Preparation method of hindered amine light stabilizer tetra-piperidine silicate
Through the reaction of orthosilicate and tetra-(V) methylpiperidol in acid catalysts and organic solvents, the problems of high production costs and high solid waste in the preparation of existing tetra-piperidyl silicate are solved, and high Preparation of tetrapiridine silicate with purity and high yield is suitable for industrial production and meets environmental protection requirements.
Patent Information
- Application Number
- CN202411164889.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-19
AI Technical Summary
The use of silicon tetrapiridine silicate in the existing preparation method for tetrapiridine silicate results in high production costs, high solid waste generation, high corrosion resistance requirements of equipment, and is sensitive to water, affecting product purity and yield.
Orthosilicate and tetrahydrofuranol react in non-polar organic solvents and acid catalysts to produce tetrahydrofuranol under normal pressure, reducing the generation of solid waste and wastewater, and achieving Recycling and reuse of alcohol.
It reduces production costs, simplifies operations, improves product purity and yield, is suitable for industrial production, and meets the requirements of circular economy and green environmental protection.
Smart Images

Figure CN118978544A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hindered amine light stabilizer synthesis, and particularly relates to a method for preparing tetrapiperidinyl silicate, a hindered amine light stabilizer. Background Art
[0002] Tetrapiperidinium silicate is a light stabilizer suitable for polymer materials such as polyethylene, polypropylene, polyvinyl chloride, polyurethane, polyamide, etc. It can be used alone. Due to the presence of silicon atoms in its structure, silicon dioxide will be produced during the combustion process, and silicon dioxide has a flame retardant effect.
[0003] Due to the unique structure of four bonds between silicon atoms, silicon-containing organic compounds have the properties of both inorganic and organic materials, and have the advantages of high and low temperature resistance, oxidation stability, weather resistance, and flame retardancy.
[0004] Silicone is called the "MSG" of industrial chemistry. A small amount of addition can greatly improve product performance. In particular, due to the further confirmation of the physiological inertness of siloxane and its safety and reliability to the human body, the number of applications of silicone in medical and cosmetics has increased dramatically. Light stabilizers containing silicone have also gradually entered the field of vision of scientific research staff.
[0005] Patents SU2041804 and CN113004317 both propose a method for preparing tetrapiperidinyl silicate, wherein silicon tetrachloride is used to synthesize tetrapiperidinyl silicate. The synthesis process requires the use of anhydrous reagents, resulting in high production costs. In the subsequent treatment, an organic base or an inorganic base must be used to neutralize the generated hydrogen chloride, which will result in the generation of a large amount of solid waste. In addition, since silicon tetrachloride is extremely sensitive to water vapor, it is very easy to hydrolyze to generate hydrogen chloride gas, which has a great impact on the purity and yield of the product. The use of silicon tetrachloride has high requirements on production equipment, requiring the production equipment to be corrosion-resistant, thereby increasing production costs.
[0006] Therefore, the present invention provides a method for preparing a hindered amine light stabilizer tetrapiperidinyl silicate to solve the above problems. Summary of the invention
[0007] The purpose of the present invention is to provide a method for preparing a hindered amine light stabilizer tetrapiperidinyl silicate, in view of the deficiencies in the prior art. Orthosilicate and tetra(penta)methylpiperidinol are used as raw materials, and a target product is generated by reacting in a non-polar organic solvent and an acidic catalyst under normal pressure.
[0008] The present invention adopts the following technical solutions: The invention provides a method for preparing tetrapiperidinyl silicate, a hindered amine light stabilizer. The method comprises the following steps: mixing 4-hydroxy-2,2,6,6-tetramethylpiperidinol or 4-hydroxy-1,2,2,6,6-pentamethylpiperidinol with an orthosilicate and a solvent, adding a catalyst, charging an inert gas, heating and stirring the mixture for reaction, and preparing tetra(2,2,6,6-tetramethylpiperidinyl)orthosilicate or tetra(1,2,2,6,6-pentamethylpiperidinyl)orthosilicate. The reaction formula is: ; Wherein, R is a methyl group or a hydrogen atom, and R' is a methyl group, an ethyl group, a propyl group or an isopropyl group.
[0009] Furthermore, the molar ratio of the orthosilicate to 4-hydroxy-2,2,6,6-tetramethylpiperidinol or 4-hydroxy-1,2,2,6,6-pentamethylpiperidinol is 1:(4.0-5.0), and the more preferred molar ratio is 1:(4.0-4.2).
[0010] Furthermore, the molar ratio of the orthosilicate to 4-hydroxy-2,2,6,6-tetramethylpiperidinol or 4-hydroxy-1,2,2,6,6-pentamethylpiperidinol is preferably 1:4.02.
[0011] Furthermore, the mass ratio of the catalyst to the orthosilicate is (0.005-0.5):1, and the more preferred mass ratio is (0.01-0.06):1.
[0012] Furthermore, the mass ratio of the catalyst to the orthosilicate is preferably 0.01:1.
[0013] Furthermore, the mass ratio of the orthosilicate to the solvent is 1:(1.0-5.0), and more preferably the mass ratio is 1:(2.8-4.6).
[0014] Furthermore, the mass ratio of the orthosilicate to the solvent is preferably 1:3.
[0015] Furthermore, the reaction temperature is 60-120° C., and the reaction time is 4-6 hours.
[0016] Furthermore, the reaction temperature is preferably 80-100-90°C.
[0017] Furthermore, the orthosilicate is one of methyl orthosilicate, ethyl orthosilicate, propyl orthosilicate and isopropyl orthosilicate.
[0018] Furthermore, the catalyst is an acidic catalyst, specifically one of sulfuric acid and methanesulfonic acid or a mixture of the two.
[0019] Furthermore, the catalyst is preferably sulfuric acid or methanesulfonic acid.
[0020] Furthermore, the solvent is n-heptane, n-octane or cyclohexane, preferably n-heptane.
[0021] Furthermore, during the reaction, the reaction material product is heated to reflux to separate the generated lower alcohol; after the reaction is completed, the reaction material product system is cooled to room temperature, the solid-liquid separation is performed, and the obtained solid is washed with an alcohol-water mixture to obtain tetrapiperidinyl silicate.
[0022] Furthermore, the alcohol in the alcohol-water mixture is methanol, ethanol or isopropanol, and the mass percentage concentration of the alcohol in the alcohol-water mixture is 5-20%, preferably 5%.
[0023] Beneficial effects of the present invention: (1) The present invention uses orthosilicate and piperidinol as raw materials, uses orthosilicate to carry out ester exchange reaction, and the alcohol produced can be effectively recycled and reused, and relatively less three wastes are produced, especially solid waste, and only a small amount of solid waste is produced when the catalyst is neutralized; and the method of the present invention produces less wastewater, is simple to operate, and is suitable for industrial production; (2) After the reaction of the present invention is completed, the product is precipitated and the separation is simple. In addition, the continuous evaporation of small alcohol molecules during the reaction can promote the forward reaction and improve the reaction efficiency. (3) After the reaction of the present invention is completed, the reaction solvent and excess piperidinol can be recovered and reused. After the reaction solvent of the present invention is reused three times, it will not affect the product quality, reduce the consumption of raw materials, save energy, and meet the requirements of circular economy and green environmental protection; (4) The GC detection content of the target product obtained by the method of the present invention can reach more than 99.8%, and the yield can reach 95%. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The gas chromatography analysis spectrum of the product prepared in Example 1 of the present invention; Figure 2 The gas chromatography analysis spectrum of the product prepared in Example 2 of the present invention; Figure 3 The gas chromatography analysis spectrum of the product prepared in Example 3 of the present invention; Figure 4 The gas chromatography analysis spectrum of the product prepared in Example 4 of the present invention; Figure 5 This is the H NMR spectrum of the product prepared in Example 1 of the present invention; Figure 6 This is the H NMR spectrum of the product prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0026] Example 1 The embodiment of the present invention provides a method for preparing tetrapiperidinyl silicate, the preparation method comprising: Step 1: Add 35 g (229.5 mmol) of methyl orthosilicate, 145.3 g (924.4 mmol) of 4-hydroxy-2,2,6,6-tetramethylpiperidinol and 2 g of sulfuric acid to a reactor, add 150 ml of n-heptane, fill with nitrogen, then stir and heat to 80-10090 °C, and keep the temperature for 4 h. During the reaction, the product was refluxed and the methanol produced was separated.
[0027] Step 2: After the reaction is completed, the product system is cooled to room temperature, the solid-liquid separation is performed, and the solid is washed with an alcohol-water mixture (5% methanol in water), then rinsed with water, and dried to obtain 139 g of the target compound tetrakis(2,2,6,6-tetramethylpiperidinyl)orthosilicate. The gas chromatography analysis shows Figure 1 , H NMR spectrum analysis see Figure 5 The yield calculated based on methyl orthosilicate was 93%, and the content detected by GC was ≥ 99.9%.
[0028] Example 2 The embodiment of the present invention provides a method for preparing tetrapiperidinyl silicate, the preparation method comprising: Step 1: Add 50 g (328.5 mmol) of methyl orthosilicate, 217 g (1380 mmol) of 4-hydroxy-2,2,6,6-tetramethylpiperidinol and 0.5 g of sulfuric acid to a reactor, add 250 ml of n-heptane, fill with nitrogen, then stir and heat to 80-10090 °C, and keep the temperature for 4.5 h. During the reaction, the product was refluxed and the methanol produced was separated.
[0029] Step 2: After the reaction is completed, the product system is cooled to room temperature, the solid-liquid separation is performed, and the solid is washed with an alcohol-water mixture (10% methanol in water), then rinsed with water, and dried to obtain 199 g of the target compound tetrakis(2,2,6,6-tetramethylpiperidinyl)orthosilicate. The gas chromatography analysis shows Figure 2 The yield calculated based on methyl orthosilicate was 93%, and the content detected by GC was ≥ 99.9%.
[0030] Example 3 The embodiment of the present invention provides a method for preparing tetrapiperidinyl silicate, the preparation method comprising: Step 1: Add 30 g (197.1 mmol) of methyl orthosilicate, 135.7 g (792.3 mmol) of 4-hydroxy-1,2,2,6,6-pentamethylpiperidinol and 0.8 g of sulfuric acid to a reactor, add 200 ml of n-heptane, fill with nitrogen, then stir and heat to 80-10090 °C, and keep the temperature for 5 h. During the reaction, the product was refluxed and the methanol produced was separated.
[0031] Step 2: After the reaction was completed, the product system was cooled to room temperature, the solid-liquid separation was performed, and the obtained solid was washed with an alcohol-water mixture (15% methanol in water), then rinsed with water, and dried to obtain 132 g of the target compound tetrakis(1,2,2,6,6-pentamethylpiperidinyl)orthosilicate. The gas chromatography analysis showed Figure 3 , H NMR spectrum analysis see Figure 6 The yield calculated based on methyl orthosilicate was 95%, and the content detected by GC was ≥ 99.9%.
[0032] Example 4 The embodiment of the present invention provides a method for preparing tetrapiperidinyl silicate, the preparation method comprising: Step 1: Add 30 g (114 mmol) of ethyl orthosilicate, 91.0 g (578.9 mmol) of 4-hydroxy-2,2,6,6-tetramethylpiperidinol and 0.5 g of methanesulfonic acid to a reactor, add 200 ml of n-heptane, fill with nitrogen, then stir and heat to 80-10090 °C, and keep the temperature for 5 h. During the reaction, the product was refluxed and the ethanol produced was separated.
[0033] Step 2: After the reaction is completed, the product system is cooled to room temperature, the solid-liquid separation is performed, and the obtained solid is washed with an alcohol-water mixture (8% methanol in water), then rinsed with water, and dried to obtain 85 g of the target compound tetrakis(2,2,6,6-tetramethylpiperidinyl)orthosilicate. The gas chromatography analysis shows Figure 4 The yield calculated based on ethyl orthosilicate was 95%, and the content detected by GC was ≥ 99.9%.
[0034] The present invention uses orthosilicate and piperidinol as raw materials, adopts orthosilicate to carry out ester exchange reaction to prepare light stabilizer tetrapiperidinyl silicate, compared with the prior art, the method of the present invention produces less three wastes, especially solid waste, only a small amount of solid waste produced when the catalyst is neutralized, and the waste water produced is less, and the produced alcohol can be effectively recycled. In addition, the method of the present invention does not produce hydrogen chloride gas, has low requirements on production equipment, reduces production cost, is easy to operate, and is suitable for industrial production. After the reaction of the present invention is completed, the reaction solvent and excessive piperidinol can be recycled, thereby reducing raw material consumption, saving energy, and meeting the requirements of circular economy and green environmental protection.
[0035] The above are only preferred implementations of the present invention. The protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications without departing from the principle of the present invention should be regarded as the protection scope of the present invention.
Claims
1. A method for preparing a hindered amine light stabilizer tetrapiperidinyl silicate, It is characterized in that The preparation method is: 4-hydroxy-2,2,6,6-tetramethylpiperidinol or 4-hydroxy-1,2,2,6,6-pentamethylpiperidinol is mixed with orthosilicate and solvent, a catalyst is added, an inert gas is introduced, and the mixture is heated and stirred for reaction to prepare tetrakis(2,2,6,6-tetramethylpiperidinyl)orthosilicate or tetrakis(1,2,2,6,6-pentamethylpiperidinyl)orthosilicate.
2. The method for preparing the hindered amine light stabilizer tetrapiperidinyl silicate according to claim 1, It is characterized in that The molar ratio of the orthosilicate to 4-hydroxy-2,2,6,6-tetramethylpiperidinol or 4-hydroxy-1,2,2,6,6-pentamethylpiperidinol is 1:(4.0-5.0).
3. The method for preparing the hindered amine light stabilizer tetrapiperidinyl silicate according to claim 1, It is characterized in that The mass ratio of the catalyst to the orthosilicate is (0.005-0.5):
1.
4. The method for preparing the hindered amine light stabilizer tetrapiperidinyl silicate according to claim 1, It is characterized in that The mass ratio of the orthosilicate to the solvent is 1:(1.0-5.0).
5. The method for preparing the hindered amine light stabilizer tetrapiperidinyl silicate according to claim 1, It is characterized in that The reaction temperature is 60-120° C., and the reaction time is 4-6 hours.
6. The method for preparing the hindered amine light stabilizer tetrapiperidinyl silicate according to claim 1, It is characterized in that The orthosilicate is one of methyl orthosilicate, ethyl orthosilicate, propyl orthosilicate and isopropyl orthosilicate.
7. The method for preparing the hindered amine light stabilizer tetrapiperidinyl silicate according to claim 1, It is characterized in that The catalyst is an acidic catalyst, specifically one of sulfuric acid and methanesulfonic acid or a mixture of the two.
8. The method for preparing the hindered amine light stabilizer tetrapiperidinyl silicate according to claim 1, It is characterized in that The solvent is n-heptane, n-octane or cyclohexane.
9. The method for preparing the hindered amine light stabilizer tetrapiperidinyl silicate according to claim 1, It is characterized in that During the reaction, the reaction material product is heated to reflux and the generated lower alcohol is separated; After the reaction is completed, the reaction material product system is cooled to room temperature, the solid-liquid separation is performed, and the obtained solid is washed with an alcohol-water mixture to obtain tetrapiperidinyl silicate.
10. The method for preparing the hindered amine light stabilizer tetrapiperidinyl silicate according to claim 9, It is characterized in that The alcohol in the alcohol-water mixture is methanol, ethanol or isopropanol, and the mass percentage concentration of the alcohol in the alcohol-water mixture is 5-20%.