Thermal insulation material as well as preparation method and application thereof

By adding nanocellulose to the automotive insulation materials, a microscopic multi-stage pore network structure is formed, which solves the problem of flammability and fracture of existing materials at high temperatures, and a thermal insulation material with high physical strength and flame retardant properties is achieved. Suitable for high temperature environments.

CN118978381APending Publication Date: 2024-11-19ZHONGQING FIBER COMPOSITE MATERIALS TECHNOLOGY (LANGFANG) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411069610.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing automotive thermal insulation materials are prone to combustion, flue gas, deformation or breaking in high temperature environments, resulting in a degradation of thermal insulation performance, and inorganic binders make the material hard and brittle and easy to break.

Method used

The thermal insulation materials including organic fibers, inorganic fibers, fillers, flame retardants, binders and nanocellulose are used to form a microscopic multi-stage pore network structure through vacuum dehydration and pressing to enhance mechanical strength and heat resistance.

Benefits of technology

It significantly improves the physical strength and flame retardant properties of the thermal insulation material, maintains the integrity of the form at a high temperature of 600℃, does not burn or produce smoke, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978381A_ABST
    Figure CN118978381A_ABST
Patent Text Reader

Abstract

The invention provides a thermal insulation material as well as a preparation method and application thereof, and relates to the technical field of porous materials. In the thermal insulation material provided by the invention, the inorganic fibers, the organic fibers and the filler form a first-stage network structure, the inorganic fibers are thin, long and stiff, the organic fibers are thin, long and soft, and the long fibers of the inorganic fibers and the organic fibers are distributed in a staggered manner to form a microscopic multi-stage pore network structure. The nano cellulose is added, so that the nano cellulose is filled between the inorganic fibers and the organic fibers, and a submicron microscopic multi-stage pore network structure is formed. The thermal insulation material provided by the invention is high in physical strength and good in heat resistance and flame retardance, adapts to complex geometrical shapes, does not burn, does not generate smoke, does not break or break after being treated at a high temperature (600 DEG C), keeps the original complete shape and form, and completely meets the mechanical and thermal property requirements of the thermal insulation material for the automobile engine and the exhaust manifold.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of porous materials, and in particular to a heat insulating material and a preparation method and application thereof. Background Art

[0002] Automotive heat shields are mainly installed on the outside of automobile engines and exhaust manifolds to isolate the heat radiation of the engine and exhaust manifold, protect other parts with lower temperature resistance in the engine compartment, and prevent rapid aging or ignition of plastic or rubber parts. Common structures of heat shields are single-layer structure and sandwich structure. Sandwich-type automotive heat shields are also called sandwich heat shields. They are composed of two layers of outer shell and one layer of filling material. The outer shell is generally made of metal plates, plastic plates, rubber plates and other materials, and the filling material is made of fibrous materials, foam plastics, rubber and other materials.

[0003] Cellulosic thermal insulation materials are generally made by papermaking, where mineral fibers, pulp fibers, fillers and additives (such as binders, flame retardants, etc.) are dispersed in water to form a uniform slurry, which is then filtered, squeezed and dried under vacuum. Mineral fibers have good heat resistance, but poor mutual bonding; inorganic binders easily make the material hard and brittle and break; organic binders will pyrolyze and lose their bonding effect at high temperatures; pulp fibers can increase the physical strength of the material, but due to their poor heat resistance, the thermal insulation material will burn, produce smoke, deform or even break and shatter in a high temperature environment (such as 600°C), thus affecting the thermal insulation performance.

[0004] Zhang Qiaoxin et al. (Zhang Qiaoxin, Fu Qiang. Preparation and performance research of new high-temperature composite insulation paper [J]. China Papermaking, 2008, 27 (7): 3.) prepared a thermal insulation paper without any organic components using aluminum silicate fiber, glass fiber, potassium hexatitanate whisker and homemade inorganic binder as the main components. When the amount of aluminum silicate fiber is 80% and the amount of glass fiber is 20%, the maximum tensile strength of the composite insulation paper (width is 15mm, thickness is 0.3mm) is 3.4N, and its tensile strength is equivalent to about 0.76MPa. However, the tensile strength of the composite insulation paper is low, and the inorganic raw materials used will make the composite insulation paper hard, brittle and easy to break. Summary of the invention

[0005] In view of this, the object of the present invention is to provide a thermal insulation material and a preparation method and application thereof. The thermal insulation material provided by the present invention has high physical strength, good heat resistance and flame retardancy.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The invention provides a heat-insulating material, wherein the raw materials for preparing the heat-insulating material include effective ingredients and water; in terms of mass percentage, the effective ingredients include 1-10% organic fiber, 1-80% inorganic fiber, 1-80% filler, 1-10% flame retardant, 1-10% binder and 0.5-5% nano cellulose.

[0008] Preferably, the organic fiber includes one or more of chemical coniferous wood pulp, chemical hardwood wood pulp, cotton pulp, straw pulp and aramid fiber.

[0009] Preferably, the inorganic fiber includes one or more of aluminum silicate fiber, magnesium silicate fiber, mineral fiber, glass fiber and ceramic fiber.

[0010] Preferably, the filler comprises one or more of kaolin, diatomaceous earth, wollastonite, ceramic powder and slag.

[0011] Preferably, the flame retardant includes one or more of aluminum hydroxide, magnesium hydroxide and borate.

[0012] Preferably, the binder includes one or more of water glass, silica sol, polyvinyl alcohol, sodium carboxymethyl cellulose, styrene-butadiene latex, styrene-acrylic latex and nitrile-butadiene latex.

[0013] Preferably, the nanocellulose has a diameter of less than 100 nm and a length of 0.1 to 100 μm.

[0014] The present invention provides a method for preparing the thermal insulation material described in the above technical solution, comprising the following steps: mixing the active ingredients with water, and sequentially performing dehydration, forming and drying to obtain the thermal insulation material.

[0015] Preferably, the dehydration forming comprises sequentially performing vacuum dehydration and pressing;

[0016] The vacuum degree of the vacuum dehydration is 0.01-0.06 MPa, and the time is 3-300 s;

[0017] The pressing pressure is 50-400 kPa and the pressing time is 10-300 s;

[0018] The drying temperature is 70-120° C. and the drying time is 10-1000 seconds.

[0019] The present invention provides application of the heat insulating material described in the above technical solution or the heat insulating material prepared by the preparation method described in the above technical solution in a heat insulating cover for a vehicle.

[0020] Inorganic fibers, organic fibers and fillers form a first-level network structure: inorganic fibers are slender and stiff, and organic fibers are slender and soft. The long fibers of these inorganic fibers and organic fibers are interlaced and distributed to form a microscopic multi-level pore network structure. Nanocellulose is a fiber aggregate with a diameter of <100nm and a length of nanometer to micrometer obtained by treating fibers by chemical, physical, biological or a combination of several means. Its surface contains a large number of hydroxyl groups, has excellent mechanical properties, huge specific surface area, high crystallinity, high transparency, low density, good biodegradability and biocompatibility. The present invention adds a small amount of nanocellulose so that the nanocellulose is filled between the above-mentioned inorganic fibers and organic fibers (surface and inside) to form a submicron-level microscopic multi-level pore network structure. In this porous structure, a large number of hydrogen bonds are formed between nanocellulose and organic fibers, between nanocellulose and inorganic fibers, and between nanocellulose itself. At the same time, a synergistic effect is generated between nanocellulose and the binder, which significantly improves the mechanical strength of the material. The present invention has found that nanocellulose can not only improve the physical strength of thermal insulation materials at room temperature, but also improve the physical strength of thermal insulation materials at high temperatures, and can keep the thermal insulation materials intact and avoid cracking and crushing. The basic chemical structure of nanocellulose is glucose units, which can still maintain good morphological integrity and strength of the material at 600°C, which is different from the application effect of nanocellulose in other industries. As shown in the test results of the embodiment, when 1% (1% of the mass of the slurry) of nanocellulose is used, the tensile strength of the thermal insulation material can be increased from 0.42MPa to 2.20MPa. After burning at 600°C, the thermal insulation material does not burn, does not produce smoke, and maintains its original shape. It shows that after adding nanocellulose, the amount of organic fiber in the thermal insulation material can be reduced, and the thermal insulation material still maintains a high physical strength and better thermal insulation and flame retardant properties, reducing the production cost of the thermal insulation material.

[0021] The preparation method of the heat insulating material provided by the invention has simple process, simple operation, low cost and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The state diagram of the thermal insulation materials prepared in Example 1 (right) and Comparative Example 1 (left) when placed in a 600° C. high-temperature furnace;

[0023] Figure 2 The morphology of the thermal insulation materials prepared in Example 1 (right) and Comparative Example 1 (left) after being placed at 600°C for 1 hour. DETAILED DESCRIPTION

[0024] The invention provides a heat-insulating material, the preparation raw materials of which include effective ingredients and water; in terms of mass percentage, the effective ingredients (dry weight) include 1-10% organic fiber, 1-80% inorganic fiber, 1-80% filler, 1-10% flame retardant, 1-10% binder and 0.5-5% nano cellulose.

[0025] Unless otherwise specified, the materials and equipment used in the present invention are all commercially available products in the art.

[0026] In the present invention, the mass of the active ingredient accounts for 0.5-5wt% of the total mass of the active ingredient and water, more preferably 1-4wt%, further preferably 2-3wt%, specifically preferably 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt% or 5wt%.

[0027] In the present invention, the effective ingredients include 1-10% by weight of organic fiber, preferably 2-9%, and specifically preferably 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5% or 10% by weight of dry weight of organic fiber. In the present invention, the organic fiber preferably includes one or more of chemical coniferous wood pulp, chemical broadleaf wood pulp, cotton pulp, straw pulp and aramid fiber; the length of the organic fiber is preferably 0.5-5 mm, more preferably 1-3 mm; the diameter of the organic fiber is preferably 0.1-50 μm, and the diameter of the aramid fiber is more preferably 1-10 μm; the diameter of the plant fiber in the chemical coniferous wood pulp, chemical broadleaf wood pulp, cotton pulp and straw pulp is more preferably 15-20 μm.

[0028] In the present invention, the effective ingredients include 1-80% of inorganic fibers, preferably 10-70%, and specifically preferably 1%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75% or 80% by mass percentage. In the present invention, the inorganic fibers preferably include one or more of aluminum silicate fibers, magnesium silicate fibers, mineral fibers, glass fibers and ceramic fibers; the length of the inorganic fibers is preferably 1-10 mm, more preferably 1-5 mm; the diameter of the inorganic fibers is preferably 1-50 μm, more preferably 1-15 μm.

[0029] In the present invention, the effective ingredients include 1-80% filler, preferably 10-70%, and specifically preferably 1%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75% or 80% by mass percentage. In the present invention, the filler preferably includes one or more of kaolin, diatomaceous earth, wollastonite, ceramic powder and slag.

[0030] In the present invention, the active ingredient comprises 1-10% of the flame retardant, preferably 2-9%, and specifically preferably 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5% or 10% by mass percentage. In the present invention, the flame retardant preferably comprises one or more of aluminum hydroxide, magnesium hydroxide and borate.

[0031] In the present invention, the effective ingredients include 1-10% of the dry weight of the binder, preferably 2-9%, and specifically preferably 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5% or 10% by mass percentage. In the present invention, the binder preferably includes one or more of water glass, silica sol, polyvinyl alcohol, sodium carboxymethyl cellulose, styrene-butadiene latex, styrene-acrylic latex and nitrile latex. In the present invention, the concentration of the water glass is preferably 5-50wt%, more preferably 10-30wt%. In the present invention, the content of silicon dioxide in the silica sol is preferably 15-40wt%, more preferably 20-30wt%, and further preferably 20-25wt%; the dispersion medium in the silica sol is preferably water. In the present invention, the solvent in the styrene-butadiene latex, styrene-acrylic latex and nitrile latex is preferably water, and the solid content is independently preferably 40-50%. The present invention has no special restrictions on the styrene-butadiene latex, styrene-acrylic latex and nitrile latex, and they can be prepared by commercial products well known to those skilled in the art or by preparation methods well known to those skilled in the art (for example, see: Zhang Yang, Qin Qi. Current status and production process of styrene-butadiene latex for paperboard coating [J]. Ningbo Chemical Industry, 1997 (3): 3.).

[0032] In the present invention, the effective ingredient includes 0.5-5% of nanocellulose, preferably 1-4%, and specifically preferably 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5% by mass percentage. In the present invention, the diameter of the nanocellulose is preferably <100nm, more preferably 10-30nm; the length of the nanocellulose is preferably 0.1-100μm. In the present invention, the nanocellulose preferably includes a nanocellulose aqueous dispersion and / or a nanocellulose solid powder; the solid content of the nanocellulose aqueous dispersion is preferably 1-6%, more preferably 2-5%, further preferably 3-4%, and specifically preferably 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5% or 6%.

[0033] In the present invention, the weight of the thermal insulation material is preferably 500 to 3000 g / m 2 , more preferably 1000 to 2000 g / m 2 , preferably 1200g / m 2 , 1500g / m 2 or 2000g / m 2 The thickness of the thermal insulation material is preferably 0.2 to 5 mm, more preferably 1 to 4 mm, further preferably 1.5 to 2 mm, and specifically preferably 1.3 mm, 1.5 mm or 1.9 mm; the tightness of the thermal insulation material is preferably 0.5 to 3 g / cm 3 , more preferably 0.8 to 2 g / cm 3 , preferably 0.92 g / cm 3 , 1.0g / cm 3 or 1.05g / cm 3 ; The tensile strength of the thermal insulation material is preferably >1MPa, more preferably 2-3MPa, and specifically preferably 2.2MPa, 2.78MPa or 2.95MPa; the thermal conductivity (150°C) of the thermal insulation material is preferably ≤0.15W / (m·K), more preferably ≤0.103W / (m·K), and specifically preferably 0.085W / (m·K), 0.098W / (m·K) or 0.103W / (m·K); the loss on ignition (600°C, 1h) of the thermal insulation material is preferably ≤20%, more preferably ≤16.9%, and specifically preferably 10.9% or 11.3%, 16.9%.

[0034] The present invention also provides a method for preparing the thermal insulation material described in the above technical solution, comprising the following steps: mixing the active ingredients with water, and sequentially performing dehydration, forming and drying to obtain the thermal insulation material.

[0035] In the present invention, the mixing of the active ingredient and water preferably includes the following steps: first stirring and mixing the organic fiber, the inorganic fiber and the water, second stirring and mixing the filler, the binder and the flame retardant, and third stirring and mixing the nanocellulose to obtain a slurry. In the present invention, the speed of the first stirring and mixing, the second stirring and mixing and the third stirring and mixing are independently preferably 50 to 1000 r / min, more preferably 100 to 500 r / min; the present invention has no special restrictions on the time of the first stirring and mixing and the second stirring and mixing, as long as the raw materials can be evenly dispersed in the water.

[0036] In the present invention, the dehydration forming preferably includes vacuum dehydration and pressing in sequence, specifically including the following steps: pouring the slurry into a former for vacuum dehydration, and then pressing to obtain a wet paper sheet; the vacuum dehydration preferably includes vacuum filtration; the vacuum degree of the vacuum dehydration is preferably 0.01 to 0.06 MPa, more preferably 0.02 to 0.05 MPa, and further preferably 0.03 to 0.04 MPa; the time of the vacuum dehydration is preferably 3 to 300 s, more preferably 10 to 100 s, and further preferably 15 to 60 s.

[0037] In the present invention, the pressing pressure is preferably 50-400 kPa, more preferably 100-350 kPa, and more preferably 200-300 kPa; the pressing time is preferably 10-300 s, more preferably 40-100 s, and further preferably 50-60 s; the pressing preferably includes wet pressing, and the wet pressing is preferably carried out in a wet press; the purpose of the pressing is to further dehydrate.

[0038] In the present invention, the drying temperature is preferably 70-120°C, more preferably 80-110°C, and further preferably 90-150°C; the drying time is preferably 10-1000s, more preferably 100-800s, and further preferably 500-600s; and the drying is preferably carried out in a drying cylinder.

[0039] After the drying is completed, the present invention preferably further comprises calendering the dried material to obtain a heat insulating material. In the present invention, the calendering pressure is preferably 100 to 1000 kPa, more preferably 200 to 500 kPa; the calendering temperature is preferably 20 to 150° C., more preferably 25 to 80° C.; the calendering time is preferably 1 to 60 s, more preferably 10 to 60 s, more preferably 20 to 50 s; the calendering is preferably performed in a calender.

[0040] The present invention provides the use of the thermal insulation material described in the above technical solution or the thermal insulation material prepared by the preparation method described in the above technical solution in automobiles. In the present invention, the thermal insulation material is preferably used for automotive heat insulation covers, and the automotive heat insulation cover is preferably a heat insulation cover for automotive engines or a heat insulation cover for exhaust manifolds; the thermal insulation material is more preferably used as an internal filling material for "sandwich" type automotive heat insulation covers. The thermal insulation material provided by the present invention has high physical strength, good heat resistance and flame retardancy, is adaptable to complex geometric shapes, does not burn, does not generate smoke, does not break, does not fracture, and maintains its original complete shape and form after high temperature (600°C) treatment, and fully meets the mechanical and thermal performance requirements of thermal insulation materials for automotive engines and exhaust manifolds.

[0041] In order to further illustrate the present invention, the thermal insulation material provided by the present invention and its preparation method and application are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0042] In the following examples and comparative examples, mineral fibers and ceramic fibers were purchased from Hebei Shijiazhuang Mineral Raw Materials Company. Slag was purchased from Hebei Lingshou Slag Plant. Silica sol was purchased from Shandong Linyi Silica Sol Plant. The water glass concentration was 30wt%. The solid content of styrene-butadiene latex was 50%, and the solvent was water. The solid content of nitrile latex was 40%, and the solvent was water. Slag was purchased from Hebei Lingshou Slag Plant, and the main components included SiO2, CaO, and Al2O3. The diameter of nanocellulose was <100nm and the length was 0.1 to 100μm. The length of organic fiber was 0.5 to 5mm and the diameter was 0.1 to 50μm.

[0043] Example 1

[0044] The dry weight ratio of the effective ingredients in the slurry is as follows: 9% chemical softwood pulp, 10% aluminum silicate fiber, 10% glass fiber, 30% kaolin, 30% slag, 5% aluminum hydroxide, 1% water glass, 4% styrene-butadiene latex, and 1% nanocellulose. The solvent is water, and the solid content of the slurry is 2.2%. Among them, the solid content of the nanocellulose liquid is 3.5%.

[0045] The organic fiber, inorganic fiber and water are stirred and mixed evenly, the filler, binder and flame retardant are added and stirred and mixed evenly, the nanocellulose is added and stirred and mixed evenly, the obtained slurry is poured into the molding machine, and dehydrated and formed for 19 seconds under the condition of vacuum degree of 0.05MPa; then wet pressed for 60 seconds under the condition of pressure of 300kPa by wet press; put into 95℃ drying cylinder for 600 seconds, and then calendered for 10 seconds at room temperature and 200kPa by calender to obtain the thermal insulation material. The quantitative of the thermal insulation material is 1500g / m 2 , thickness is 1.5mm, tightness is 1.0g / cm 3, tensile strength is 2.20MPa, thermal conductivity (150℃) is 0.098W / (m·K); after being placed in a 600℃ high temperature furnace, the insulation material basically does not produce smoke (such as Figure 1 As shown in the figure, the sample on the right), after being placed at 600℃ for 1h, the material still maintains its original flat shape (as shown in the figure Figure 2 As shown, the sample on the right), the weight loss rate is 16.9%.

[0046] Example 2

[0047] The dry weight ratio of effective ingredients in the slurry is as follows: 5% chemical softwood pulp, 5% aluminum silicate fiber, 10% mineral fiber, 3% ceramic fiber, 30% kaolin, 28% slag, 3% wollastonite, 5% aluminum hydroxide, 2% zinc borate, 5% nitrile latex, 2% silica sol, 2% nanocellulose, the solvent is water, and the solid content of the slurry is 3%. Among them, the solid content of the nanocellulose liquid is 3.5%.

[0048] The organic fiber, inorganic fiber and water are stirred and mixed evenly, the filler, binder and flame retardant are added and stirred and mixed evenly, the nanocellulose is added and stirred and mixed evenly, the obtained slurry is poured into the molding machine, and dehydrated and formed for 16 seconds under the condition of vacuum degree of 0.06MPa; then wet pressed for 55 seconds under the condition of pressure of 350kPa by wet press; put into 105℃ drying cylinder to dry for 600 seconds, and then calendered for 20 seconds under the condition of 80℃ and pressure of 150kPa by calender to obtain the thermal insulation material. The quantitative of the thermal insulation material is 2000g / m 2 , thickness is 1.9mm, tightness is 1.05g / cm 3 , tensile strength is 2.95MPa, thermal conductivity (150℃) is 0.085W / (m·K); after being placed in a 600℃ high-temperature furnace, the thermal insulation material basically does not produce smoke. After being placed at 600℃ for 1h, the thermal insulation material still maintains its original flat shape, and the weight loss rate is 11.3%.

[0049] Example 3

[0050] The dry weight ratio of the effective ingredients in the slurry is calculated by mass percentage: 7% chemical hardwood pulp, 10% mineral fiber, 40% kaolin, 28% slag, 3% diatomaceous earth, 4% aluminum hydroxide, 1% zinc borate, 1% water glass, 1% silica sol, 3% nitrile latex, and 2% nanocellulose; the solvent is water, and the solid content of the slurry is 2%. Among them, the solid content of the nanocellulose liquid is 3%.

[0051] The organic fiber, inorganic fiber and water are stirred and mixed evenly, the filler, binder and flame retardant are added and stirred and mixed evenly, the nanocellulose is added and stirred and mixed evenly, the obtained slurry is poured into the molding machine, and dehydrated and formed for 18 seconds under the condition of vacuum degree of 0.06MPa; then wet pressed for 60 seconds under the condition of pressure of 300kPa by wet press; put into 105℃ drying cylinder to dry for 500 seconds, and then calendered for 10 seconds under the condition of room temperature and pressure of 100kPa by calender to obtain the thermal insulation material. The quantitative of the thermal insulation material is 1200g / m 2 , thickness is 1.3mm, tightness is 0.92g / cm 3 , tensile strength is 2.78MPa, thermal conductivity (150℃) is 0.103W / (m·K); after being placed in a 600℃ high-temperature furnace, the thermal insulation material basically does not produce smoke. After being placed for 1 hour, the thermal insulation material still maintains its original flat shape, and the weight loss rate is 10.9%.

[0052] Comparative Example 1

[0053] The dry weight ratio of the effective components in the slurry is: 10% chemical softwood pulp, 10% aluminum silicate fiber, 10% glass fiber, 30% kaolin, 30% slag, 5% aluminum hydroxide, 1% water glass, and 4% styrene-butadiene latex. The solvent is water, and the solid content of the slurry is 2.2%.

[0054] The organic fiber, inorganic fiber and water are stirred and mixed evenly, and fillers, binders and flame retardants are added and stirred and mixed evenly. The obtained slurry is poured into a molding machine and dehydrated and formed for 20 seconds under a vacuum degree of 0.05MPa; then wet pressed for 60 seconds under a pressure of 300kPa using a wet press; dried in a 95℃ drying cylinder for 600 seconds, and then calendered for 10 seconds at room temperature and a pressure of 200kPa using a calender to obtain a thermal insulation material. The basis weight of the thermal insulation material is 1500g / m 2 , thickness is 1.5mm, tightness is 1.0g / cm 3 , tensile strength is 0.42MPa, thermal conductivity (150℃) is 0.169W / (m·K); after being placed in a 600℃ high temperature furnace, the material produces slight smoke (such as Figure 1 As shown in the figure, the sample on the left), after being placed at 600℃ for 1h, the insulation material loses its original flat shape and is very easy to break (such as Figure 2 As shown, the sample on the left), the weight loss rate is 17.9%.

[0055] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A thermal insulation material, characterized in that: The preparation raw materials include effective ingredients and water; in terms of mass percentage, the effective ingredients include 1-10% organic fiber, 1-80% inorganic fiber, 1-80% filler, 1-10% flame retardant, 1-10% binder, and 0.5-5% nano cellulose.

2. The thermal insulation material according to claim 1, characterized in that: The organic fiber includes one or more of chemical coniferous wood pulp, chemical broadleaf wood pulp, cotton pulp, straw pulp and aramid fiber.

3. The thermal insulation material according to claim 1, characterized in that: The inorganic fibers include one or more of aluminum silicate fibers, magnesium silicate fibers, mineral fibers, glass fibers, and ceramic fibers.

4. The thermal insulation material according to claim 1, characterized in that: The filler includes one or more of kaolin, diatomaceous earth, wollastonite, ceramic powder and slag.

5. The thermal insulation material according to claim 1, characterized in that: The flame retardant includes one or more of aluminum hydroxide, magnesium hydroxide and borate.

6. The thermal insulation material according to claim 1, characterized in that: The binder includes one or more of water glass, silica sol, polyvinyl alcohol, sodium carboxymethyl cellulose, styrene-butadiene latex, styrene-acrylic latex and nitrile-butadiene latex.

7. The thermal insulation material according to claim 1, characterized in that: The diameter of the nanocellulose is less than 100 nm and the length is 0.1 to 100 μm.

8. The method for preparing the thermal insulation material according to any one of claims 1 to 7, comprising the following steps: The active ingredient and water are mixed, and dehydration forming and drying are performed in sequence to obtain the thermal insulation material.

9. The preparation method according to claim 8, characterized in that: The dehydration forming comprises sequentially performing vacuum dehydration and pressing; The vacuum degree of the vacuum dehydration is 0.01-0.06 MPa, and the time is 3-300 s; The pressing pressure is 50-400 kPa and the pressing time is 10-300 s; The drying temperature is 70-120° C. and the drying time is 10-1000 seconds.

10. Use of the thermal insulation material according to any one of claims 1 to 7 or the thermal insulation material prepared by the preparation method according to claim 8 or 9 in a heat insulation cover for a vehicle.