 0.8 to 5.0.

[0125] From the viewpoint of improving the adhesion between the obtained resin cured layer (III) and other layers, the epoxy resin composition may further contain a coupling agent. Examples of the coupling agent include silane coupling agents, titanate coupling agents, aluminate coupling agents, etc., and from the viewpoint of improving the adhesion between the obtained resin cured layer (III) and other layers, silane coupling agents are preferred.

[0126] Examples of the silane coupling agent include silane coupling agents having a vinyl group, silane coupling agents having an amino group, silane coupling agents having an epoxy group, silane coupling agents having a (meth)acryloyl group, silane coupling agents having a mercapto group, etc. Among them, from the viewpoint of improving the adhesion between the obtained resin cured layer (III) and other layers, at least one selected from the group consisting of silane coupling agents having an amino group and silane coupling agents having an epoxy group is preferred.

[0127] When a coupling agent is used, the content of the coupling agent in the epoxy resin composition is preferably 0.1 to 10 parts by mass, more preferably 1 to 8 parts by mass, based on 100 parts by mass of the epoxy resin curing agent.

[0128] The epoxy resin composition may contain an organic solvent, and a non-reactive solvent is preferably used as the organic solvent. As specific examples thereof, one or more of the following solvents may be preferably used: protic polar solvents such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methoxyethanol, 2-ethoxyethanol, 2-propoxyethanol, 2-butoxyethanol, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, 1-propoxy-2-propanol, and ethyl acetate, butyl acetate, methyl isobutyl ketone, toluene, and the like.

[0129] Among the above, at least one selected from the group consisting of methanol, ethanol and ethyl acetate is preferred from the viewpoint of improving the drying rate.

[0130] When the epoxy resin composition contains an organic solvent, the solid content concentration of the epoxy resin composition is not particularly limited, but is preferably 10% by mass or more, more preferably 20% by mass or more, and further preferably 30% by mass or more from the viewpoint of coating properties. In addition, from the viewpoint of coating properties and adjusting the obtained resin cured layer (III) to a desired thickness, it is preferably 60% by mass or less, more preferably 50% by mass or less, and further preferably 40% by mass or less.

[0131] The epoxy resin composition may contain additives such as a thermosetting resin, a wetting agent, a tackifier, a defoaming agent, a curing accelerator, a rust-proofing additive, a pigment, and an oxygen scavenger as needed within a range not impairing the effects of the present invention.

[0132] The total content of the additives in the epoxy resin composition is preferably 20.0 parts by mass or less, more preferably 0.001 to 15.0 parts by mass, based on 100 parts by mass of the total amount of the epoxy resin and the epoxy resin curing agent, from the viewpoint of exhibiting higher adhesion.

[0133] However, from the viewpoint of obtaining the effect of the present invention, the total content of the epoxy resin and the epoxy resin curing agent in the solid content of the epoxy resin composition is preferably 60% by mass or more, more preferably 70% by mass or more, further preferably 80% by mass or more, and further preferably 85% by mass or more, and the upper limit is 100% by mass. "The solid content of the epoxy resin composition" refers to the components after removing the water and organic solvent in the epoxy resin composition.

[0134] In the epoxy resin composition, the content of the lubricant is preferably small from the viewpoint that the obtained resin cured layer (III) exhibits higher adhesiveness. Specifically, the content of the lubricant in the epoxy resin composition is preferably less than 10 parts by mass, more preferably less than 5 parts by mass, further preferably less than 2 parts by mass, further preferably less than 1 part by mass, further preferably less than 0.1 parts by mass, further preferably less than 0.01 parts by mass, and further preferably 0 parts by mass, relative to 100 parts by mass of the total amount of the epoxy resin and the epoxy resin curing agent in the epoxy resin composition.

[0135] The lubricant contains, in addition to conventionally known components as lubricants, unsaturated fatty acid amides having 14 to 24 carbon atoms, such as erucamide and oleamide.

[0136] From the viewpoint that the obtained resin cured layer (III) will exhibit higher adhesion, the epoxy resin composition preferably has a small content of fillers such as organic or inorganic powders and organic or inorganic fibers. Specifically, the content of the filler in the epoxy resin composition is preferably less than 10 parts by mass, more preferably less than 5 parts by mass, further preferably less than 2 parts by mass, further preferably less than 1 part by mass, further preferably less than 0.1 parts by mass, further preferably less than 0.01 parts by mass, and further preferably 0 parts by mass, relative to 100 parts by mass of the total amount of the epoxy resin and the epoxy resin curing agent in the epoxy resin composition.

[0137] (Preparation of epoxy resin composition)

[0138] The epoxy resin composition can be prepared by, for example, mixing an epoxy resin, an epoxy resin curing agent including an amine curing agent, and additives and an organic solvent used as needed in predetermined amounts, and then stirring and mixing using a known method and apparatus. It should be noted that the epoxy resin and the epoxy resin curing agent can also be mixed just before use.

[0139] (Formation of Cured Resin Layer (III))

[0140] The resin cured layer (III) is formed using the aforementioned epoxy resin composition. The epoxy resin composition is a thermosetting resin composition containing the aforementioned epoxy resin and the aforementioned epoxy resin curing agent. For example, when making a laminate, the epoxy resin composition is applied to a plastic film (I) or other layers, and after removing the organic solvent as needed, another plastic film or layer is attached, and then cured to form the resin cured layer (III). The curing method of the epoxy resin composition is not particularly limited, and is carried out by a known method at a concentration and temperature sufficient to obtain the epoxy resin composition of its cured product.

[0141] The details of the method for forming the cured resin layer (III) will be described later in the section “Method for producing a laminate”.

[0142] From the viewpoint of improving adhesion and facilitating recovery of the plastic film (I) from the laminate, the thickness of the resin cured layer (III) is preferably 0.05 to 20 μm, more preferably 0.1 to 15 μm, further preferably 0.2 to 10 μm, further preferably 0.5 to 7 μm, further preferably 1 to 5 μm, further preferably 2 to 5 μm. The above thickness is the thickness per layer of the resin cured layer (III).

[0143] (Layer Structure of Laminated Body)

[0144] The laminate used in the present invention may have one or more of the aforementioned plastic film (I), inorganic layer (II) and resin cured layer (III), or may have two or more. When there are two or more plastic films (I), inorganic layers (II) and resin cured layers (III), the type and thickness of the multilayer plastic film (I) may be all the same or different. The same is true for the type and thickness of the inorganic layer (II) and the resin cured layer (III).

[0145] When two or more plastic films (I) are included, it is preferred that the resins constituting all the plastic films (I) are of the same type from the viewpoint of easy recycling of the plastic films (I).

[0146] The stacking order of the plastic film (I), the inorganic layer (II) and the resin cured layer (III) is not particularly limited, and the laminate preferably contains more than two plastic films (I). In addition, from the viewpoint that the plastic film (I) can be easily recovered from the laminate, the inorganic layer (II) and the resin cured layer (III) are preferably stacked between any two plastic films (I).

[0147] The laminate may have a layer other than the plastic film (I), the inorganic layer (II) and the resin cured layer (III). Examples of such layers include a primer layer, an anchor coating layer, an outer coating layer, an ink layer, a thermoplastic resin layer other than the plastic film (I), a cured product of a photocurable or thermosetting resin composition, i.e., a resin cured layer, an adhesive layer other than the resin cured layer (III), and the like, and may include one or more of these.

[0148] Among the above, when a laminate derived from a packaging material is used, for example, the laminate may further include an ink layer. The ink layer may include a coloring layer formed of an ink containing a coloring agent and a medium layer formed of an ink not containing a coloring agent.

[0149] The color layer in the ink layer can be formed using, for example, a printing ink containing a colorant such as a pigment and a binder resin, and the medium layer can be formed using a printing ink (medium) containing no colorant.

[0150] The ink layer may be formed on the entire surface of the laminate or may be formed partially. In addition, the ink layer may be formed by applying characters, logos, patterns, etc.

[0151] The thickness of the ink layer is usually 0.05 to 20 μm, preferably 0.1 to 15 μm, more preferably 0.2 to 5 μm, and further preferably 0.4 to 2 μm. The above thickness is the thickness per one ink layer.

[0152] The ink layer is preferably formed by a known printing method using printing ink. Examples of the printing method include gravure printing, flexographic printing, and screen printing. From the viewpoint of productivity, gravure printing is preferred.

[0153] Examples of the laminate comprising two or more plastic films (I) include a laminate comprising a plastic film (I), an inorganic layer (II), a cured resin layer (III), and a plastic film (I) in this order.

[0154] Preferred layer structures of the laminated body comprising two or more plastic films (I) are as follows: In the following description, when described as I / II / III, it means that the layers are stacked in order from the top: I, II, and III.

[0155] (1): Plastic film (I) / inorganic layer (II) / resin cured layer (III) / plastic film (I)

[0156] (2): Plastic film (I) / inorganic layer (II) / coloring layer / dielectric layer / resin cured layer (III) / plastic film (I)

[0157] (3): Plastic film (I) / coloring layer / dielectric layer / resin cured layer (III) / inorganic layer (II) / plastic film (I)

[0158] (4): Plastic film (I) / adhesive layer / resin cured layer (III) / inorganic layer (II) / plastic film (I)

[0159] (5): Plastic film (I) / resin cured layer (III) / adhesive layer / inorganic layer (II) / plastic film (I)

[0160] (6): Plastic film (I) / inorganic layer (II) / coloring layer / dielectric layer / resin cured layer (III) / adhesive layer / plastic film (I)

[0161] (7): Plastic film (I) / coloring layer / dielectric layer / adhesive layer / resin cured layer (III) / inorganic layer (II) / plastic film (I)

[0162] (8): Plastic film (I) / inorganic layer (II) / resin cured layer (III) / inorganic layer (II) / plastic film (I)

[0163] (9): Plastic film (I) / inorganic layer (II) / coloring layer / dielectric layer / resin cured layer (III) / inorganic layer (II) / plastic film (I)

[0164] (10) Plastic film (I) / inorganic layer (II) / adhesive layer / resin cured layer (III) / inorganic layer (II) / plastic film (I)

[0165] However, the layer structure of the laminate is not limited to the above, and any interlayer of the above layers may also have a primer layer, an anchor coating layer, an outer coating layer, etc. In addition, it is not limited to the structure of (8) to (10), and it may include two or more inorganic layers (II), and it may also include two or more resin cured layers (III).

[0166] From the viewpoint of being able to easily recover the plastic film (I) from the laminate, the laminate preferably has a structure in which the inorganic layer (II) and the resin cured layer (III) are adjacent to each other, or exist with one or two layers between them. More preferably, the inorganic layer (II) and the resin cured layer (III) are adjacent to each other, or exist with only one layer between them. Further preferably, the inorganic layer (II) and the resin cured layer (III) are adjacent to each other.

[0167] The laminate may also be in the form of a film. In addition, as long as it has a laminated structure comprising a plastic film (I), an inorganic layer (II) and a resin cured layer (III), it may also be in the form of a bag, a bottle, or a cover material, a sealing material, a cylindrical plastic label or other films thereof.

[0168] <Method for producing laminate>

[0169] The method for producing the laminate is not particularly limited, and a known method can be used.

[0170] For example, as a method for manufacturing a laminate having the structure of the aforementioned (1): plastic film (I) / inorganic layer (II) / resin cured layer (III) / plastic film (I), the following method can be cited: an inorganic layer (II) is formed on one side of any plastic film (I) by the aforementioned method, and the aforementioned epoxy resin composition is applied to the surface of the inorganic layer (II) side in a manner to obtain a desired thickness, and another plastic film (I) is immediately attached to the coated surface by a nip roller, etc., and then the epoxy resin composition is cured by the aforementioned method to form a resin cured layer (III). Alternatively, a film having an inorganic layer (II) formed on the plastic film (I) in advance can be used, and a resin cured layer (III) can be formed on the surface of the inorganic layer (II).

[0171] As the coating method when applying the epoxy resin composition, for example, rod coating, Meyer rod coating, air knife coating, gravure coating, reverse gravure coating, micro gravure coating, micro reverse gravure coating, die coating, slot die coating, vacuum die coating, dip coating, spin coating, roll coating, spray coating, brush coating, etc. Among them, rod coating, roll coating or spray coating is preferred, and gravure coating, reverse gravure coating, micro gravure coating or micro reverse gravure coating is industrially preferred.

[0172] After the epoxy resin composition is applied, a step of volatilizing the solvent (drying step) is performed as necessary. The conditions in the drying step can be appropriately selected, and for example, the drying step can be performed at a drying temperature of 40 to 180° C. and a drying time of 5 to 180 seconds.

[0173] After the drying step, the epoxy resin composition is cured to form a cured resin layer (III). The curing temperature can be selected, for example, in the range of 10 to 140° C., preferably in the range of 10 to 80° C. In addition, the curing time can be selected, for example, in the range of 1 minute to 7 days, preferably in the range of 2 to 100 hours.

[0174] <Acidic or alkaline aqueous solution>

[0175] The method of the present invention comprises the step of bringing the laminate into contact with an aqueous acid solution or an aqueous alkali solution.

[0176] The acid used in the aqueous acid solution may be either an inorganic acid or an organic acid.

[0177] Examples of the inorganic acid include hydrochloric acid, sulfuric acid, nitric acid, and phosphoric acid.

[0178] As organic acid, carboxylic acid compounds, sulfonic acid compounds, and organic phosphoric acid compounds can be listed. From the viewpoint that the plastic film (I) can be easily recovered from the laminate, at least one selected from the group consisting of carboxylic acid compounds and sulfonic acid compounds is preferred. As carboxylic acid compounds, formic acid, acetic acid, citric acid, malic acid, lactic acid, adipic acid, sebacic acid, stearic acid, maleic acid, succinic acid, tartaric acid, fumaric acid, gluconic acid, etc. can be listed. As sulfonic acid compounds, methanesulfonic acid, ethanesulfonic acid, p-toluenesulfonic acid, etc. can be listed.

[0179] The above acids may be used alone or in combination of two or more.

[0180] Among the above, from the viewpoint of easily recovering the plastic film (I) from the laminate and from the viewpoint of economic efficiency, the acid used in the acid aqueous solution is preferably at least one selected from the group consisting of hydrochloric acid and carboxylic acid compounds, more preferably at least one selected from the group consisting of hydrochloric acid, acetic acid, citric acid and lactic acid, further preferably at least one selected from the group consisting of hydrochloric acid, acetic acid and lactic acid, and still further preferably at least one selected from the group consisting of acetic acid and lactic acid.

[0181] The concentration of the acid in the aqueous acid solution is preferably 0.1 to 4N, more preferably 0.2 to 3N, and even more preferably 0.5 to 2N, from the viewpoint of easily recovering the plastic film (I) from the laminate and suppressing degradation of the plastic film (I).

[0182] From the viewpoint of easily recovering the plastic film (I) from the laminate, the pH of the acid aqueous solution at 25°C is preferably 6.0 or less, more preferably 5.0 or less, further preferably 4.0 or less, and further preferably 3.0 or less. From the viewpoint of easily recovering the plastic film (I) from the laminate and from the viewpoint of suppressing the deterioration of the plastic film (I), it is preferably 0.2 or more, more preferably 0.5 or more, further preferably 1.0 or more, and further preferably 1.8 or more.

[0183] The alkaline compound used in the alkaline aqueous solution may be any of an inorganic alkaline compound and an organic alkaline compound.

[0184] Examples of the inorganic base compound include alkali metal hydroxides such as lithium hydroxide, sodium hydroxide and potassium hydroxide; alkali metal carbonates or hydrogen carbonates such as lithium carbonate, lithium hydrogen carbonate, potassium carbonate, potassium hydrogen carbonate, sodium carbonate and sodium hydrogen carbonate; and ammonia.

[0185] Examples of the organic base compound include amine compounds, tetraalkylammonium hydroxides, etc. Examples of the amine compound include alkanolamines, alkylamines, arylalkylamines, etc., and the carbon number of these is preferably 10 or less, more preferably 8 or less, from the viewpoint of water solubility.

[0186] Examples of the alkanolamine include mono-, di- or tri-methanolamine and mono-, di- or tri-ethanolamine, and examples of the alkylamine include methylamine, dimethylamine, ethylamine, diethylamine, N-methylethylamine, propylamine, butylamine, and examples of the aralkylamine include benzylamine.

[0187] Examples of the tetraalkylammonium hydroxide include tetramethylammonium hydroxide and tetraethylammonium hydroxide.

[0188] The above-mentioned base compounds may be used alone or in combination of two or more.

[0189] Among the above, from the viewpoint of easily recovering the plastic film (I) from the laminate and from the viewpoint of economic efficiency, the alkali compound used in the alkali aqueous solution is preferably an inorganic alkali compound, more preferably an alkali metal hydroxide, and further preferably at least one selected from the group consisting of sodium hydroxide and potassium hydroxide.

[0190] The concentration of the alkali compound in the aqueous alkali solution varies depending on the type of the alkali compound, but is preferably 0.1 to 20% by mass, more preferably 1 to 15% by mass, and even more preferably 2 to 10% by mass, from the viewpoint of easily recovering the plastic film (I) from the laminate and suppressing the degradation of the plastic film (I).

[0191] From the viewpoint of easily recovering the plastic film (I) from the laminate, the pH of the alkaline aqueous solution at 25°C is preferably 8.0 or more, more preferably 9.0 or more, and further preferably 10.0 or more. From the viewpoint of suppressing the degradation of the plastic film (I), it is preferably 15.0 or less.

[0192] From the viewpoint of more easily recovering the plastic film (I) from the laminate, particularly when the inorganic layer (II) is a layer composed of at least one selected from the group consisting of aluminum and aluminum oxide (aluminum oxide), the method of the present invention preferably includes a step of contacting the laminate with an aqueous acid solution, and more preferably includes a step of immersing the laminate in the aqueous acid solution.

[0193] Examples of a method for contacting the laminate with an aqueous acid solution or an aqueous alkali solution include immersion, spraying, and casting. From the viewpoint of easily recovering the plastic film (I) from the laminate, immersion is preferred.

[0194] The temperature of the aqueous solution when the laminate is brought into contact with the acid aqueous solution or the alkali aqueous solution is not particularly limited, but is preferably 5 to 90°C, more preferably 5 to 70°C, further preferably 10 to 60°C, and further preferably 15 to 45°C, from the viewpoint of easily recovering the plastic film (I) from the laminate and suppressing the degradation of the plastic film (I).

[0195] The time for which the laminate is brought into contact with the acidic aqueous solution or the alkaline aqueous solution is not particularly limited, but is preferably 30 minutes to 7 days, more preferably 1 hour to 5 days, from the viewpoint of the recovery efficiency of the plastic film (I).

[0196] From the viewpoint of easily recovering the plastic film (I) from the laminate and from the viewpoint of economic efficiency, the amount of the aqueous acid solution or the aqueous alkali solution used when the laminate is contacted with the aqueous acid solution or the aqueous alkali solution is preferably 2 to 2,000 times the mass of the laminate, more preferably 2 to 500 times, and even more preferably 2 to 100 times.

[0197] The laminated body after contacting with the acid aqueous solution or the alkaline aqueous solution and the plastic film (I) peeled from the laminated body can be washed with water, dried, and recovered.

[0198] It should be noted that in the method of the present invention, in a laminate containing only one plastic film (I), when the film can be separated from one or more other layers (preferably the inorganic layer (II)), it is judged that the recycling of the plastic film is easy; in a laminate containing two or more plastic films (I), when the films are separable from each other, it is judged that the recycling of the plastic film is easy.

[0199] The separated plastic film (I) may have other layers remaining thereon, in which case the method of the present invention may further include a step of removing the other layers. For example, when the ink layer remains on the plastic film (I), the ink layer can be easily removed by a known deinking process.

[0200] Example

[0201] Next, the present invention will be specifically described by way of examples, but the present invention is not limited by these examples in any way.

[0202] Production Example 1 (Preparation of epoxy resin curing agent solution A containing an amine curing agent)

[0203] 1 mol of m-xylylenediamine (MXDA) was added to the reaction vessel. The temperature was raised to 60°C under a nitrogen stream, and 0.93 mol of methyl acrylate was added dropwise over 1 hour. The generated methanol was distilled off while the temperature was raised to 165°C, and the temperature was maintained at 165°C for 2.5 hours to obtain an amine curing agent. Methanol was added dropwise over 1.5 hours, and 3-aminopropyltriethoxysilane ("KBE-903" manufactured by Shin-Etsu Chemical Co., Ltd.) as a silane coupling agent was added to obtain an epoxy resin curing agent solution A with 62.2% by mass of amine curing agent, 2.8% by mass of 3-aminopropyltriethoxysilane, and 35% by mass of methanol.

[0204] Preparation Example 2 (Preparation of epoxy resin curing agent solution B containing amine curing agent)

[0205] 1 mol of meta-xylylenediamine (MXDA) was added to the reaction vessel. The temperature was raised to 60°C under a nitrogen stream, and 0.93 mol of methyl acrylate was added dropwise over 1 hour. The generated methanol was distilled off while the temperature was raised to 165°C and maintained at 165°C for 2.5 hours to obtain an amine curing agent. Industrial ethanol ("ECONOL H" manufactured by IMAZU CHEMICAL Co., Ltd.) was added dropwise over 1.5 hours, and 3-aminopropyltriethoxysilane ("KBE-903" manufactured by Shin-Etsu Chemical Co., Ltd.) as a silane coupling agent was further added to prepare a solution of 62.2% by mass of an amine curing agent, 2.8% by mass of 3-aminopropyltriethoxysilane, and 35% by mass of ethanol.

[0206] 35.2 g of ethanol and 42.6 g of ethyl acetate as diluents and 21.2 g of the above solution were added and stirred, and 1 g of erucamide was added thereto and stirred to obtain an epoxy resin curing agent solution B having a solid content concentration of 14.7% by mass.

[0207] Production Example 3 (Preparation of epoxy resin composition A)

[0208] 1.98 g of methanol and 3.25 g of ethyl acetate as diluent solvents and 3.64 g of epoxy resin curing agent solution A obtained in Production Example 1 were added and stirred. 1.13 g of an epoxy resin having a glycidylamino group derived from meta-xylylenediamine ("TETRAD-X" manufactured by Mitsubishi Gas Chemical Co., Ltd.) (number of active hydrogens in the epoxy resin curing agent / number of epoxy groups in the epoxy resin = 1.2) was added and stirred to prepare an epoxy resin composition A for forming a resin cured layer (III)-1 having a solid content concentration of 35% by mass.

[0209] Production Example 4 (Preparation of epoxy resin composition B)

[0210] 1.56 g of methanol and 3.25 g of ethyl acetate as diluent solvents and 4.83 g of epoxy resin curing agent solution A obtained in Production Example 1 were added and stirred. 0.36 g of an epoxy resin having a glycidylamino group derived from meta-xylylenediamine ("TETRAD-X" manufactured by Mitsubishi Gas Chemical Co., Ltd.) was added as an epoxy resin (the number of active hydrogens in the epoxy resin curing agent / the number of epoxy groups in the epoxy resin = 5.0) and stirred to prepare an epoxy resin composition B for forming a resin cured layer (III)-2 having a solid content concentration of 35% by mass.

[0211] Production Example 5 (Preparation of Epoxy Resin Composition C)

[0212] 2.15 g of methanol and 3.25 g of ethyl acetate as diluent solvents and 3.13 g of epoxy resin curing agent solution A obtained in Production Example 1 were added and stirred. 1.46 g of an epoxy resin having a glycidylamino group derived from meta-xylylenediamine ("TETRAD-X" manufactured by Mitsubishi Gas Chemical Co., Ltd.) (number of active hydrogens in the epoxy resin curing agent / number of epoxy groups in the epoxy resin = 0.8) was added and stirred to prepare an epoxy resin composition C for forming a resin cured layer (III)-3 having a solid content concentration of 35% by mass.

[0213] Production Example 6 (Preparation of epoxy resin composition D)

[0214] 8.83 g of ethanol as a diluent solvent and 1.14 g of the epoxy resin curing agent solution B obtained in Production Example 2 were added and stirred. 0.03 g of an epoxy resin having a glycidylamino group derived from meta-xylylenediamine ("TETRAD-X" manufactured by Mitsubishi Gas Chemical Co., Ltd.) was added as an epoxy resin (the number of active hydrogens in the epoxy resin curing agent / the number of epoxy groups in the epoxy resin = 3.0) and stirred to prepare an epoxy resin composition D for forming a resin cured layer (III)-4 having a solid content concentration of 2% by mass.

[0215] Example 1 (Preparation of laminate and recovery of plastic film)

[0216] (Production of Laminated Body)

[0217] A laminate having the layer structure shown in Table 1 was produced in the following manner.

[0218] On one side of a biaxially stretched polypropylene film (OPP) ("FOR" manufactured by FUTAMURA CHEMICAL CO., LTD., thickness: 25 μm), white ink (diluted 2-fold with a diluent solvent ("L solvent" manufactured by SAKATA INX CORPORATION) by using a rod coater No. 8) was applied, and the film was heated at 80° C. for 10 seconds to dry (thickness after drying: about 0.5 μm) to form a colored layer. On the colored layer, a reverse-side printing gravure ink (diluted 2-fold with a diluent solvent ("K solvent" manufactured by SAKATA INX CORPORATION) by using a rod coater No. 8 was applied, and the film was heated at 80° C. for 10 seconds to dry (thickness after drying: about 0.5 μm) to form a dielectric layer. In the following table, the colored layer and the dielectric layer are collectively referred to as the "ink layer".

[0219] Then, the epoxy resin composition A obtained in Production Example 3 was applied to the dielectric layer using a bar coater No. 8, and dried by heating at 80° C. for 10 seconds (thickness after drying: about 3 μm). The coated surface of the epoxy resin composition was placed opposite to the aluminum-deposited surface of an unstretched polypropylene film (CPP) ("SF-1" manufactured by Nakai Industry Co., Ltd., thickness: 25 μm) in which aluminum was deposited on one side thereof, and the two layers were laminated using a nip roller and heated at 40° C. for 2 days to form a resin cured layer (III)-1, thereby obtaining a laminate having the layer structure shown in Table 1.

[0220] (Recycling and evaluation of plastic films)

[0221] The obtained laminate was cut into strips of 1.5 cm x 5 cm, and one strip of the laminate was immersed in a 1N acetic acid aqueous solution (about 10 g) at 40°C for 16 hours. After the immersion, the laminate was recovered and subjected to the following evaluation.

[0222] <Peeling interface>

[0223] In the laminated body recovered after immersion in 1N acetic acid aqueous solution, whether or not peeling occurred at the interface of any layer was visually observed and the results are shown in Table 1. The "peeling interface" described in Table 1 means that peeling occurred at the interface indicated by " / / ".

[0224] <State of the deposited layer>

[0225] The presence or absence of dissolution of the aluminum vapor-deposited layer in the laminate was visually observed, and the results are shown in Table 1. In the table, the case where at least a portion of the vapor-deposited layer was observed to be dissolved was described as "dissolved".

[0226] <Separation of CPP>

[0227] The separation state of the CPP film from the laminate was evaluated based on the following criteria and the results are shown in Table 1.

[0228] [Evaluation criteria]

[0229] A: The CPP film was peeled off from the laminate, and the surface of the recovered CPP film was analyzed by SEM-EDX (scanning electron microscope-energy dispersive X-ray spectroscopy). The result showed that no aluminum remained on the film surface.

[0230] B: The CPP film is peeled off from the laminate, but aluminum remains on the surface of the recovered CPP film.

[0231] C: The CPP film is not peeled off from the laminate and cannot be recycled

[0232] [SEM-EDX measurement conditions]

[0233] Equipment used: Scanning electron microscope "SU-8020" manufactured by Hitachi High-Tech Corporation

[0234] Determination conditions:

[0235]

[0236] <Separation of OPP+Ink Layer>

[0237] In the laminate recovered after immersion in 1N acetic acid aqueous solution, the separation state of the OPP film + ink layer was evaluated by visual observation according to the following criteria and the results are shown in Table 1.

[0238] [Evaluation criteria]

[0239] A: OPP film + ink layer peeled off from the laminate, and the cured resin layer did not remain on the ink layer

[0240] B: OPP film + ink layer peeled off from the laminate, but the cured resin layer remained on the ink layer

[0241] C: OPP film + ink layer peeled off from the laminate, but the resin cured layer and part of the vapor deposited layer remained on the ink layer

[0242] D: OPP film + ink layer is not peeled off from the laminate and cannot be recycled

[0243] Embodiments 2 to 4

[0244] Evaluation was performed in the same manner as in Example 1 except that the aqueous solution in which the laminate was immersed was changed to that shown in Table 1. The results are shown in Table 1.

[0245] Example 5

[0246] In Example 1, except that the epoxy resin composition B obtained in Preparation Example 4 was used instead of the epoxy resin composition A obtained in Preparation Example 3, a laminate having the layer structure shown in Table 1 was prepared and evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0247] Embodiments 6 to 8

[0248] Evaluation was carried out in the same manner as in Example 5 except that the aqueous solution in which the laminate was immersed was changed to that described in Table 1. The results are shown in Table 1.

[0249] Comparative Example 1

[0250] In Example 2, except that a urethane adhesive ("TM-569 / CAT-RT37" manufactured by Toyo-Morton Co., Ltd.) was used instead of the epoxy resin composition A obtained in Production Example 3, a laminate having the layer structure shown in Table 1 was prepared and evaluated in the same manner as in Example 2. The results are shown in Table 1.

[0251] Comparative Examples 2 to 3

[0252] Evaluation was performed in the same manner as in Comparative Example 1 except that the aqueous solution in which the laminate was immersed in Comparative Example 1 was changed to that described in Table 1. The results are shown in Table 1.

[0253] [Table 1]

[0254]

[0255] As shown in Table 1, by immersing the laminate having an OPP film and a CPP film, an aluminum vapor-deposited layer, and a predetermined resin cured layer (III) in an acid aqueous solution, the CPP film and the OPP film + ink layer can be separated (Examples 1 to 8). In particular, in Examples 1, 2, 4 to 6, and 8 in which the laminate was immersed in a 1N-acetic acid aqueous solution, a 1N-lactic acid aqueous solution, or a 1N-hydrochloric acid solution, no vapor-deposited layer remained on the CPP film, which is beneficial for the recovery of the CPP film. In contrast, in Comparative Examples 1 to 3, the plastic film could not be separated.

[0256] Example 9 (Preparation of laminate and recovery of plastic film)

[0257] (Production of Laminated Body)

[0258] A laminate having the layer structure shown in Table 2 was produced in the following steps.

[0259] On the alumina-deposited surface of alumina-deposited PET ("Barrialox1011HG" manufactured by TORAY ADVANCED FILM CO., LTD., thickness: 12 μm) in which alumina is deposited on one side of a biaxially stretched polyethylene terephthalate film (PET), white ink (a product obtained by diluting "Belle Color R115" manufactured by SAKATA INX CORPORATION by 2 times with a diluent solvent ("L solvent" manufactured by SAKATA INX CORPORATION)) was applied using a rod coater No. 8, and the ink was dried by heating at 80°C for 10 seconds (thickness after drying: about 0.5 μm) to form a colored layer. On the colored layer, a reverse printing gravure ink ("BelleFlora R medium" manufactured by SAKATA INX CORPORATION diluted 2 times with a diluent solvent ("K solvent" manufactured by SAKATA INX CORPORATION)) was applied using a bar coater No. 8 and dried by heating at 80°C for 10 seconds (thickness after drying: about 0.5 μm) to form a medium layer.

[0260] Then, the epoxy resin composition C obtained in Production Example 5 was applied onto the dielectric layer using a bar coater No. 8, and dried by heating at 80° C. for 10 seconds (thickness after drying: about 3 μm). The coated surface of the epoxy resin composition was placed opposite to an unstretched polypropylene film (CPP) (“PYLEN Film-CT P1146” manufactured by Toyobo Co., Ltd., thickness: 50 μm), and laminated with a nip roll, and heated at 40° C. for 2 days to form a resin cured layer (III)-3, thereby obtaining a laminate having the layer structure shown in Table 2.

[0261] (Recycling and evaluation of plastic films)

[0262] The obtained laminate was cut into strips of 1.5 cm x 5 cm, and one strip of the laminate was immersed in a 1N acetic acid aqueous solution (about 10 g) at 40°C for 16 hours. After the immersion, the laminate was recovered and subjected to the following evaluation.

[0263] <State of peeling interface and vapor deposition layer>

[0264] The same method as in Example 1 was used for evaluation.

[0265] <Separation of PET>

[0266] The separation state of the PET film from the laminate was evaluated based on the following criteria and is shown in Table 2. The SEM-EDX measurement conditions were the same as those described above.

[0267] [Evaluation criteria]

[0268] A: The PET film was peeled off from the laminate, and the surface of the recovered PET film was analyzed by SEM-EDX measurement. The results showed that no aluminum oxide remained on the film surface.

[0269] B: The PET film is peeled off from the laminate, but aluminum oxide remains on the surface of the recovered PET film.

[0270] C: The PET film is not peeled off from the laminate and cannot be recycled

[0271] <Separation of CPP+resin cured layer>

[0272] In the laminate recovered after immersion in 1N acetic acid aqueous solution, the separation state of CPP+resin cured layer was evaluated by visual observation according to the following criteria and the results are shown in Table 2.

[0273] [Evaluation criteria]

[0274] A: The CPP film + resin cured layer is peeled off from the laminate, and the ink layer does not remain on the resin cured layer

[0275] B: CPP film + resin cured layer peeled off from the laminate, but the ink layer remained on the resin cured layer

[0276] C: CPP film + cured resin layer is not peeled off from the laminate and cannot be recycled

[0277] Embodiments 10 to 11

[0278] The evaluation was carried out in the same manner as in Example 9 except that the aqueous solution in which the laminate was immersed was changed to that described in Table 2. The results are shown in Table 2.

[0279] Comparative Example 4

[0280] In Example 9, except that a urethane adhesive ("TM-569 / CAT-RT37" manufactured by Toyo-Morton Co., Ltd.) was used instead of the epoxy resin composition C obtained in Production Example 5, a laminate having the layer structure shown in Table 2 was prepared in the same manner as in Example 9 and evaluated. The results are shown in Table 2.

[0281] Comparative Examples 5-6

[0282] The evaluation was carried out in the same manner as in Comparative Example 4 except that the aqueous solution in which the laminate was immersed was changed to that described in Table 2. The results are shown in Table 2.

[0283] [Table 2]

[0284]

[0285] Example 12 (Production of laminate and recovery of plastic film)

[0286] (Production of Laminated Body)

[0287] A laminate having the layer structure shown in Table 3 was produced in the following steps.

[0288] The epoxy resin composition A obtained in Production Example 3 was applied to the silica-deposited surface of a biaxially stretched polyethylene terephthalate film (PET) ("TECHBARRIER L" manufactured by Mitsubishi Chemical Corporation, thickness: 12 μm) in which silica was deposited on one side thereof, using a bar coater No. 8, and heated at 80° C. for 10 seconds to dry (thickness after drying: about 3 μm). The coated surface of the epoxy resin composition was placed opposite to an unstretched polypropylene film (CPP) ("PYLEN Film-CT P1146" manufactured by Toyobo Co., Ltd., thickness: 25 μm), and laminated with a nip roll, and heated at 40° C. for 2 days to form a resin cured layer (III)-1, and a laminate having the layer structure shown in Table 3 was obtained.

[0289] (Recycling and evaluation of plastic films)

[0290] The obtained laminate was cut into strips of 1.5 cm x 5 cm, and one strip of the laminate was immersed in a 1N acetic acid aqueous solution (about 10 g) at 40°C for 16 hours. After the immersion, the laminate was recovered and subjected to the following evaluation.

[0291] <State of peeling interface and vapor deposition layer>

[0292] The same method as in Example 1 was used for evaluation.

[0293] <Separation of PET>

[0294] The separation state of the PET film from the laminate was evaluated based on the following criteria and is shown in Table 3. The SEM-EDX measurement conditions were the same as those described above.

[0295] [Evaluation criteria]

[0296] A: The PET film was peeled off from the laminate, and the surface of the recovered PET film was analyzed by SEM-EDX measurement. The results showed that no silicon dioxide remained on the film surface.

[0297] B: The PET film is peeled off from the laminate, but silica remains on the surface of the recovered PET film

[0298] C: The PET film is not peeled off from the laminate and cannot be recycled

[0299] <Separation of CPP+resin cured layer>

[0300] In the laminate recovered after immersion in 1N acetic acid aqueous solution, the separation state of CPP+resin cured layer was evaluated by visual observation according to the following criteria and the results are shown in Table 3.

[0301] [Evaluation criteria]

[0302] A: CPP film + cured resin layer peeled off from the laminate

[0303] C: CPP film + cured resin layer is not peeled off from the laminate and cannot be recycled

[0304] Embodiments 13-14

[0305] Evaluation was carried out in the same manner as in Example 12 except that the aqueous solution in which the laminate was immersed was changed to that described in Table 3. The results are shown in Table 3.

[0306] Comparative Example 7

[0307] In Example 12, except that a urethane adhesive ("TM-569 / CAT-RT37" manufactured by Toyo-Morton Co., Ltd.) was used instead of the epoxy resin composition A obtained in Production Example 3, a laminate having the layer structure shown in Table 3 was prepared in the same manner as in Example 12 and evaluated. The results are shown in Table 3.

[0308] Comparative Examples 8 to 9

[0309] Evaluation was performed in the same manner as in Comparative Example 7 except that the aqueous solution in which the laminate was immersed in Comparative Example 7 was changed to that described in Table 3. The results are shown in Table 3.

[0310] [Table 3]

[0311]

[0312] Example 15 (Preparation of laminate and recovery of plastic film)

[0313] (Production of Laminated Body)

[0314] A laminate having the layer structure shown in Table 4 was produced in the following steps.

[0315] The epoxy resin composition A obtained in Production Example 3 was applied to one side of a biaxially stretched polypropylene film (OPP) ("FOR" manufactured by FUTAMURA CHEMICAL CO., LTD., thickness: 25 μm) using a bar coater No. 8, and dried by heating at 80°C for 10 seconds (thickness after drying: about 3 μm). The coated surface of the epoxy resin composition was opposed to the aluminum-deposited surface of an unstretched polypropylene film (CPP) ("SF-1" manufactured by Nakai Industry Co., Ltd., thickness: 25 μm) in which aluminum was deposited on one side, and the two were laminated with a nip roll and heated at 40°C for 2 days to form a resin cured layer (III)-1, thereby obtaining a laminate having the layer structure shown in Table 4.

[0316] (Recycling and evaluation of plastic films)

[0317] The obtained laminate was cut into strips of 1.5 cm x 5 cm, and one strip of the laminate was immersed in 1N hydrochloric acid (about 10 g) at 23°C for 96 hours. After the immersion, the laminate was recovered and subjected to the following evaluation.

[0318] <State of peeling interface and vapor deposition layer>

[0319] The same method as in Example 1 was used for evaluation.

[0320] <Separation of CPP>

[0321] The same method as in Example 1 was used for evaluation.

[0322] <Separation of OPP+cured resin layer>

[0323] In the laminate recovered after immersion in 1N hydrochloric acid, the separation state of the OPP film+resin cured layer was evaluated by visual observation according to the following criteria and the results are shown in Table 4.

[0324] [Evaluation criteria]

[0325] A: OPP film + cured resin layer peeled off from the laminate

[0326] C: OPP film + cured resin layer is not peeled off from the laminate and cannot be recycled

[0327] Example 16

[0328] The evaluation was carried out in the same manner as in Example 15 except that the aqueous solution in which the laminate was immersed was changed to a 5%-KOH aqueous solution (pH: 14.7 at 25°C).

[0329] Example 17 (Production of laminate and recovery of plastic film)

[0330] (Production of Laminated Body)

[0331] A laminate having the layer structure shown in Table 4 was produced in the following steps.

[0332] The epoxy resin composition D obtained in Preparation Example 6 was applied to the aluminum-deposited surface of an unstretched polypropylene film (CPP) ("SF-1" manufactured by Nakai Industry Co., Ltd., thickness: 25 μm) in which aluminum was vapor-deposited on one side thereof, using a rod coater No. 3, and heated at 80° C. for 30 seconds to dry it (thickness after drying: about 0.1 μm).

[0333] Then, a urethane adhesive ("TM-569 / CAT-RT37" manufactured by Toyo-Morton Co., Ltd.) was applied to one side of a biaxially stretched polypropylene film (OPP) ("FOR" manufactured by FUTAMURA CHEMICAL CO., LTD., thickness: 25 μm) using a bar coater No. 8, and dried by heating at 80° C. for 10 seconds (thickness after drying: about 3 μm). The coated surface of the epoxy resin composition and the urethane adhesive layer were made to face each other, and they were laminated with a nip roll and heated at 40° C. for 2 days to form a resin cured layer (III)-4, and a laminate having the layer structure shown in Table 4 was obtained.

[0334] (Recycling and evaluation of plastic films)

[0335] The obtained laminate was cut into strips of 1.5 cm x 5 cm, and one strip of the laminate was immersed in 1N hydrochloric acid (about 10 g) at 23°C for 96 hours. After the immersion, the laminate was recovered and evaluated in the same manner as in Example 12. The results are shown in Table 4.

[0336] Embodiment 18

[0337] The evaluation was carried out in the same manner as in Example 17 except that the aqueous solution in which the laminate was immersed was changed to a 5%-KOH aqueous solution (pH: 14.7 at 25°C).

[0338] [Table 4]

[0339]

[0340] As can be seen from Tables 2 to 4, according to the method of the present invention, even when a laminate having a different layer structure is used, the plastic film can be separated using an acid aqueous solution or an alkali aqueous solution.

[0341] Example 19 (Production of laminate and recovery of plastic film)

[0342] (Production of Laminated Body)

[0343] A laminate having the layer structure shown in Table 5 was produced in the following steps.

[0344] The epoxy resin composition A obtained in Production Example 3 was applied to the silica-deposited surface of a polyethylene terephthalate film (PET) having silica deposited on one side thereof ("TECHBARRIER L" manufactured by Mitsubishi Chemical Corporation, thickness: 12 μm) using a bar coater No. 8, and dried by heating at 80° C. for 10 seconds (thickness after drying: about 3 μm). The epoxy resin composition-coated surface was opposed to the deposited surface of a two-component deposited PET sealant film ("VE034" manufactured by Toyobo Co., Ltd., thickness: 30 μm) having a two-component deposited layer of silica-alumina formed on one side thereof, and the two were laminated with a nip roll and heated at 40° C. for 2 days to form a resin cured layer (III)-1, thereby obtaining a laminate having the layer structure shown in Table 5.

[0345] (Recycling and evaluation of plastic films)

[0346] The obtained laminate was cut into strips of 1.5 cm x 5 cm, and one strip of the laminate was immersed in a 5%-KOH aqueous solution (about 10 g) at 40°C for 16 hours. After the immersion, the laminate was recovered and subjected to the following evaluation.

[0347] <State of peeling interface and vapor deposition layer>

[0348] The same method as in Example 1 was used for evaluation.

[0349] <Separation of PET>

[0350] The separation state of the PET film from the laminate was evaluated based on the following criteria and is shown in Table 5. The SEM-EDX measurement conditions were the same as those described above.

[0351] [Evaluation criteria]

[0352] A: The PET film was peeled off from the laminate, and the surface of the recovered PET film was analyzed by SEM-EDX measurement. The results showed that no silicon dioxide remained on the film surface.

[0353] B: The PET film is peeled off from the laminate, but silica remains on the surface of the recovered PET film

[0354] C: The PET film is not peeled off from the laminate and cannot be recycled

[0355] <Separation of PET sealant>

[0356] The separation state of the PET sealant from the laminate was evaluated based on the following criteria and the results are shown in Table 5.

[0357] [Evaluation criteria]

[0358] A: PET sealant was peeled off from the laminate, and the surface of the recovered PET sealant was analyzed by SEM-EDX measurement. The results showed that no 2-element vapor deposition layer remained on the sealant surface.

[0359] B: PET sealant is peeled off from the laminate, but the 2-element vapor-deposited layer remains on the surface of the recycled PET sealant

[0360] C: PET sealant is not peeled off from the laminate and cannot be recycled

[0361] Embodiments 20 to 22

[0362] The evaluation was carried out in the same manner as in Example 19 except that the aqueous solution in which the laminate was immersed was changed to that described in Table 5. The results are shown in Table 5.

[0363] Comparative Example 10

[0364] In Example 19, except that a urethane adhesive ("TM-569 / CAT-RT37" manufactured by Toyo-Morton Co., Ltd.) was used instead of the epoxy resin composition A obtained in Production Example 3, a laminate having the layer structure shown in Table 5 was prepared in the same manner as in Example 19 and evaluated. The results are shown in Table 5.

[0365] Comparative Examples 11 to 13

[0366] The evaluation was carried out in the same manner as in Comparative Example 10 except that the aqueous solution in which the laminate was immersed in Comparative Example 10 was changed to that described in Table 5. The results are shown in Table 5.

[0367] [Table 5]

[0368]

[0369] Example 23 (Production of laminate and recovery of plastic film)

[0370] (Production of Laminated Body)

[0371] In Example 19, a laminate having the layer structure shown in Table 6 was obtained in the same manner as in Example 19 except that a PET sealant film ("HS-PET (C)" manufactured by NISSEI CHEMICAL CO., LTD.) was used instead of the two-dimensional vapor-deposited PET sealant film.

[0372] (Recycling and evaluation of plastic films)

[0373] The obtained laminate was cut into strips of 1.5 cm x 5 cm, and one strip of the laminate was immersed in a 5%-KOH aqueous solution (about 10 g) at 40°C for 96 hours. After the immersion, the laminate was recovered and subjected to the following evaluation.

[0374] <State of peeling interface and vapor deposition layer>

[0375] The same method as in Example 1 was used for evaluation.

[0376] <Separation of PET>

[0377] The separation state of the PET film from the laminate was evaluated based on the following criteria and is shown in Table 6. The SEM-EDX measurement conditions were the same as those described above.

[0378] [Evaluation criteria]

[0379] A: The PET film was peeled off from the laminate, and the surface of the recovered PET film was analyzed by SEM-EDX measurement. The results showed that no silicon dioxide remained on the film surface.

[0380] B: The PET film is peeled off from the laminate, but silica remains on the surface of the recovered PET film

[0381] C: The PET film is not peeled off from the laminate and cannot be recycled

[0382] <Separation of PET sealant + cured resin layer>

[0383] In the laminate recovered after immersion in a 5%-KOH aqueous solution, the separation state of the PET sealant+resin cured layer was evaluated by visual observation according to the following criteria and the results are shown in Table 6.

[0384] [Evaluation criteria]

[0385] A: PET sealant + cured resin layer peeled off from the laminate

[0386] C: PET sealant + cured resin layer is not peeled off from the laminate and cannot be recycled

[0387] Embodiments 24 to 26

[0388] Evaluation was carried out in the same manner as in Example 19 except that the aqueous solution in which the laminate was immersed in Example 23 was changed to that described in Table 6. The results are shown in Table 6.

[0389] Comparative Example 14

[0390] In Example 24, except that a urethane adhesive ("TM-569 / CAT-RT37" manufactured by Toyo-Morton Co., Ltd.) was used instead of the epoxy resin composition A obtained in Production Example 3, a laminate having the layer structure shown in Table 6 was prepared in the same manner as in Example 24 and evaluated. The results are shown in Table 6.

[0391] Comparative Examples 15-16

[0392] Evaluation was performed in the same manner as in Comparative Example 14 except that the aqueous solution in which the laminate was immersed in Comparative Example 14 was changed to that described in Table 6. The results are shown in Table 6.

[0393] [Table 6]

[0394]

[0395] Example 27 (Preparation of laminate and recovery of plastic film)

[0396] (Production of Laminated Body)

[0397] A laminate having the layer structure shown in Table 7 was produced in the following steps.

[0398] On one side of a biaxially stretched polyethylene terephthalate film (PET) ("E5100" manufactured by Toyobo Co., Ltd., thickness: 12 μm), white ink (a product obtained by diluting "BelleColor R115" manufactured by Sakata Inx Corporation by 2 times with a diluting solvent ("L solvent" manufactured by Sakata Inx Corporation)) was applied using a rod coater No. 8, and the film was heated at 80° C. for 10 seconds to dry (thickness after drying: about 0.5 μm), thereby forming a colored layer. On the colored layer, a reverse-side printing gravure ink (a product obtained by diluting "BelleFlora R medium" manufactured by Sakata Inx Corporation by 2 times with a diluting solvent ("K solvent" manufactured by Sakata Inx Corporation)) was applied using a rod coater No. 8, and the film was heated at 80° C. for 10 seconds to dry (thickness after drying: about 0.5 μm), thereby forming a medium layer.

[0399] Then, the epoxy resin composition A obtained in Manufacturing Example 3 was applied to the dielectric layer using a rod coater No. 8, and dried by heating at 80° C. for 10 seconds (thickness after drying: about 3 μm). The coated surface of the epoxy resin composition was made opposite to the vapor-deposited surface of a two-dimensional vapor-deposited PET sealant film ("VE034" manufactured by Toyobo Co., Ltd., thickness: 30 μm) having a two-dimensional vapor-deposited layer of silica-alumina formed on one side of the PET sealant, and the two layers were laminated with a nip roller and heated at 40° C. for 2 days to form a resin cured layer (III)-1, thereby obtaining a laminate having the layer structure shown in Table 7.

[0400] (Recycling and evaluation of plastic films)

[0401] The obtained laminate was cut into strips of 1.5 cm x 5 cm, and one strip of the laminate was immersed in a 5%-KOH aqueous solution (about 10 g) at 40°C for 16 hours. After the immersion, the laminate was recovered and subjected to the following evaluation.

[0402] <State of peeling interface and vapor deposition layer>

[0403] The same method as in Example 1 was used for evaluation.

[0404] <Separation of PET>

[0405] The separation state of the PET film from the laminate was evaluated based on the following criteria and is shown in Table 7. The SEM-EDX measurement conditions were the same as those described above.

[0406] [Evaluation criteria]

[0407] A: The PET film is peeled off from the laminate, and no ink layer remains on the surface of the recovered PET film.

[0408] B: The PET film is peeled off from the laminate, but the ink layer remains on the surface of the recovered PET film

[0409] C: The PET film is not peeled off from the laminate and cannot be recycled

[0410] <Separation of PET sealant>

[0411] The separation state of the PET sealant from the laminate was evaluated according to the following criteria and the results are shown in Table 7.

[0412] [Evaluation criteria]

[0413] A: PET sealant was peeled off from the laminate, and the surface of the recovered PET sealant was analyzed by SEM-EDX measurement. The results showed that no 2-element vapor deposition layer remained on the sealant surface.

[0414] B: PET sealant is peeled off from the laminate, but the 2-element vapor-deposited layer remains on the surface of the recycled PET sealant

[0415] C: PET sealant is not peeled off from the laminate and cannot be recycled

[0416] Embodiments 28 to 31

[0417] Evaluation was carried out in the same manner as in Example 27 except that the aqueous solution in which the laminate was immersed was changed to that described in Table 7. The results are shown in Table 7.

[0418] Comparative Example 17

[0419] In Example 27, except that a urethane adhesive ("TM-569 / CAT-RT37" manufactured by Toyo-Morton Co., Ltd.) was used instead of the epoxy resin composition A obtained in Production Example 3, a laminate having the layer structure shown in Table 7 was prepared in the same manner as in Example 27 and evaluated. The results are shown in Table 7.

[0420] Comparative Examples 18 to 21

[0421] Evaluation was performed in the same manner as in Comparative Example 17 except that the aqueous solution in which the laminate was immersed in Comparative Example 17 was changed to that described in Table 7. The results are shown in Table 7.

[0422] [Table 7]

[0423]

[0424] As shown in Tables 5 to 7, according to the method of the present invention, even when using laminates with different layer structures, the plastic film (PET or PET sealant) can be separated using an acid aqueous solution or an alkali aqueous solution. In addition, it can be seen that when the vapor-deposited layer in the laminate contains silicon dioxide, it is preferably in contact with an alkali aqueous solution.

[0425] Example 32 (Recycling of plastic film based on actual machine)

[0426] Using the laminate having the layer structure of Example 1 (OPP / ink layer / resin cured layer (III) / Al vapor deposited layer / CPP), the plastic film was recovered by the following method.

[0427] The laminated body (film roll with a width of 300 mm) of the layer structure of Example 1 was put into a dry pulverizer having a fixed blade and a rotating blade and equipped with a screen with a mesh size of 12 mm, and the laminated body was pulverized. The shape of the pulverized laminated body was as follows: Figure 1 shown.

[0428] 300 mL of 1N-lactic acid aqueous solution was added to a 500 mL separable flask and heated to 75° C. using an oil bath. After heating to 75° C., 10 g of the pulverized laminate was added to the flask and stirred at 240 rpm for 1 hour using a stirring blade. In addition, it was confirmed that the aluminum vapor-deposited layer was completely dissolved at the time point of stirring for 30 minutes.

[0429] After stirring for 1 hour, the flask was taken out of the oil bath and left to cool, and stirred for another 1 hour. After the stirring was completed, the separated resin solidified layer was precipitated at the bottom of the flask, and the OPP / ink layer and CPP film floated on the surface of the aqueous solution, and the OPP / ink layer and CPP film could be easily recovered.

[0430] The recovered film was placed in 500 mL of water and stirred at 300 rpm for 1 hour at room temperature for cleaning. SEM-EDX analysis of the cleaned OPP / ink layer and CPP film showed that no residual aluminum vapor deposition layer was observed.

[0431] In addition, when the plastic film recovery test was conducted again using the lactic acid aqueous solution after the resin cured layer and the film were recovered in the same manner as above, the same results as above were obtained. Therefore, it can be said that the lactic acid aqueous solution can be reused.

[0432] Industrial Applicability

[0433] According to the method of the present invention, the plastic film can be efficiently recovered from a laminate containing the plastic film. In the method of the present invention, the degree of freedom of the recovery conditions of the plastic film is high, and in particular, the plastic film can be easily recovered from a laminate having a laminated form of two or more plastic films.

Claims

1. A method for recovering a plastic film from a laminate, wherein: The laminate comprises: Plastic film (I); an inorganic layer (II) of at least one selected from the group consisting of silicon oxide, aluminum, and aluminum oxide; and Resin cured layer (III), The resin cured layer (III) is a cured product of an epoxy resin composition, wherein the epoxy resin composition contains an epoxy resin and an epoxy resin curing agent including an amine curing agent. The method includes a step of bringing the laminate into contact with an acid aqueous solution or an alkali aqueous solution.

2. The method according to claim 1, wherein: The amine curing agent comprises the following amine curing agent (i), (i) a reaction product of the following component (A) and component (B): (A) at least one selected from the group consisting of m-xylylenediamine and p-xylylenediamine (B) at least one selected from the group consisting of an unsaturated carboxylic acid represented by the following general formula (1) and its derivatives, In formula (1), R 1 , R 2 Each independently represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aralkyl group having 7 to 13 carbon atoms.

3. The method according to claim 1 or 2, wherein: The inorganic layer (II) is an inorganic evaporated layer.

4. The method according to any one of claims 1 to 3, wherein: The inorganic layer (II) is an aluminum vapor-deposited layer.

5. The method according to any one of claims 1 to 4, wherein: The laminate comprises two or more plastic films (I).

6. The method according to any one of claims 1 to 5, wherein: In the epoxy resin composition, the ratio of the number of active hydrogens in the epoxy resin curing agent to the number of epoxy groups in the epoxy resin (number of active hydrogens in the epoxy resin curing agent / number of epoxy groups in the epoxy resin) is in the range of 0.2 to 8.

0.

7. The method according to any one of claims 1 to 6, wherein: The thickness of the resin cured layer (III) is 0.05 to 20 μm.

8. The method according to any one of claims 1 to 7, wherein: The laminate further includes an ink layer. 9 . The method according to claim 1 , further comprising the step of immersing the laminate in an aqueous acid solution.