Graphene composite hydrogel as well as preparation method and application thereof
By adding potassium ferrate to the preparation of graphene composite hydrogel and optimizing the raw material ratio, the problem of conductivity reduction caused by lignin sulfonate is solved, the degree of graphitization and conductivity are improved, and it is suitable for flexible supercapacitor electrode materials. .
Patent Information
- Application Number
- CN202411052111.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
AI Technical Summary
In the prior art, when improving the porous mesh structure of graphene hydrogels, the addition of lignin sulfonate will lead to a decrease in the degree of graphitization and conductivity, affecting its electrochemical properties as an electrode material.
During the preparation of graphene composite hydrogel, potassium ferrate is added, and the addition order and mass ratio of raw materials are optimized. A three-dimensional porous composite hydrogel is formed through hydrothermal reaction to improve the degree of graphitization and conductivity.
It is achieved to improve the degree of graphitization and conductivity on the basis of maintaining electrochemical properties, enhance the performance of flexible supercapacitor electrodes, simplify the preparation process and reduce costs.
Smart Images

Figure CN118978153A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of graphene hydrogels, and specifically relates to a graphene composite hydrogel and a preparation method and application thereof. Background Art
[0002] Graphene has unique electrical, thermal and mechanical properties. It can not only self-assemble into graphene hydrogels with excellent electrochemical properties, but also be compounded with small molecules or polymers to prepare multifunctional composite hydrogels. As an electrode material, graphene hydrogels can increase the electron transfer rate during the charge and discharge process, and can also maintain a high capacitance retention rate after multiple charge and discharge cycles, showing excellent cycle stability. In addition, graphene hydrogels are highly controllable as electrode materials, making them widely used in various energy storage devices, sensors, photocatalysis, electronics and health monitoring.
[0003] At present, in order to improve the porous network structure of graphene hydrogel, lignin sulfonate containing a variety of oxygen-containing functional groups is often used to modify graphene hydrogel to obtain lignin sulfonate / graphene composite hydrogel. Although this method can effectively improve the porous structure of electrode materials, the addition of lignin sulfonate will reduce the degree of graphitization and conductivity, thereby affecting the electrochemical performance of graphene composite hydrogel as an electrode material. Summary of the invention
[0004] The purpose of the present invention is to provide a graphene composite hydrogel and a preparation method and application thereof. In the preparation process of lignin sulfonate / graphene composite hydrogel, potassium ferrate is added, and the addition sequence and mass ratio of raw materials are optimized to obtain a dispersion. After a hydrothermal reaction, the raw materials are self-assembled into a three-dimensional porous composite hydrogel, the degree of graphitization and conductivity are improved, and the composite hydrogel has great potential in the preparation of electrodes for flexible supercapacitors.
[0005] In order to achieve the above object, the present invention is implemented through the following technical solutions:
[0006] In the first aspect, an embodiment of the present invention provides a method for preparing a graphene composite hydrogel, wherein a lignin sulfonate aqueous solution, a graphene oxide aqueous solution and a potassium ferrate aqueous solution are mixed to obtain a dispersion, a hydrothermal reaction is performed, and the graphene composite hydrogel is obtained by washing. The carbon content of the lignin sulfonate is 45-47%; and the methoxy content of the lignin sulfonate is 5-7%.
[0007] In some other embodiments, the lignin sulfonate is sodium lignin sulfonate or ammonium lignin sulfonate;
[0008] The purity of the lignin sulfonate is 90-95%;
[0009] The molecular weight of the lignin sulfonate is 2000 to 4000;
[0010] The concentration of the lignin sulfonate aqueous solution is 50-60 mg / mL.
[0011] In some other embodiments, the concentration of the graphene oxide aqueous solution is 5.64 to 5.88 mg / mL;
[0012] The graphene oxide sheet has a thickness of 0.335 to 1.675 nm;
[0013] The particle size of the graphene oxide is 0.20 to 0.55 μm;
[0014] The graphene oxide is Hummers method, improved Hummers synthesis or commercially available graphene oxide.
[0015] In some other embodiments, the concentration of the potassium ferrate aqueous solution is 50-60 mg / mL; the purity of the potassium ferrate is 95-98%.
[0016] In some other embodiments, the mixing volume ratio of the graphene oxide aqueous solution: the lignin sulfonate aqueous solution: the potassium ferrate aqueous solution is 1: (0.059-0.12): (0.012-0.059);
[0017] The mixing is 300-400W ultrasonic dispersion for 10-20min;
[0018] In some other embodiments, the temperature of the hydrothermal reaction is 175-195° C., the hydrothermal treatment time is 9-12 h, or the volume ratio of the dispersion to the reactor in the hydrothermal reaction is (0.1-0.6):1.
[0019] In some other embodiments, the washing is performed using deionized water at 40-60°C.
[0020] In some other embodiments, the order of mixing the lignin sulfonate aqueous solution, the graphene oxide aqueous solution and the potassium ferrate aqueous solution is: adding the lignin sulfonate aqueous solution to the graphene oxide aqueous solution to form solution a; adding the potassium ferrate aqueous solution to solution a, and obtaining a dispersion after ultrasonic dispersion.
[0021] In a second aspect, an embodiment of the present invention provides a graphene composite hydrogel obtained by the preparation method described in the first aspect.
[0022] In a third aspect, an embodiment of the present invention provides an application of the graphene composite hydrogel described in the second aspect in an electrode material.
[0023] The beneficial effects of the above embodiments of the present invention are as follows:
[0024] (1) The graphene oxide used in the present invention has a large number of oxygen-containing functional groups, such as hydroxyl and carboxyl groups, and is a hydrophilic substance; the addition of lignin sulfonate can improve the dispersibility and surface properties of graphene oxide and increase its interlayer spacing; potassium ferrate is a green and mild activator, and adding it to the solution formed by the lignin sulfonate aqueous solution and the graphene oxide aqueous solution is beneficial to activate and improve the graphitization degree of graphene oxide.
[0025] (2) The present invention obtains a dispersion by regulating the concentration and mixing volume ratio of a lignin sulfonate aqueous solution, a graphene oxide aqueous solution and a potassium ferrate aqueous solution. After a hydrothermal reaction, the raw materials self-assemble into a three-dimensional porous composite hydrogel, thereby improving the degree of graphitization and electrical conductivity.
[0026] (3) The method of the present invention is simple and easy to operate. The prepared graphene composite hydrogel has a high degree of graphitization and is an electrode material with good electrochemical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0028] Figure 1 The SEM images of the composite hydrogels prepared in Comparative Example 1 and Example 1 of the present invention, wherein: Figure 1 (a) is Comparative Example 1, Figure 1 (b) Example 1 except that potassium ferrate was added. DETAILED DESCRIPTION
[0029] An embodiment of the present invention provides a method for preparing a graphene composite hydrogel, comprising mixing a lignin sulfonate aqueous solution, a graphene oxide aqueous solution and a potassium ferrate aqueous solution to obtain a dispersion, performing a hydrothermal reaction, and washing to obtain the graphene composite hydrogel; wherein the carbon content of the lignin sulfonate is 45-47%; and the methoxy content of the lignin sulfonate is 5-7%.
[0030] In some other embodiments, the lignin sulfonate is sodium lignin sulfonate or ammonium lignin sulfonate;
[0031] The purity of the lignin sulfonate is 90-95%;
[0032] The molecular weight of the lignin sulfonate is 2000 to 4000;
[0033] The concentration of the lignin sulfonate aqueous solution is 50-60 mg / mL.
[0034] In some other embodiments, the concentration of the graphene oxide aqueous solution is 5.64 to 5.88 mg / mL;
[0035] The graphene oxide sheet has a thickness of 0.335 to 1.675 nm;
[0036] The particle size of the graphene oxide is 0.20 to 0.55 μm;
[0037] The graphene oxide is Hummers method, improved Hummers synthesis or commercially available graphene oxide.
[0038] In some other embodiments, the concentration of the potassium ferrate aqueous solution is 50-60 mg / mL; the purity of the potassium ferrate is 95-98%.
[0039] In some other embodiments, the mixing volume ratio of the graphene oxide aqueous solution: the lignin sulfonate aqueous solution: the potassium ferrate aqueous solution is 1: (0.059-0.12): (0.012-0.059);
[0040] The mixing is 300-400W ultrasonic dispersion for 10-20min;
[0041] In some other embodiments, the temperature of the hydrothermal reaction is 175-195° C., the hydrothermal treatment time is 9-12 h, or the volume ratio of the dispersion to the reactor in the hydrothermal reaction is (0.1-0.6):1.
[0042] In some other embodiments, the washing is performed using deionized water at 40-60° C., which is beneficial for ensuring the integrity of the hydrogel structure and making it easier to fully clean the hydrogel.
[0043] In some other embodiments, the order of mixing the lignin sulfonate aqueous solution, the graphene oxide aqueous solution and the potassium ferrate aqueous solution is: adding the lignin sulfonate aqueous solution to the graphene oxide aqueous solution to form solution a; adding the potassium ferrate aqueous solution to solution a, and obtaining a dispersion after ultrasonic dispersion.
[0044] The preparation method of the present invention is simple to operate, and the raw materials used are cheap and easy to obtain. The potassium ferrate added therein is a green and mild activator, which is conducive to activating and improving the graphitization degree of graphene oxide. Graphene oxide has a large number of oxygen-containing functional groups, such as hydroxyl and carboxyl groups, and it is a hydrophilic substance. As a natural polymer anionic surfactant, lignin sulfonate has the characteristics of abundant sources, low price, renewable, and degradable, and is often used as a dispersant. The carbon content and methoxy content in lignin sulfonate can improve the surface properties of graphene oxide, increase its interlayer spacing, and improve the dispersion performance of graphene. Through hydrothermal reaction, the raw materials self-assemble into a three-dimensional porous composite hydrogel to improve the graphitization degree and conductivity.
[0045] During the experiment, the inventors found that the carbon content and methoxy content of lignin sulfonate can affect the electrical conductivity and mechanical properties of the hydrogel, and can also adjust the swelling and release properties of the hydrogel. Potassium ferrate (K2FeO4) decomposes to generate KOH and Fe(OH)3 during the hydrothermal process. Under certain temperature and pressure, the potassium compound generated by KOH can etch the carbon material to form carbon dioxide and carbon monoxide gas, thereby causing the material to produce a porous structure. Fe(OH)3 reacts with the carbon material to generate iron particles. These iron particles act as catalysts to catalyze the conversion of amorphous carbon into graphitized carbon, thereby increasing the degree of graphitization of the material and further improving the crystallinity and conductivity of the carbon material.
[0046] The graphene composite hydrogel obtained by the preparation method of the present invention is used in electrode materials. The graphene composite hydrogel is used as a self-supporting electrode material, 0.1M HClO4 is used as an electrolyte, and a supercapacitor is assembled to perform electrochemical testing in an electrochemical workstation.
[0047] Example 1
[0048] (1) Prepare a 50 mg / mL sodium lignin sulfonate aqueous solution, a 5.88 mg / mL graphite oxide solution, and a 60 mg / mL potassium ferrate aqueous solution, wherein the sodium lignin sulfonate has a purity of 90%, a molecular weight of 2000, a carbon content of 45%, and a methoxy content of 7%; graphene oxide is prepared by the Hummers method, with a sheet thickness of 1.005 nm and a particle size of 0.55 μm; and the purity of potassium ferrate is 95%.
[0049] (2) adding a sodium lignin sulfonate aqueous solution to a graphene oxide aqueous solution to form a solution a, and adding a potassium ferrate aqueous solution to a solution, and mixing to form a dispersion, wherein the volume ratio of the sodium lignin sulfonate aqueous solution: the graphene oxide aqueous solution: the potassium ferrate aqueous solution is 0.059:1:0.012.
[0050] (3) After the dispersion was dispersed in an ultrasonic cleaner with a power of 300 W for 20 min, it was transferred to a high-pressure reactor and reacted at 195° C. for 12 h. The volume ratio of the dispersion to the high-pressure reactor was 0.4:1. After the hydrothermal reaction was completed, it was cooled to room temperature and washed with deionized water at 60° C. to obtain a graphene composite hydrogel.
[0051] Example 2
[0052] (1) Prepare a 55 mg / mL aqueous solution of ammonium lignin sulfonate, a 5.64 mg / mL graphite oxide solution, and a 60 mg / mL potassium ferrate aqueous solution, respectively. The purity of ammonium lignin sulfonate is 92%, the molecular weight is 4000, the concentration is 55 mg / mL, the carbon content is 45%, and the methoxy content is 6%; graphene oxide is prepared by an improved Hummers method (the prior art, refer to the improved Hummers method for preparing graphene oxide and its mechanism analysis, Plastic Industry, 2018, 46 (01)) with a sheet thickness of 1.675 nm and a particle size of 0.28 μm; the purity of potassium ferrate is 98%.
[0053] (2) adding an ammonium lignin sulfonate aqueous solution to an aqueous graphene oxide solution to form a solution a, and adding an aqueous potassium ferrate solution to the solution a, and mixing them to form a dispersion, wherein the volume ratio of the ammonium lignin sulfonate aqueous solution: the graphene oxide aqueous solution: the potassium ferrate aqueous solution is 0.12:1:0.012.
[0054] (3) After the dispersion was dispersed in an ultrasonic cleaner with a power of 400 W for 15 min, it was transferred to a high-pressure reactor and reacted at 175° C. for 9 h. The volume ratio of the dispersion to the high-pressure reactor was 0.6:1. After the hydrothermal reaction was completed, it was cooled to room temperature and washed with deionized water at 40° C. to obtain a graphene composite hydrogel.
[0055] Example 3
[0056] (1) Prepare a sodium lignin sulfonate aqueous solution with a concentration of 55 mg / mL, a graphite oxide solution with a concentration of 5.64 mg / mL, and a potassium ferrate aqueous solution with a concentration of 55 mg / mL. The sodium lignin sulfonate has a purity of 95%, a molecular weight of 3500, a carbon content of 46%, and a methoxy content of 6%. The graphene oxide uses commercially available graphene oxide (graphene oxide produced by Chengdu Organic Chemistry Co., Ltd., Chinese Academy of Sciences), has a sheet thickness of 0.335 nm, and a particle size of 0.20 μm. The purity of potassium ferrate is 95%.
[0057] (2) adding the sodium lignin sulfonate aqueous solution to the graphene oxide aqueous solution to form solution a, and adding the potassium ferrate aqueous solution to the solution a, and mixing them to form a dispersion, wherein the volume ratio of the ammonium lignin sulfonate aqueous solution: the graphene oxide aqueous solution: the potassium ferrate aqueous solution is 0.059:1:0.012.
[0058] (3) After the dispersion was dispersed in an ultrasonic cleaner with a power of 350 W for 15 min, it was transferred to a high-pressure reactor and reacted at 195° C. for 10 h. The volume ratio of the dispersion to the high-pressure reactor was 0.4:1. After the hydrothermal reaction was completed, it was cooled to room temperature and washed with deionized water at 60° C. to obtain a graphene composite hydrogel.
[0059] Comparative Example 1
[0060] The difference from Example 1 is that the potassium ferrate aqueous solution with a concentration of 60 mg / mL in Example 1 is replaced by deionized water. The other processes are exactly the same as those in Example 1, and the specific preparation process is as follows:
[0061] (1) A sodium lignin sulfonate aqueous solution with a concentration of 50 mg / mL and a graphite oxide solution with a concentration of 5.88 mg / mL were prepared respectively. The purity of the sodium lignin sulfonate was 90%, the molecular weight was 2000, the carbon content was 45%, and the methoxy content was 7%; graphene oxide was prepared by the Hummers method, and the sheet thickness was 1.005 nm and the particle size was 0.55 μm.
[0062] (2) adding the sodium lignin sulfonate aqueous solution to the graphene oxide aqueous solution to form solution a, adding deionized water to solution a, and mixing to form a dispersion, wherein the volume ratio of the sodium lignin sulfonate aqueous solution: the graphene oxide aqueous solution: the deionized water is 0.059:1:0.012.
[0063] (3) After the dispersion was dispersed in an ultrasonic cleaner with a power of 300 W for 20 min, it was transferred to a high-pressure reactor and reacted at 195° C. for 12 h. The volume ratio of the dispersion to the high-pressure reactor was 0.4:1. After the hydrothermal reaction was completed, it was cooled to room temperature and washed with deionized water at 60° C. to obtain a graphene composite hydrogel.
[0064] Figure 1 The SEM images of the composite hydrogels prepared in Example 1 and Comparative Example 1 show that, compared with Comparative Example 1, Example 1 exhibits a more porous structure, and the increase in the void structure is attributed to the decomposition of potassium ferrate (K2FeO4) to generate KOH and Fe(OH)3 during the hydrothermal process. Under a certain temperature and pressure, the potassium compound generated by KOH can etch the carbon material to form carbon dioxide and carbon monoxide gases, thereby causing the material to produce a porous structure.
[0065] Comparative Example 2
[0066] The difference from Example 1 is that the potassium ferrate aqueous solution is added to the graphene oxide aqueous solution to form solution a, and the sodium lignin sulfonate aqueous solution is added to solution a, and mixed to form a dispersion. The other processes are exactly the same as those in Example 1, and the specific preparation process is as follows:
[0067] (1) Prepare a sodium lignin sulfonate aqueous solution with a concentration of 50 mg / mL, a graphite oxide solution with a concentration of 5.88 mg / mL, and a potassium ferrate aqueous solution with a concentration of 60 mg / mL. The sodium lignin sulfonate has a purity of 90%, a molecular weight of 2000, a carbon content of 45%, and a methoxy content of 7%; the graphite oxide is prepared by the Hummers method, with a sheet thickness of 1.005 nm and a particle size of 0.55 μm; and the purity of potassium ferrate is 95%.
[0068] (2) adding potassium ferrate aqueous solution to graphene oxide aqueous solution to form solution a, adding sodium lignin sulfonate aqueous solution to solution a, and mixing to form a dispersion, wherein the volume ratio of sodium lignin sulfonate aqueous solution: graphene oxide aqueous solution: potassium ferrate aqueous solution is 0.059:1:0.012.
[0069] (3) After the dispersion was dispersed in an ultrasonic cleaner with a power of 300 W for 20 min, it was transferred to a high-pressure reactor and reacted at 195° C. for 12 h. The volume ratio of the dispersion to the high-pressure reactor was 0.4:1. After the hydrothermal reaction was completed, it was cooled to room temperature and washed with deionized water at 60° C. to obtain a graphene composite hydrogel.
[0070] Comparative Example 3
[0071] The difference from Example 2 is that the potassium ferrate aqueous solution with a concentration of 60 mg / mL in Example 2 is replaced by deionized water. The other processes are exactly the same as those in Example 2, and the specific preparation process is as follows:
[0072] (1) Prepare a 55 mg / mL aqueous solution of ammonium lignin sulfonate and a 5.64 mg / mL graphite oxide solution, wherein the ammonium lignin sulfonate has a purity of 92%, a molecular weight of 4000, a concentration of 55 mg / mL, a carbon content of 45%, and a methoxy content of 6%; the graphite oxide is prepared by an improved Hummers method, with a sheet thickness of 1.675 nm and a particle size of 0.28 μm.
[0073] (2) adding an aqueous solution of ammonium lignin sulfonate to an aqueous solution of graphene oxide to form a solution a, and adding deionized water to the solution a, and mixing them to form a dispersion, wherein the volume ratio of the aqueous solution of ammonium lignin sulfonate: the aqueous solution of graphene oxide: the deionized water is 0.12:1:0.012.
[0074] (3) After the dispersion was dispersed in an ultrasonic cleaner with a power of 400 W for 15 min, it was transferred to a high-pressure reactor and reacted at 175° C. for 9 h. The volume ratio of the dispersion to the high-pressure reactor was 0.6:1. After the hydrothermal reaction was completed, it was cooled to room temperature and washed with deionized water at 40° C. to obtain a graphene composite hydrogel.
[0075] Comparative Example 4
[0076] The difference from Example 2 is that the potassium ferrate aqueous solution is added to the graphene oxide aqueous solution to form solution a, and the ammonium lignin sulfonate aqueous solution is added to solution a to form a dispersion after mixing. The other processes are exactly the same as those in Example 2, and the specific preparation process is as follows:
[0077] (1) Prepare a 55 mg / mL aqueous solution of ammonium lignin sulfonate, a 5.64 mg / mL graphite oxide solution, and a 60 mg / mL aqueous solution of potassium ferrate, respectively. The purity of ammonium lignin sulfonate is 92%, the molecular weight is 4000, the concentration is 55 mg / mL, the carbon content is 45%, and the methoxy content is 6%. The graphene oxide is prepared by the improved Hummers method, with a sheet thickness of 1.675 nm and a particle size of 0.28 μm. The purity of potassium ferrate is 98%.
[0078] (2) adding potassium ferrate aqueous solution to graphene oxide aqueous solution to form solution a, adding ammonium lignin sulfonate aqueous solution to solution a, and mixing to form a dispersion, wherein the volume ratio of ammonium lignin sulfonate aqueous solution: graphene oxide aqueous solution: potassium ferrate aqueous solution is 0.12:1:0.012.
[0079] (3) After the dispersion was dispersed in an ultrasonic cleaner with a power of 400 W for 15 min, it was transferred to a high-pressure reactor and reacted at 175° C. for 9 h. The volume ratio of the dispersion to the high-pressure reactor was 0.6:1. After the hydrothermal reaction was completed, it was cooled to room temperature and washed with deionized water at 40° C. to obtain a graphene composite hydrogel.
[0080] Comparative Example 5
[0081] The difference from Example 3 is that the potassium ferrate aqueous solution with a concentration of 55 mg / mL in Example 3 is replaced by deionized water. The other processes are exactly the same as those in Example 3, and the specific preparation process is as follows:
[0082] (1) A sodium lignin sulfonate aqueous solution with a concentration of 55 mg / mL and a graphite oxide solution with a concentration of 5.64 mg / mL were prepared respectively. The sodium lignin sulfonate had a purity of 95%, a molecular weight of 3500, a carbon content of 46%, and a methoxy content of 6%. The graphene oxide used was commercially available graphene oxide with a sheet thickness of 0.335 nm and a particle size of 0.20 μm.
[0083] (2) adding the sodium lignin sulfonate aqueous solution to the graphene oxide aqueous solution to form solution a, and adding deionized water to solution a, and mixing to form a dispersion, wherein the volume ratio of the ammonium lignin sulfonate aqueous solution: the graphene oxide aqueous solution: the deionized water is 0.059:1:0.012.
[0084] (3) After the dispersion was dispersed in an ultrasonic cleaner with a power of 350 W for 15 min, it was transferred to a high-pressure reactor and reacted at 195° C. for 10 h. The volume ratio of the dispersion to the high-pressure reactor was 0.4:1. After the hydrothermal reaction was completed, it was cooled to room temperature and washed with deionized water at 60° C. to obtain a graphene composite hydrogel.
[0085] Comparative Example 6
[0086] The difference from Example 3 is that the potassium ferrate aqueous solution is added to the graphene oxide aqueous solution to form solution a, and the sodium lignin sulfonate aqueous solution is added to solution a to form a dispersion after mixing. The other processes are exactly the same as those in Example 3, and the specific preparation process is as follows:
[0087] (1) Prepare a sodium lignin sulfonate aqueous solution with a concentration of 55 mg / mL, a graphite oxide solution with a concentration of 5.64 mg / mL, and a potassium ferrate aqueous solution with a concentration of 55 mg / mL. The sodium lignin sulfonate has a purity of 95%, a molecular weight of 3500, a carbon content of 46%, and a methoxy content of 6%; the graphite oxide uses commercially available graphene oxide with a sheet thickness of 0.335 nm and a particle size of 0.20 μm; and the purity of potassium ferrate is 95%.
[0088] (2) adding potassium ferrate aqueous solution to graphene oxide aqueous solution to form solution a, adding sodium lignin sulfonate aqueous solution to solution a, and mixing to form a dispersion, wherein the volume ratio of ammonium lignin sulfonate aqueous solution: graphene oxide aqueous solution: potassium ferrate aqueous solution is 0.059:1:0.012.
[0089] (3) After the dispersion was dispersed in an ultrasonic cleaner with a power of 350 W for 15 min, it was transferred to a high-pressure reactor and reacted at 195° C. for 10 h. The volume ratio of the dispersion to the high-pressure reactor was 0.4:1. After the hydrothermal reaction was completed, it was cooled to room temperature and washed with deionized water at 60° C. to obtain a graphene composite hydrogel.
[0090] Performance Testing:
[0091] The graphene composite hydrogels prepared in Examples 1 to 3 and Comparative Examples 1 to 6 were used as self-supporting electrode materials, and 0.1 M HClO4 was used as the electrolyte. They were assembled into supercapacitors and electrochemically tested on an electrochemical workstation. The constant current charge and discharge (GCD) test was performed at 1 mA / cm 2 The current density is 0.1V and the test voltage window is 0-1V. The area specific capacitance calculation formula is C A =2I d / [(ΔV / Δt)A], where C A (mFcm -2 ), I d (mA), Δt (s), ΔV (V) and A (cm 2 ) represent the area specific capacitance, discharge current, discharge time, discharge voltage window and the area of a single electrode respectively. The test results are shown in Table 1.
[0092] The graphene composite hydrogels prepared in Examples 1 to 3 and Comparative Examples 1 to 6 were freeze-dried (-60° C., 2 d) and then subjected to Raman spectroscopy (scanning wavelength of 532 nm). D / I G The degree of graphitization was verified and the test results are shown in Table 1.
[0093] Table 1 Specific capacitance and graphitization degree of graphene composite hydrogel
[0094] <![CDATA[Specific capacitance (mF / cm 2 )]]> <![CDATA[Graphitization degree (I D / I G )]]> Example 1 136 0.849 Example 2 126.5 0.856 Example 3 147 0.807 Comparative Example 1 108 0.955 Comparative Example 2 126 0.884 Comparative Example 3 98 0.967 Comparative Example 4 118 0.932 Comparative Example 5 102 0.959 Comparative Example 6 129 0.871
[0095] Lignin sulfonates containing a variety of oxygen-containing functional groups can modify graphene hydrogels, but excessive addition will reduce the conductivity of the resulting hydrogel electrode material. Potassium ferrate has activation and graphitization effects, but due to its large mass, the hydrogel has a limited loading capacity for it, so both drugs must be added within a certain mass range. Compared with hydrogel electrode materials without potassium ferrate added, since potassium ferrate plays both activation and graphitization roles, adding it to the composite hydrogel electrode material improves the specific capacitance, and the order of adding potassium ferrate aqueous solution directly affects the multi-level pore structure and quantity of the hydrogel electrode material, further improving the specific capacitance and graphitization degree of the composite hydrogel.
[0096] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a graphene composite hydrogel, characterized in that: A lignin sulfonate aqueous solution, a graphene oxide aqueous solution and a potassium ferrate aqueous solution are mixed to obtain a dispersion, and a hydrothermal reaction is carried out. The graphene composite hydrogel is obtained by washing. The carbon content of the lignin sulfonate is 45-47%; and the methoxy content of the lignin sulfonate is 5-7%.
2. The preparation method according to claim 1, characterized in that The lignin sulfonate is sodium lignin sulfonate or ammonium lignin sulfonate; The purity of the lignin sulfonate is 90-95%; The molecular weight of the lignin sulfonate is 2000 to 4000; The concentration of the lignin sulfonate aqueous solution is 50-60 mg / mL.
3. The preparation method according to claim 1, characterized in that: The concentration of the graphene oxide aqueous solution is 5.64-5.88 mg / mL; The graphene oxide sheet has a thickness of 0.335 to 1.675 nm; The particle size of the graphene oxide is 0.20 to 0.55 μm; The graphene oxide is Hummers method, improved Hummers synthesis or commercially available graphene oxide.
4. The preparation method according to claim 1, characterized in that: The concentration of the potassium ferrate aqueous solution is 50-60 mg / mL; the purity of the potassium ferrate is 95-98%.
5. The preparation method according to claim 1, characterized in that: The mixing volume ratio of the graphene oxide aqueous solution: the lignin sulfonate aqueous solution: the potassium ferrate aqueous solution is 1: (0.059-0.12): (0.012-0.059); The mixing is performed by ultrasonic dispersion at 300-400W for 10-20min.
6. The preparation method according to claim 1, characterized in that: The temperature of the hydrothermal reaction is 175-195°C, and the hydrothermal treatment time is 9-12h; Alternatively, the volume ratio of the dispersion to the reactor in the hydrothermal reaction is (0.1-0.6):
1.
7. The preparation method according to claim 1, characterized in that: The washing is performed using deionized water at 40-60°C.
8. The preparation method according to claim 1, characterized in that: The order of mixing the lignin sulfonate aqueous solution, the graphene oxide aqueous solution and the potassium ferrate aqueous solution is: adding the lignin sulfonate aqueous solution to the graphene oxide aqueous solution to form solution a; adding the potassium ferrate aqueous solution to solution a, and obtaining a dispersion after ultrasonic dispersion.
9. A graphene composite hydrogel obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the graphene composite hydrogel according to claim 9 in electrode materials.
Citation Information
Patent Citations
Preparation of electroactive biomass-based conductive composite film and self-reinforced cellulose hydrogel and application thereof to wearable supercapacitor
CN110797204A
Sodium lignin sulfonate / graphene oxide composite material, preparation method and applications thereof
CN110975827A
Method for preparing thermal reduction graphene oxide film by blending sodium lignin sulfonate and graphene oxide
CN112062121A
Preparation method and application of oxygen-enriched layered porous graphene
CN114014306A
Preparation method and application of aerogel with three-dimensional porous vertical orientation network structure
CN114656797A
Cited By
Biomass / MXene composite aerogel as well as preparation method and application thereof
CN121401981A