Vacuum insulated panel core material as well as preparation method and application thereof
By adding nanofillers and multi-stage stretching process to PET, the problem of high core density of vacuum insulation boards is solved, and a lightweight, high-insulation and low-thermal conduction vacuum insulation board is achieved, which improves the comprehensive performance and service life of the product .
Patent Information
- Application Number
- CN202411077956.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-19
AI Technical Summary
The existing vacuum insulation board core material has a high density, resulting in an increase in product weight, a decrease in production efficiency, a high transportation cost, and an increase in structural load, which limits the industrial development of low-energy consumption and high-temperature insulation products.
By adding specific amounts and proportions of nanosilicon dioxide and nanoalumina to PET, combined with twin-screw extruder and spinneret technology, a multi-stage stretching process is carried out to significantly reduce the core material density and thermal conductivity and improve the vacuum insulation plate. comprehensive performance.
It significantly reduces the weight and thermal conductivity of the vacuum insulation plate, improves tensile strength and wear resistance, extends service life, reduces transportation and installation difficulty, and meets the demand for lightweight and high-temperature insulation materials in special fields.
Smart Images

Figure CN118977385A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of vacuum thermal insulation materials, and in particular to a method for preparing a vacuum thermal insulation board core material. Background Art
[0002] "Dual carbon" is the abbreviation of carbon peak and carbon neutrality. With the increasing requirements of "dual carbon", the development of home appliances, biology, medical care, materials and other fields has put higher and higher requirements on thermal insulation materials.
[0003] Vacuum insulation panels (VIP) play an important role in achieving the "dual carbon" goals. VIP panels are a highly efficient thermal insulation material with extremely low thermal conductivity and good thermal insulation effect. Its high thermal insulation performance can significantly reduce energy consumption in construction and cold chain logistics, thereby reducing carbon dioxide emissions. In addition, the raw materials of VIP panels do not contain ozone-depleting substances and have environmentally friendly characteristics. In the construction field, VIP panels can be used for exterior wall insulation, energy-saving renovation of existing buildings, and new ultra-low energy consumption buildings, significantly improving the thermal insulation performance of buildings and reducing energy consumption. In short, as an advanced insulation material, VIP panels have important application prospects and contributions in achieving the "dual carbon" goals.
[0004] The core material of the vacuum insulation board in the prior art is usually made of inorganic fiber or composite fiber, which results in a high density of the vacuum insulation board, and inconvenient operation when using the ultra-thick VIP board. For example, CN 117432884A discloses a vacuum insulation board core material, a vacuum insulation board and a method for preparing a vacuum insulation board, wherein the vacuum insulation board core material used is a layered structure, and the vacuum insulation board core material includes a hollow structure layer, a first inorganic fiber layer and a second inorganic fiber layer, wherein the hollow structure layer has a plurality of cavities; the first inorganic fiber layer and the second inorganic fiber layer are respectively arranged on opposite sides of the hollow structure layer. And by setting the vacuum insulation board core material as a layered structure, a hollow structure layer is arranged between the first inorganic fiber layer and the second inorganic fiber layer. Since the hollow structure layer has a plurality of cavities, the density of the vacuum insulation board core material can be reduced, and the inorganic fiber layer is any one of glass fiber, ceramic fiber and rock wool fiber or a mixture of at least two.
[0005] It can be seen that most vacuum insulation panels at home and abroad currently use inorganic fibers (chopped glass fiber, ultra-fine glass wool, rock wool, ceramic fiber, etc.) as core materials. However, inorganic fibers themselves have a high density and a high self-weight, which does not meet the needs of certain special fields or special products. For example, the industry currently has increasingly higher requirements for insulation products such as refrigerators, and thicker vacuum insulation panels are needed to meet this requirement. Thicker vacuum insulation panels mean increased product self-weight, reduced product production efficiency, higher transportation costs, and increased structural loads, which in turn leads to a decrease in the overall quality of the product, restricting the industrial development of low-energy consumption and high-insulation products.
[0006] Therefore, developing a new lightweight, high thermal insulation vacuum insulation board core material to overcome the problems of existing inorganic fiber board core materials, reduce the self-weight of vacuum insulation boards, improve the production efficiency of related products, reduce product transportation costs, and reduce structural loads is of great significance to the development of the industry. Summary of the invention
[0007] In order to solve the above problems, the present invention provides a vacuum insulation panel core material and a preparation method and application thereof. The present invention significantly reduces the density and thermal conductivity of the core material and improves the comprehensive performance of the vacuum insulation panel by using a specific amount and a specific proportion of nanofillers combined with a specific stretching process.
[0008] A method for preparing a vacuum insulation panel core material comprises the following steps:
[0009] S1, mixing PET with nano silicon dioxide, nano aluminum oxide and polyethylene oxide to obtain a mixed raw material;
[0010] S2, melting the mixed raw material in a twin-screw extruder, then transferring it from a melt pump to a spinneret for melt spinning, and then cooling it to obtain a raw fiber;
[0011] S3, stretching the raw silk to obtain a vacuum insulation board core material.
[0012] Further, the addition amount of the nano-silicon dioxide and nano-alumina is 0.1wt% to 5wt% of PET. Preferably, the addition amount of the nano-silicon dioxide and nano-alumina is 1wt% to 3wt% of PET; more preferably, the addition amount of the nano-silicon dioxide and nano-alumina is 2.5wt% of PET.
[0013] Furthermore, the weight ratio of the nano-silicon dioxide to the nano-alumina is (1-2):(4-5). Preferably, the weight ratio of the nano-silicon dioxide to the nano-alumina is 1:5.
[0014] Further, the amount of polyethylene oxide added is 0.1 wt% to 1 wt% of PET. Preferably, the amount of polyethylene oxide added is 0.4 wt% to 0.6 wt% of PET. More preferably, the amount of polyethylene oxide added is 0.5 wt% of PET.
[0015] Furthermore, the twin-screw extruder is a co-rotating twin-screw extruder.
[0016] Further, the aspect ratio of the twin-screw extruder is (20-40): 1. Preferably, the aspect ratio of the twin-screw extruder is (30-40): 1. More preferably, the aspect ratio of the twin-screw extruder is 40:1.
[0017] Further, the twin-screw extruder adopts four-zone heating, wherein the heating temperature of the first zone is 280°C to 290°C, the heating temperature of the second zone is 290°C to 300°C, the heating temperature of the third zone is 300°C to 310°C, and the heating temperature of the fourth zone is 310°C to 320°C. Preferably, the twin-screw extruder adopts four-zone heating, wherein the heating temperature of the first zone is 280°C, the heating temperature of the second zone is 290°C, the heating temperature of the third zone is 310°C, and the heating temperature of the fourth zone is 320°C.
[0018] Further, the screw speed of the twin-screw extruder is 150 to 200 rpm. Preferably, the screw speed of the twin-screw extruder is 160 to 190 rpm. More preferably, the screw speed of the twin-screw extruder is 180 rpm.
[0019] Furthermore, the apparent shear velocity of the spinning nozzle wall is 250 to 400 s. -1 , the spinneret temperature is 320°C to 350°C. Preferably, the apparent shear velocity of the spinning nozzle wall is 250 to 350s -1 , the spinneret temperature is 320°C to 340°C. More preferably, the apparent shear velocity of the spinning nozzle wall is 350s -1 , the spinneret temperature is 330℃.
[0020] Furthermore, the cooling is water cooling or air cooling.
[0021] Further, the stretching is performed in three passes, the first stretching temperature is 180-230°C, the second stretching temperature is 100°C-150°C, the third stretching temperature is 50°C-100°C, and the stretching ratio is (1-10): 1. Preferably, the stretching is performed in three passes, the first stretching temperature is 190-220°C, the second stretching temperature is 110°C-140°C, the third stretching temperature is 60°C-90°C, and the stretching ratio is (2-5): 1. More preferably, the stretching is performed in three passes, the first stretching temperature is 200°C, the second stretching temperature is 135°C, the third stretching temperature is 75°C, and the stretching ratio is 3.5:1.
[0022] Furthermore, the core material diameter of the vacuum insulation panel is 4 to 12 μm.
[0023] The present invention also provides a vacuum insulation board core material prepared according to the above method.
[0024] The vacuum insulation panel core material of the present invention is used for preparing high-performance lightweight vacuum insulation panels.
[0025] The high-performance lightweight vacuum insulation panel includes a core board, the surface of the core board is wrapped with a film material, and a getter is arranged inside the core board; the film material includes a vacuum-evaporated aluminum BOPP film, a TPEE film, an EVAL film and a TPV aluminum-plated film, the outer surface of the vacuum-evaporated aluminum BOPP film is bonded to the TPEE film by polyurethane glue, the outer surface of the TPEE film is bonded to the EVAL film by polyurethane glue, and the outer surface of the EVAL film is bonded to the TPV aluminum-plated film by polyurethane glue.
[0026] Furthermore, the thickness of the TPEE film is 5 to 20 μm.
[0027] Furthermore, the thickness of the EVAL film is 5 to 15 μm.
[0028] Compared with the prior art, the beneficial technical effects of the present invention are:
[0029] The invention significantly reduces the thermal conductivity of the core material by adding a specific amount of nano silicon dioxide and nano aluminum oxide into PET, thereby improving the thermal insulation performance of the vacuum insulation panel.
[0030] The core material of the vacuum insulation panel of the present invention has higher tensile strength and wear resistance, so that the core material is more durable and stable during use.
[0031] The core material of the vacuum insulation panel of the present invention has a low density, so that the weight of the vacuum insulation panel is significantly reduced, and it is convenient to transport and install.
[0032] The core material of the vacuum insulation board of the present invention has high chemical stability, so that it can still maintain good performance in harsh environments.
[0033] The invention significantly improves the durability and service life of the core material by optimizing the ratio of the fiber and the nano material.
[0034] The vacuum insulation board core material of the present invention retains the excellent properties of traditional glass fiber while further improving the comprehensive performance of the core material in other aspects, and significantly reduces the weight of the core material (up to about 50% reduction) and thermal conductivity, and can reduce the thickness and weight of the board while ensuring good thermal insulation performance. The vacuum insulation board core of the present invention has significant advantages in improving construction efficiency, reducing transportation costs, reducing structural loads, and improving portability, and can meet the special needs of certain special fields, special working conditions, and special products for vacuum insulation boards. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] The present invention will be further described below in conjunction with the accompanying drawings.
[0036] Figure 1 This is a process flow chart of the preparation of the core material of the vacuum insulation panel of the present invention;
[0037] Figure 2 This is a schematic diagram of the structure of the high-performance lightweight vacuum insulation panel of the present invention;
[0038] Explanation of the reference numerals: 1. Film material, 11. Vacuum-evaporated aluminum BOPP film, 12. TPEE film, 13. EVAL film, 14. TPV aluminum-coated film, 2. Core board, 3. Getter. DETAILED DESCRIPTION
[0039] The present invention provides a method for preparing a vacuum insulation panel core material, comprising the following steps:
[0040] S1, mixing PET with nano silicon dioxide, nano aluminum oxide and polyethylene oxide at high speed at room temperature to obtain a mixed raw material;
[0041] S2, melting the mixed raw material in a twin-screw extruder, then transferring it from a melt pump to a spinneret for melt spinning, and then cooling it to obtain a raw fiber;
[0042] S3, stretching the raw silk to obtain a vacuum insulation board core material.
[0043] In one embodiment, the addition amount of the nano-silicon dioxide and nano-aluminum oxide is 0.1 wt% to 5 wt% of PET.
[0044] In one embodiment, the addition amount of the nano silicon dioxide and nano aluminum oxide is 1 wt% to 3 wt% of PET.
[0045] In one embodiment, the addition amount of the nano-silicon dioxide and nano-aluminum oxide is 2.5 wt % of PET.
[0046] In one embodiment, the weight ratio of the nano-silicon dioxide to the nano-aluminum oxide is (1-2):(4-5).
[0047] In one embodiment, the weight ratio of the nano-silicon dioxide to the nano-aluminum oxide is 1:5.
[0048] The present invention promotes the crystallinity, molecular chain orientation and grain refinement of the fiber to varying degrees by adding nano-silicon dioxide and nano-alumina. Specifically, the addition of a specific amount of nano-filler improves the fluidity of the raw material and inhibits the crystallization and molecular chain orientation in the primary silk. After multi-stage stretching at a specific temperature, the crystallinity and molecular chain orientation of the fiber are improved, and the comprehensive properties related to mechanical properties, thermal stability, chemical stability, etc. are significantly improved. In addition, more importantly, the addition of fillers in a specific proportion can reduce the amorphous area in the fiber, thereby reducing the hygroscopicity of the fiber. Hygroscopicity is one of the important factors affecting the performance of vacuum insulation board core materials, especially vacuum insulation board core materials prepared from polymer materials (glass fiber materials themselves have low hygroscopicity, while fibers prepared from polymer materials have high hygroscopicity). Vacuum insulation board core materials with high hygroscopicity will absorb moisture in the air, resulting in an increase in thermal conductivity, thereby reducing insulation performance; at the same time, core materials with high hygroscopicity will shorten the service life, increase weight, and may trigger internal chemical reactions, resulting in material degradation or performance degradation. Therefore, the use of nanofillers can reduce the hygroscopicity of the core material, thereby ensuring its excellent thermal insulation performance and extending the service life of the product.
[0049] But at the same time, the present invention strictly limits the amount of nanofiller used and the ratio between nanosilica and nanoalumina. Limiting the amount of nanofiller added can optimize the core material performance and ensure the uniform dispersion of nanofiller. Appropriate nanofiller addition can significantly improve the thermal conductivity, tensile strength and wear resistance of the material, while avoiding uneven dispersion and performance degradation caused by too much or too little. In addition, a reasonable amount of addition helps to control production costs, avoid adverse reactions such as material embrittlement, and ensure its stability and reliability in practical applications. Secondly, limiting the ratio of nanosilica and nanoalumina is to optimize the comprehensive performance of the material. Different ratios will affect the thermal conductivity, mechanical strength and wear resistance of the material. By optimizing the ratio, it can be ensured that the material has the best comprehensive performance. In addition, the reasonable ratio of the two nanofillers helps to evenly disperse the nanomaterials in the matrix, avoid agglomeration, and thus improve the overall performance of the material.
[0050] In one embodiment, the amount of polyethylene oxide added is 0.1 wt% to 1 wt% of PET.
[0051] In one embodiment, the amount of polyethylene oxide added is 0.4 wt % to 0.6 wt % of PET.
[0052] In one embodiment, the amount of polyethylene oxide added is 0.5 wt % of PET.
[0053] In actual research, it is found that the addition amount of nanofiller within a certain range can make the core material have the best comprehensive performance, especially thermal conductivity and mechanical properties. However, under this condition, the amount of nanofiller used is high and it is difficult to achieve good dispersion. Therefore, the present invention prevents the agglomeration of nanofillers and improves its dispersibility by adding a certain amount of polyethylene oxide. At the same time, the addition of polyethylene oxide can also avoid the aggregation of nanoparticles in the amorphous region during the subsequent stretching process. In addition, the interaction between polyethylene oxide and nanoparticles can enhance the interfacial bonding force, thereby improving the mechanical properties and stability of the core material, so that the final core material has higher strength and heat resistance. In addition, the synergistic effect of polyethylene oxide and nanomaterials can effectively reduce the thermal conductivity of the material, thereby improving the thermal insulation performance. Although some raw materials can reduce the thermal conductivity of the material to a certain extent, the effect is significantly less than polyethylene oxide. Therefore, the present invention strictly limits the addition of polyethylene oxide. In addition, the presence of polyethylene oxide can improve the fluidity of the mixture, making it easier to handle and shape during processing. That is, polyethylene oxide can improve the fluidity of the mixture while reducing the thermal conductivity of the material, which is not available in other raw materials except polyethylene oxide.
[0054] In one embodiment, the twin-screw extruder is a co-rotating twin-screw extruder.
[0055] In one embodiment, the aspect ratio of the twin-screw extruder is (20-40):1.
[0056] In one embodiment, the aspect ratio of the twin-screw extruder is (30-40):1.
[0057] In one embodiment, the length-to-diameter ratio of the twin-screw extruder is 40:1.
[0058] In one embodiment, the twin-screw extruder adopts four-zone heating, wherein the heating temperature of the first zone is 280℃~290℃, the heating temperature of the second zone is 290℃~300℃, the heating temperature of the third zone is 300℃~310℃, and the heating temperature of the fourth zone is 310℃~320℃.
[0059] In one embodiment, the twin-screw extruder adopts four-zone heating, wherein the heating temperature of the first zone is 280°C, the heating temperature of the second zone is 290°C, the heating temperature of the third zone is 310°C, and the heating temperature of the fourth zone is 320°C.
[0060] In one embodiment, the screw speed of the twin-screw extruder is 150-200 rpm.
[0061] In one embodiment, the screw speed of the twin-screw extruder is 160-190 rpm.
[0062] In one embodiment, the screw speed of the twin-screw extruder is 180 rpm.
[0063] In one embodiment, the apparent shear velocity of the spinning nozzle wall is 250-400 s -1 , the spinneret temperature is 320℃~350℃.
[0064] In one embodiment, the apparent shear velocity of the spinning nozzle wall is 250 to 350 s -1 , the spinneret temperature is 320℃~340℃.
[0065] In one embodiment, the apparent shear velocity of the spinning nozzle wall is 350s -1 , the spinneret temperature is 330℃.
[0066] The present invention strictly limits the apparent shear velocity of the spinning nozzle wall to ensure the quality and performance of the fiber during the spinning process. An appropriate shear velocity can help control the diameter of the fiber so that it is within a predetermined range, thereby ensuring the uniformity and consistency of the fiber; it helps the orderly arrangement and orientation of the molecular chains, increases the number of crystalline regions, and improves the mechanical strength and wear resistance of the fiber; it prevents the fiber from breaking or producing defects during the spinning process, reduces the occurrence of broken fibers and defects, and improves production efficiency and product quality; it optimizes processing conditions to ensure the stability and controllability of the spinning process. By reasonably limiting the apparent shear velocity of the spinning nozzle wall, the quality and performance of the core material can be significantly improved, ensuring its excellent performance in the core material of the vacuum insulation board.
[0067] In one embodiment, the cooling is water cooling or air cooling.
[0068] In one embodiment, the stretching is performed in three passes, the first stretching temperature is 180-230°C, the second stretching temperature is 100-150°C, the third stretching temperature is 50-100°C, and the stretching ratio is (1-10):1.
[0069] In one embodiment, the stretching is performed in three passes, the first stretching temperature is 190-220°C, the second stretching temperature is 110-140°C, the third stretching temperature is 60-90°C, and the stretching ratio is (2-5):1.
[0070] In one embodiment, the stretching is performed in three passes, the first stretching temperature is 200° C., the second stretching temperature is 135° C., the third stretching temperature is 75° C., and the stretching ratio is 3.5:1.
[0071] The present invention adopts three stretching passes at different temperatures, that is, by gradually stretching the modified fiber at high temperature, medium temperature and low temperature, to optimize the mechanical properties and structural stability of the fiber. The first stretching pass is carried out at high temperature to preliminarily shape the fiber and eliminate internal stress; the second stretching pass is carried out at medium temperature to further adjust the molecular arrangement, improve uniformity and toughness; the third stretching pass is carried out at low temperature to ensure the final shaping and stability, and further improve the mechanical properties and wear resistance. Through this staged stretching treatment, a core material with excellent performance is finally obtained, which significantly improves the overall performance of the core material of the vacuum insulation board. In addition, the stretching of the present invention is carried out at a higher temperature to promote the nanofiller to play a positive role in the stretching process. That is, the orderly orientation of the molecular chain segments in the molecular chain is achieved, so that more crystalline regions are produced in the amorphous region. This orderly orientation and the increase of the crystalline region significantly improve the mechanical properties and structural stability of the fiber, so that the core material fiber shows more excellent performance in the core material of the vacuum insulation board.
[0072] In one embodiment, the core material of the vacuum insulation panel has a diameter of 4 to 12 μm.
[0073] The present invention also provides a vacuum insulation board core material prepared according to the above method.
[0074] The vacuum insulation panel core material of the present invention is used for preparing high-performance lightweight vacuum insulation panels.
[0075] The high-performance lightweight vacuum insulation panel includes a core board, the surface of the core board is wrapped with a film material, and a getter is arranged inside the core board; the film material includes a vacuum-evaporated aluminum BOPP film, a TPEE film, an EVAL film and a TPV aluminum-plated film, the outer surface of the vacuum-evaporated aluminum BOPP film is bonded to the TPEE film by polyurethane glue, the outer surface of the TPEE film is bonded to the EVAL film by polyurethane glue, and the outer surface of the EVAL film is bonded to the TPV aluminum-plated film by polyurethane glue.
[0076] In one embodiment, the TPEE film has a thickness of 5 to 20 μm.
[0077] In one embodiment, the EVAL film has a thickness of 5 to 15 μm.
[0078] The technical solution provided by the present invention is further described below in conjunction with embodiments.
[0079] Example 1
[0080] A method for preparing a vacuum insulation panel core material, comprising the following steps:
[0081] S1, PET and 2.5wt% of nano filler (nano silicon dioxide, nano aluminum oxide) and 0.5wt% of polyethylene oxide are uniformly mixed to obtain a mixed raw material;
[0082] The weight ratio of nano silicon dioxide to nano aluminum oxide is 1:5;
[0083] S2, melting the mixed raw material in a co-rotating twin-screw extruder with a length-to-diameter ratio of 40:1, and then transferring the mixed raw material from a melt pump to a spinneret for melt spinning, and then water cooling to obtain raw yarn;
[0084] The twin-screw extruder adopts four-zone heating, wherein the heating temperature of the first zone is 280°C, the heating temperature of the second zone is 290°C, the heating temperature of the third zone is 310°C, the heating temperature of the fourth zone is 320°C, the screw speed is 180rpm; the apparent shear velocity of the spinning nozzle wall is 350s -1 , spinneret temperature is 330℃;
[0085] S3, stretching the raw silk to obtain a vacuum insulation panel core material with a diameter of 12 μm;
[0086] The stretching is performed in three passes, with the first stretching temperature being 200° C., the second stretching temperature being 135° C., the third stretching temperature being 75° C., and the stretching ratio being 3.5:1.
[0087] Example 2
[0088] A method for preparing a vacuum insulation panel core material, comprising the following steps:
[0089] S1, PET and 1wt% of nano filler (nano silicon dioxide, nano aluminum oxide) and 0.4wt% of polyethylene oxide are uniformly mixed to obtain a mixed raw material;
[0090] The weight ratio of nano silicon dioxide to nano aluminum oxide is 1:5;
[0091] S2, melting the mixed raw material in a co-rotating twin-screw extruder with a length-to-diameter ratio of 40:1, and then transferring the mixed raw material from a melt pump to a spinneret for melt spinning, and then water cooling to obtain raw yarn;
[0092] The twin-screw extruder adopts four-zone heating, wherein the heating temperature of the first zone is 280°C, the heating temperature of the second zone is 290°C, the heating temperature of the third zone is 300°C, the heating temperature of the fourth zone is 310°C, the screw speed is 160rpm; the apparent shear rate of the spinning nozzle wall is 250s -1 , spinneret temperature is 320℃;
[0093] S3, stretching the raw silk to obtain a vacuum insulation panel core material with a diameter of 12 μm;
[0094] The stretching is performed in three passes, with the first stretching temperature being 190° C., the second stretching temperature being 110° C., the third stretching temperature being 60° C., and the stretching ratio being 3.5:1.
[0095] Example 3
[0096] A method for preparing a vacuum insulation panel core material, comprising the following steps:
[0097] S1, PET and 3wt% of nano filler (nano silicon dioxide, nano aluminum oxide) and 0.6wt% of polyethylene oxide are uniformly mixed to obtain a mixed raw material;
[0098] The weight ratio of nano silicon dioxide to nano aluminum oxide is 1:5;
[0099] S2, melting the mixed raw material in a co-rotating twin-screw extruder with a length-to-diameter ratio of 40:1, and then transferring the mixed raw material from a melt pump to a spinneret for melt spinning, and then water cooling to obtain raw yarn;
[0100] The twin-screw extruder adopts four-zone heating, wherein the heating temperature of the first zone is 290°C, the heating temperature of the second zone is 300°C, the heating temperature of the third zone is 310°C, the heating temperature of the fourth zone is 320°C, the screw speed is 190rpm; the apparent shear rate of the spinning nozzle wall is 350s -1 , spinneret temperature is 340℃;
[0101] S3, stretching the raw silk to obtain a vacuum insulation panel core material with a diameter of 12 μm;
[0102] The stretching is performed in three passes, with the first stretching temperature being 220° C., the second stretching temperature being 140° C., the third stretching temperature being 90° C., and the stretching ratio being 3.5:1.
[0103] Example 4
[0104] Same as Example 1, except that the weight ratio of the nano-silicon dioxide to the nano-aluminum oxide is 2:4.
[0105] Example 5
[0106] Same as Example 1, except that the stretching ratio is 2:1.
[0107] Example 6
[0108] Same as Example 1, except that the stretching ratio is 5:1.
[0109] Comparative Example 1
[0110] Same as Example 1, except that the added amount of the nanofiller is 7 wt % of PET.
[0111] Comparative Example 2
[0112] Same as Example 1, except that the amount of polyethylene oxide added is 1.5 wt % of PET.
[0113] Comparative Example 3
[0114] Same as Example 1, except that the apparent shear velocity of the spinning nozzle wall is 200 s -1 .
[0115] Comparative Example 4
[0116] Same as Example 1, except that: the stretching is performed in three passes, the first stretching temperature is 150°C, the second stretching temperature is 80°C, and the third stretching temperature is 40°C.
[0117] Comparative Example 5
[0118] Same as Example 1, except that the stretching ratio is 15:1.
[0119] Test Example 1
[0120] The performance of the materials in the examples and comparative examples was tested, with ordinary glass fibers of the same specifications used as controls. The test results are as follows:
[0121] Thermal conductivity (mW / mk) <![CDATA[Tensile strength (cN·dtex -1 )]]> Surface morphology Example 1 1.7±0.12 3.61±0.15 Smooth surface Example 2 2.0±0.04 3.52±0.23 Smooth surface Example 3 1.6±0.09 3.70±0.07 Smooth surface Example 4 2.3±0.15 3.62±0.19 Smooth surface Example 5 2.1±0.07 3.66±0.13 Smooth surface Example 6 1.7±0.10 3.58±0.04 Smooth surface Comparative Example 1 1.5±0.09 3.82±0.08 Rough surface Comparative Example 2 1.8±0.04 3.64±0.22 Smooth surface Comparative Example 3 1.7±0.13 3.33±0.24 Rough surface Comparative Example 4 2.4±0.17 3.27±0.13 Rough surface Comparative Example 5 1.7±0.06 3.32±0.18 Rough surface, a few cracks Control group 4.2±1.12 3.85±0.16 Smooth surface
[0122] After testing, the density of the product of Example 1 of the present invention after compression is 201kg / m 3 ±5kg / m 3 , significantly lower than the common glass fiber (310kg / m 3 ±7kg / m 3 ).
[0123] Example 8
[0124] A method for preparing a vacuum insulation panel core material, comprising the following steps:
[0125] S1, PET and 5wt% of nano filler (nano silicon dioxide, nano aluminum oxide) and 0.5wt% of polyethylene oxide are uniformly mixed to obtain a mixed raw material;
[0126] The weight ratio of nano silicon dioxide to nano aluminum oxide is 1:5;
[0127] S2, melting the mixed raw material in a co-rotating twin-screw extruder with a length-to-diameter ratio of 40:1, and then transferring the mixed raw material from a melt pump to a spinneret for melt spinning, and then water cooling to obtain raw yarn;
[0128] The twin-screw extruder adopts four-zone heating, wherein the heating temperature of the first zone is 280°C, the heating temperature of the second zone is 290°C, the heating temperature of the third zone is 310°C, the heating temperature of the fourth zone is 320°C, the screw speed is 180rpm; the apparent shear velocity of the spinning nozzle wall is 350s -1, spinneret temperature is 330℃;
[0129] S3, stretching the raw silk to obtain a vacuum insulation panel core material with a diameter of 12 μm;
[0130] The stretching is performed in three passes, with the first stretching temperature being 200° C., the second stretching temperature being 135° C., the third stretching temperature being 75° C., and the stretching ratio being 3.5:1.
[0131] Example 9
[0132] A method for preparing a vacuum insulation panel core material, comprising the following steps:
[0133] S1, PET and 2.5wt% of nano filler (nano silicon dioxide, nano aluminum oxide) and 0.5wt% of polyethylene oxide are uniformly mixed to obtain a mixed raw material;
[0134] The weight ratio of nano silicon dioxide to nano aluminum oxide is 1:4;
[0135] S2, melting the mixed raw material in a co-rotating twin-screw extruder with a length-to-diameter ratio of 40:1, and then transferring the mixed raw material from a melt pump to a spinneret for melt spinning, and then water cooling to obtain raw yarn;
[0136] The twin-screw extruder adopts four-zone heating, wherein the heating temperature of the first zone is 280°C, the heating temperature of the second zone is 290°C, the heating temperature of the third zone is 310°C, the heating temperature of the fourth zone is 320°C, the screw speed is 180rpm; the apparent shear velocity of the spinning nozzle wall is 350s -1 , spinneret temperature is 330℃;
[0137] S3, stretching the raw silk to obtain a vacuum insulation panel core material with a diameter of 12 μm;
[0138] The stretching is performed in three passes, with the first stretching temperature being 200° C., the second stretching temperature being 135° C., the third stretching temperature being 75° C., and the stretching ratio being 3.5:1.
[0139] Example 10
[0140] A method for preparing a vacuum insulation panel core material, comprising the following steps:
[0141] S1, PET and 2.5wt% of nano filler (nano silicon dioxide, nano aluminum oxide) and 0.5wt% of polyethylene oxide are uniformly mixed to obtain a mixed raw material;
[0142] The weight ratio of nano silicon dioxide to nano aluminum oxide is 2:5;
[0143] S2, melting the mixed raw material in a co-rotating twin-screw extruder with a length-to-diameter ratio of 40:1, and then transferring the mixed raw material from a melt pump to a spinneret for melt spinning, and then water cooling to obtain raw yarn;
[0144] The twin-screw extruder adopts four-zone heating, wherein the heating temperature of the first zone is 280°C, the heating temperature of the second zone is 290°C, the heating temperature of the third zone is 310°C, the heating temperature of the fourth zone is 320°C, the screw speed is 180rpm; the apparent shear velocity of the spinning nozzle wall is 350s -1 , spinneret temperature is 330℃;
[0145] S3, stretching the raw silk to obtain a vacuum insulation panel core material with a diameter of 12 μm;
[0146] The stretching is performed in three passes, with the first stretching temperature being 200° C., the second stretching temperature being 135° C., the third stretching temperature being 75° C., and the stretching ratio being 3.5:1.
[0147] Embodiment 11
[0148] A method for preparing a vacuum insulation panel core material, comprising the following steps:
[0149] S1, PET and 2.5wt% of nano filler (nano silicon dioxide, nano aluminum oxide) and 1wt% of polyethylene oxide are uniformly mixed to obtain a mixed raw material;
[0150] The weight ratio of nano silicon dioxide to nano aluminum oxide is 1:5;
[0151] S2, melting the mixed raw material in a co-rotating twin-screw extruder with a length-to-diameter ratio of 40:1, and then transferring the mixed raw material from a melt pump to a spinneret for melt spinning, and then water cooling to obtain raw yarn;
[0152] The twin-screw extruder adopts four-zone heating, wherein the heating temperature of the first zone is 280°C, the heating temperature of the second zone is 290°C, the heating temperature of the third zone is 310°C, the heating temperature of the fourth zone is 320°C, the screw speed is 180rpm; the apparent shear velocity of the spinning nozzle wall is 350s -1 , spinneret temperature is 330℃;
[0153] S3, stretching the raw silk to obtain a vacuum insulation panel core material with a diameter of 12 μm;
[0154] The stretching is performed in three passes, with the first stretching temperature being 200° C., the second stretching temperature being 135° C., the third stretching temperature being 75° C., and the stretching ratio being 3.5:1.
[0155] Example 12
[0156] A method for preparing a vacuum insulation panel core material, comprising the following steps:
[0157] S1, PET and 2.5wt% of nano filler (nano silicon dioxide, nano aluminum oxide) and 0.5wt% of polyethylene oxide are uniformly mixed to obtain a mixed raw material;
[0158] The weight ratio of nano silicon dioxide to nano aluminum oxide is 1:5;
[0159] S2, melting the mixed raw material in a co-rotating twin-screw extruder with a length-to-diameter ratio of 30:1, and then transferring the mixed raw material from a melt pump to a spinneret for melt spinning, and then water cooling to obtain raw yarn;
[0160] The twin-screw extruder adopts four-zone heating, wherein the heating temperature of the first zone is 280°C, the heating temperature of the second zone is 290°C, the heating temperature of the third zone is 310°C, the heating temperature of the fourth zone is 320°C, the screw speed is 180rpm; the apparent shear velocity of the spinning nozzle wall is 350s -1 , spinneret temperature is 330℃;
[0161] S3, stretching the raw silk to obtain a vacuum insulation panel core material with a diameter of 12 μm;
[0162] The stretching is performed in three passes, with the first stretching temperature being 200° C., the second stretching temperature being 135° C., the third stretching temperature being 75° C., and the stretching ratio being 3.5:1.
[0163] Embodiment 13
[0164] A method for preparing a vacuum insulation panel core material, comprising the following steps:
[0165] S1, PET and 2.5wt% of nano filler (nano silicon dioxide, nano aluminum oxide) and 0.5wt% of polyethylene oxide are uniformly mixed to obtain a mixed raw material;
[0166] The weight ratio of nano silicon dioxide to nano aluminum oxide is 1:5;
[0167] S2, melting the mixed raw material in a co-rotating twin-screw extruder with a length-to-diameter ratio of 40:1, and then transferring the mixed raw material from a melt pump to a spinneret for melt spinning, and then water cooling to obtain raw yarn;
[0168] The twin-screw extruder adopts four-zone heating, wherein the heating temperature of the first zone is 280°C, the heating temperature of the second zone is 290°C, the heating temperature of the third zone is 310°C, the heating temperature of the fourth zone is 320°C, the screw speed is 180rpm; the apparent shear velocity of the spinning nozzle wall is 350s -1 , spinneret temperature is 330℃;
[0169] S3, stretching the raw silk to obtain a vacuum insulation panel core material with a diameter of 4 μm;
[0170] The stretching is performed in three passes, with the first stretching temperature being 200° C., the second stretching temperature being 135° C., the third stretching temperature being 75° C., and the stretching ratio being 3.5:1.
[0171] Embodiment 14
[0172] A method for preparing a vacuum insulation panel core material, comprising the following steps:
[0173] S1, PET and 2.5wt% of nano filler (nano silicon dioxide, nano aluminum oxide) and 0.5wt% of polyethylene oxide are uniformly mixed to obtain a mixed raw material;
[0174] The weight ratio of nano silicon dioxide to nano aluminum oxide is 1:5;
[0175] S2, melting the mixed raw material in a co-rotating twin-screw extruder with a length-to-diameter ratio of 40:1, and then transferring the mixed raw material from a melt pump to a spinneret for melt spinning, and then water cooling to obtain raw yarn;
[0176] The twin-screw extruder adopts four-zone heating, wherein the heating temperature of the first zone is 280°C, the heating temperature of the second zone is 290°C, the heating temperature of the third zone is 310°C, the heating temperature of the fourth zone is 320°C, the screw speed is 180rpm; the apparent shear velocity of the spinning nozzle wall is 350s -1 , spinneret temperature is 330℃;
[0177] S3, stretching the raw silk to obtain a vacuum insulation panel core material with a diameter of 6 μm;
[0178] The stretching is performed in three passes, with the first stretching temperature being 200° C., the second stretching temperature being 135° C., the third stretching temperature being 75° C., and the stretching ratio being 3.5:1.
[0179] Embodiment 15
[0180] A method for preparing a vacuum insulation panel core material, comprising the following steps:
[0181] S1, PET and 2.5wt% of nano filler (nano silicon dioxide, nano aluminum oxide) and 0.5wt% of polyethylene oxide are uniformly mixed to obtain a mixed raw material;
[0182] The weight ratio of nano silicon dioxide to nano aluminum oxide is 1:5;
[0183] S2, melting the mixed raw material in a co-rotating twin-screw extruder with a length-to-diameter ratio of 40:1, and then transferring the mixed raw material from a melt pump to a spinneret for melt spinning, and then water cooling to obtain raw yarn;
[0184] The twin-screw extruder adopts four-zone heating, wherein the heating temperature of the first zone is 280°C, the heating temperature of the second zone is 290°C, the heating temperature of the third zone is 310°C, the heating temperature of the fourth zone is 320°C, the screw speed is 180rpm; the apparent shear velocity of the spinning nozzle wall is 350s -1 , spinneret temperature is 330℃;
[0185] S3, stretching the raw silk to obtain a vacuum insulation panel core material with a diameter of 8 μm;
[0186] The stretching is performed in three passes, with the first stretching temperature being 200° C., the second stretching temperature being 135° C., the third stretching temperature being 75° C., and the stretching ratio being 3.5:1.
[0187] Example 16
[0188] A method for preparing a vacuum insulation panel core material, comprising the following steps:
[0189] S1, PET and 2.5wt% of nano filler (nano silicon dioxide, nano aluminum oxide) and 0.5wt% of polyethylene oxide are uniformly mixed to obtain a mixed raw material;
[0190] The weight ratio of nano silicon dioxide to nano aluminum oxide is 1:5;
[0191] S2, melting the mixed raw material in a co-rotating twin-screw extruder with a length-to-diameter ratio of 40:1, and then transferring the mixed raw material from a melt pump to a spinneret for melt spinning, and then water cooling to obtain raw yarn;
[0192] The twin-screw extruder adopts four-zone heating, wherein the heating temperature of the first zone is 280°C, the heating temperature of the second zone is 290°C, the heating temperature of the third zone is 310°C, the heating temperature of the fourth zone is 320°C, the screw speed is 180rpm; the apparent shear velocity of the spinning nozzle wall is 350s -1 , spinneret temperature is 330℃;
[0193] S3, stretching the raw silk to obtain a vacuum insulation panel core material with a diameter of 10 μm;
[0194] The stretching is performed in three passes, with the first stretching temperature being 200° C., the second stretching temperature being 135° C., the third stretching temperature being 75° C., and the stretching ratio being 3.5:1.
[0195] Embodiment 17
[0196] A high-performance lightweight vacuum insulation panel, comprising a core board 2 prepared from the core material of Example 1, wherein the surface of the core board 2 is wrapped with a film material 1, and a getter 3 is arranged inside the core board 2; the film material 1 comprises a vacuum-evaporated aluminum BOPP film 11, a TPEE film 12, an EVAL film 13 and a TPV aluminum-plated film 14, the outer surface of the vacuum-evaporated aluminum BOPP film 11 is bonded to the TPEE film 12 by polyurethane glue, the outer surface of the TPEE film 12 is bonded to the EVAL film 13 by polyurethane glue, and the outer surface of the EVAL film 13 is bonded to the TPV aluminum-plated film 14 by polyurethane glue;
[0197] The thickness of the TPEE film 12 is 5 μm;
[0198] The thickness of the EVAL film 13 is 5 μm.
[0199] Embodiment 18
[0200] A high-performance lightweight vacuum insulation panel, comprising a core board 2 prepared from the core material of Example 1, wherein the surface of the core board 2 is wrapped with a film material 1, and a getter 3 is arranged inside the core board 2; the film material 1 comprises a vacuum-evaporated aluminum BOPP film 11, a TPEE film 12, an EVAL film 13 and a TPV aluminum-plated film 14, the outer surface of the vacuum-evaporated aluminum BOPP film 11 is bonded to the TPEE film 12 by polyurethane glue, the outer surface of the TPEE film 12 is bonded to the EVAL film 13 by polyurethane glue, and the outer surface of the EVAL film 13 is bonded to the TPV aluminum-plated film 14 by polyurethane glue;
[0201] The thickness of the TPEE film 12 is 20 μm.
[0202] The thickness of the EVAL film 13 is 15 μm.
[0203] The principles and implementation methods of the present invention are described in this article using specific examples. The description of the above embodiments is only used to help understand the method and core idea of the present invention. At the same time, for those skilled in the art, according to the idea of the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. A method for preparing a vacuum insulation panel core material, characterized in that: The following steps are involved: S1, mixing PET with nano silicon dioxide, nano aluminum oxide and polyethylene oxide to obtain a mixed raw material; S2, melting the mixed raw material in a twin-screw extruder, then transferring it from a melt pump to a spinneret for melt spinning, and then cooling it to obtain a raw fiber; S3, stretching the raw silk to obtain a vacuum insulation board core material.
2. The method for preparing a vacuum insulation panel core material according to claim 1, characterized in that: The addition amount of the nano silicon dioxide and nano aluminum oxide is 0.1wt% to 5wt% of PET.
3. The method for preparing a vacuum insulation panel core material according to claim 2, characterized in that: The addition amount of the nano silicon dioxide and nano aluminum oxide is 1wt% to 3wt% of the PET.
4. The method for preparing a vacuum insulation panel core material according to claim 1, characterized in that: The weight ratio of the nano silicon dioxide to the nano aluminum oxide is (1-2):(4-5).
5. The method for preparing a vacuum insulation panel core material according to claim 1, characterized in that: The added amount of the polyethylene oxide is 0.1 wt% to 1 wt% of PET.
6. The method for preparing a vacuum insulation panel core material according to claim 1, characterized in that: The twin-screw extruder adopts four-zone heating, wherein the heating temperature of the first zone is 280°C to 290°C, the heating temperature of the second zone is 290°C to 300°C, the heating temperature of the third zone is 300°C to 310°C, and the heating temperature of the fourth zone is 310°C to 320°C.
7. The method for preparing a vacuum insulation panel core material according to claim 1, characterized in that: The apparent shear velocity of the spinning nozzle wall is 250-400s -1 , the spinneret temperature is 320℃~350℃.
8. The method for preparing a vacuum insulation panel core material according to claim 1, characterized in that: The stretching is carried out in three passes, the first stretching temperature is 180-230°C, the second stretching temperature is 100-150°C, the third stretching temperature is 50-100°C, and the stretching ratio is (1-10):
1.
9. A vacuum insulation panel core material, characterized in that: Prepared by the method according to any one of claims 1 to 8.
10. The vacuum insulation panel core material according to claim 9 is used to prepare a high-performance lightweight vacuum insulation panel.