Preparation process of high-wear-resistance butyronitrile frosted mosquito-repellent gloves
By using butyl acetylaminopropionate as a plasticizer and mosquito repellent in mosquito repellent, and combined with the process of modifying nitrile foaming latex, the problem of insufficient wear resistance of gloves is solved, and efficient mosquito repellent is achieved It has a wear-resistant balance effect, suitable for high friction environments.
Patent Information
- Application Number
- CN202411133912.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-19
AI Technical Summary
Existing mosquito repellent gloves have shortcomings in wear resistance, making it difficult to find a balance between mosquito repellent effect and wear resistance, resulting in a degradation in long-term use or high friction environments.
Butyl acetylaminopropionate is used as a mosquito repellent and plasticizer to form an emulsified liquid through emulsion treatment, combined with modified nitrile foamed matte latex, salt spray matte treatment and vulcanization treatment to enhance the wear resistance of the gloves' coating and mosquito repellent effect.
Improves the wear resistance and mosquito repellency of gloves. The addition of butyl acetyl aminopropionate is optimal in the range of 10-20 parts, which can effectively reduce stress concentration and improve flexibility, enhance the physical and mechanical coating. Performance, ensuring that it is not easy to damage during friction or impact, and is non-toxic and allergic to the skin and mucous membranes.
Smart Images

Figure CN118978738A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of glove manufacturing, and in particular to a preparation process of highly wear-resistant nitrile frosted mosquito repellent gloves. Background Art
[0002] Products such as mosquito repellent gloves are suitable for any working environment that requires outdoor activities or possible contact with mosquitoes. For example, in activities such as camping, hiking, fishing, outdoor barbecues, etc., mosquito repellent gloves can protect hands from mosquito bites and make activities more comfortable; when doing outdoor work such as gardening and pruning flowers and plants, mosquito repellent gloves can effectively prevent mosquito interference and protect hands; farmers often face mosquito problems when working in the fields, and mosquito repellent gloves can help them reduce mosquito bites and improve work efficiency; even when conducting medical assistance or scientific research activities outdoors, mosquito repellent gloves can protect staff from mosquito bites and reduce the risk of disease transmission. Summary of the invention
[0003] The purpose of the present invention is to provide a preparation process of highly wear-resistant nitrile frosted mosquito repellent gloves, so that the surface coating of the nitrile gloves can produce certain mosquito repellent properties while improving the wear resistance.
[0004] The above technical objectives of the present invention are achieved through the following technical solutions:
[0005] A preparation process of highly wear-resistant nitrile frosted mosquito repellent gloves, characterized by comprising the following steps:
[0006] S1, preparing ethyl butyl acetylaminopropionate emulsion;
[0007] S2, preparing modified nitrile foaming frosted latex;
[0008] S3, put the nylon glove core on the hand mold and put it into the oven for preheating;
[0009] S4, the preheated nylon glove core is immersed in the coagulant;
[0010] S5, after homogenizing the glove core, immersing it in modified nitrile foaming frosted latex;
[0011] S6, after the glue is evenly coated at room temperature, a salt spraying and sanding treatment is performed;
[0012] S7, after the salt spraying and sanding treatment, the product is placed in an oven for pre-sulfurization treatment;
[0013] S8, pre-vulcanization is completed, soaking, washing, desalting and wringing, and then vulcanization is carried out;
[0014] S9, demoulding the gloves and sealing and packaging the prepared gloves in a light-proof manner.
[0015] Preferably, the specific steps of preparing the ethyl butyl acetylaminopropionate emulsion in S1 are: taking 80 parts of deionized water and 20 parts of ethyl butyl acetylaminopropionate by weight, mixing and stirring for 5 minutes, adding 3 parts of emulsifier sodium dodecylbenzene sulfonate, and using a high-speed emulsifier to whip and emulsify at a high speed of 7500 rpm. The preparation is completed after 15 minutes.
[0016] Preferably, the modified nitrile foamed frosted latex in S2 includes the following ingredients in parts by weight: 100 parts of nitrile latex, 1 part of potassium hydroxide, 1-2 parts of sulfur, 1-2 parts of zinc oxide, 1 part of accelerator ZDEC, 3-4 parts of foaming agent sodium dodecylbenzene sulfonate, 1 part of titanium dioxide, 10-20 parts of ethyl butyl acetylaminopropionate emulsion, and 1 part of color paste.
[0017] Preferably, the specific steps of preparing the modified nitrile foamed frosted latex are: gradually adding potassium hydroxide, sulfur, zinc oxide, accelerator, titanium dioxide and foaming agent to the nitrile latex solution and mixing evenly, and then slowly adding ethyl butyl acetylaminopropionate emulsion and color paste under stirring, stirring at a uniform speed for 15 minutes and then using a foamer to whip and foam at high speed, the foaming ratio is controlled at 1.2 times, and then stirring at room temperature for 5-8 hours to thicken to a viscosity of 4500mpa.s to obtain the modified nitrile foamed frosted latex.
[0018] Preferably, the oven is preheated to 60° C. in S3.
[0019] Preferably, the coagulant in S4 is a methanol solution of 3% by mass of glacial acetic acid.
[0020] Preferably, the homogenization time of the glove core in S5 is 50s.
[0021] Preferably, the gelling time in S6 is 20 seconds at room temperature.
[0022] Preferably, the pre-vulcanization treatment time in S7 is 1 hour, and the pre-vulcanization temperature is set to 95°C.
[0023] Preferably, the vulcanization time in S8 is 40 minutes, and the vulcanization temperature is set to 80°C.
[0024] In summary, the present invention has the following beneficial effects:
[0025] 1. The ethyl butyl acetylaminopropionate added in the present invention can be used as a broad-spectrum and highly effective insect repellent. Its main working principle is to directly affect the tactile organs and chemical receptors of mosquitoes, act on the nervous system of mosquitoes during the mosquito repelling process, interfere with their nerve conduction, and thus achieve the effect of repelling mosquitoes. Compared with other similar repellents, ethyl butyl acetylaminopropionate has the characteristics of lower toxicity, less irritation, longer repelling time, etc., has the advantages of no toxic side effects on the skin and mucous membranes, no allergy, no skin permeability, etc., has a high safety factor, and has a high matching degree with the formula system of nitrile latex, and will not affect the stability of the latex.
[0026] 2. In addition, ethyl butyl acetylaminopropionate itself can also be used as a plasticizer. The appropriate addition has a significant effect on the wear resistance of the glove coating surface. The mechanism of ethyl butyl acetylaminopropionate in increasing the wear resistance of latex coatings mainly involves the following two aspects: First, reducing stress concentration. By inserting between the molecular chains of latex polymers, the mutual friction between the molecular chains is reduced, so that the material can be better deformed when subjected to external forces, thereby reducing stress concentration points. Second, improving flexibility. Once the flexibility of the latex coating is increased, the coating can better absorb energy when subjected to friction or impact, rather than directly causing material damage. The coating with good flexibility is less likely to crack and fall off during the friction process, thereby improving wear resistance.
[0027] 3. The present invention adopts an emulsification method to process ethyl butyl acetylaminopropionate, and utilizes the high-speed shear force when the emulsifier is running to forcibly disperse the plasticizer ethyl butyl acetylaminopropionate to form an emulsion. The hydrophobic groups in ethyl butyl acetylaminopropionate cause dispersion and adsorption, and the charge distribution inside the molecule is uneven, forming polar regions and non-polar regions. In this way, the plasticizer molecules can be self-assembled in the solution to form a dispersed state, so that the plasticizer molecules are soluble in water or an organic solvent. When ethyl butyl acetylaminopropionate is added into the latex formula in the form of an emulsion, the effect is better. The emulsified ethyl butyl acetylaminopropionate can improve the physical and mechanical properties of the latex coating, thereby improving its wear resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The present invention is a flow chart of a preparation process of a highly wear-resistant nitrile frosted mosquito repellent glove. DETAILED DESCRIPTION
[0029] The specific implementation manner of the present invention is further described below in conjunction with the accompanying drawings, and this embodiment does not constitute a limitation of the present invention.
[0030] Example 1
[0031] like Figure 1 The preparation process of a highly wear-resistant nitrile scrub mosquito repellent gloves shown comprises the following steps:
[0032] S1, preparing ethyl butyl acetylaminopropionate emulsion: taking 80 parts by weight of deionized water and 20 parts by weight of ethyl butyl acetylaminopropionate, mixing and stirring for 5 minutes, adding 3 parts of emulsifier sodium dodecylbenzene sulfonate, and using a high-speed emulsifier to whip and emulsify at a high speed of 7500 rpm. The preparation is completed after 15 minutes;
[0033] S2, preparing modified nitrile foaming frosted latex: the modified nitrile foaming frosted latex includes the following components in parts by weight: 100 parts of nitrile latex, 1 part of potassium hydroxide, 1 part of sulfur, 1 part of zinc oxide, 1 part of accelerator ZDEC, 3 parts of sodium dodecylbenzene sulfonate as a foaming agent, 1 part of titanium dioxide, 10 parts of ethyl butyl acetylaminopropionate emulsion, and 1 part of color paste, and the specific steps are: gradually adding potassium hydroxide, sulfur, zinc oxide, accelerator, titanium dioxide and foaming agent to the nitrile latex solution and mixing them evenly, and then slowly adding ethyl butyl acetylaminopropionate emulsion and color paste under stirring, stirring at a uniform speed for 15 minutes, and then using a foamer to whip and foam at high speed, the foaming ratio is controlled at 1.2 times, and after stirring for another 5 hours at room temperature, the viscosity is thickened to 4500mpa·s, and the modified nitrile foaming frosted latex is obtained;
[0034] S3, put the nylon glove core on the hand mold and put it into a 60℃ oven for preheating;
[0035] S4, immersing the preheated nylon glove core in a methanol solution containing 3% glacial acetic acid as a coagulant;
[0036] S5, after homogenizing the glove core for 50 seconds, immerse it in modified nitrile foaming frosted latex;
[0037] S6, after 20s of glue spreading at room temperature, salt spraying and sanding treatment is performed;
[0038] S7, after the salt spraying and sanding treatment, the product is placed in an oven for pre-vulcanization treatment for 1 hour, and the pre-vulcanization temperature is set at 95°C;
[0039] S8, pre-vulcanization is completed, soak, wash, desalt and wring, then vulcanize for 40 minutes, and the vulcanization temperature is set to 80℃;
[0040] S9, demoulding the gloves and sealing and packaging the prepared gloves in a light-proof manner.
[0041] Example 2
[0042] like Figure 1 The preparation process of a highly wear-resistant nitrile scrub mosquito repellent gloves shown comprises the following steps:
[0043] S1, preparing ethyl butyl acetylaminopropionate emulsion: taking 80 parts by weight of deionized water and 20 parts by weight of ethyl butyl acetylaminopropionate, mixing and stirring for 5 minutes, adding 3 parts of emulsifier sodium dodecylbenzene sulfonate, and using a high-speed emulsifier to whip and emulsify at a high speed of 7500 rpm. The preparation is completed after 15 minutes;
[0044] S2, preparing modified nitrile foaming frosted latex: the modified nitrile foaming frosted latex includes the following components in parts by weight: 100 parts of nitrile latex, 1 part of potassium hydroxide, 1 part of sulfur, 1 part of zinc oxide, 1 part of accelerator ZDEC, 3 parts of sodium dodecylbenzene sulfonate as a foaming agent, 1 part of titanium dioxide, 15 parts of ethyl butyl acetylaminopropionate emulsion, and 1 part of color paste, and the specific steps are: gradually adding potassium hydroxide, sulfur, zinc oxide, accelerator, titanium dioxide and foaming agent to the nitrile latex solution and mixing them evenly, and then slowly adding ethyl butyl acetylaminopropionate emulsion and color paste under stirring, stirring at a uniform speed for 15 minutes, and then using a foamer to whip and foam at high speed, the foaming ratio is controlled at 1.2 times, and after stirring for another 6 hours at room temperature, the viscosity is thickened to 4500mpa·s, and the modified nitrile foaming frosted latex is obtained;
[0045] S3, put the nylon glove core on the hand mold and put it into a 60℃ oven for preheating;
[0046] S4, immersing the preheated nylon glove core in a methanol solution containing 3% glacial acetic acid as a coagulant;
[0047] S5, after homogenizing the glove core for 50 seconds, immerse it in modified nitrile foaming frosted latex;
[0048] S6, after 20s of glue spreading at room temperature, salt spraying and sanding treatment is performed;
[0049] S7, after the salt spraying and sanding treatment, the product is placed in an oven for pre-vulcanization treatment for 1 hour, and the pre-vulcanization temperature is set at 95°C;
[0050] S8, pre-vulcanization is completed, soak, wash, desalt and wring, then vulcanize for 40 minutes, and the vulcanization temperature is set to 80℃;
[0051] S9, demoulding the gloves and sealing and packaging the prepared gloves in a light-proof manner.
[0052] Example 3
[0053] like Figure 1 The preparation process of a highly wear-resistant nitrile scrub mosquito repellent gloves shown comprises the following steps:
[0054] S1, preparing ethyl butyl acetylaminopropionate emulsion: taking 80 parts by weight of deionized water and 20 parts by weight of ethyl butyl acetylaminopropionate, mixing and stirring for 5 minutes, adding 3 parts of emulsifier sodium dodecylbenzene sulfonate, and using a high-speed emulsifier to whip and emulsify at a high speed of 7500 rpm. The preparation is completed after 15 minutes;
[0055] S2, preparing modified nitrile foaming frosted latex: the modified nitrile foaming frosted latex includes the following components in parts by weight: 100 parts of nitrile latex, 1 part of potassium hydroxide, 1 part of sulfur, 1 part of zinc oxide, 1 part of accelerator ZDEC, 3 parts of sodium dodecylbenzene sulfonate as a foaming agent, 1 part of titanium dioxide, 20 parts of ethyl butyl acetylaminopropionate emulsion, and 1 part of color paste, and the specific steps are: gradually adding potassium hydroxide, sulfur, zinc oxide, accelerator, titanium dioxide and foaming agent to the nitrile latex solution and mixing them evenly, and then slowly adding ethyl butyl acetylaminopropionate emulsion and color paste under stirring, stirring at a uniform speed for 15 minutes, and then using a foamer to whip and foam at high speed, the foaming ratio is controlled at 1.2 times, and after stirring for another 7 hours at room temperature, the viscosity is thickened to 4500mpa·s, and the modified nitrile foaming frosted latex is obtained;
[0056] S3, put the nylon glove core on the hand mold and put it into a 60℃ oven for preheating;
[0057] S4, immersing the preheated nylon glove core in a methanol solution containing 3% glacial acetic acid as a coagulant;
[0058] S5, after homogenizing the glove core for 50 seconds, immerse it in modified nitrile foaming frosted latex;
[0059] S6, after 20s of glue spreading at room temperature, salt spraying and sanding treatment is performed;
[0060] S7, after the salt spraying and sanding treatment, the product is placed in an oven for pre-vulcanization treatment for 1 hour, and the pre-vulcanization temperature is set at 95°C;
[0061] S8, pre-vulcanization is completed, soak, wash, desalt and wring, then vulcanize for 40 minutes, and the vulcanization temperature is set to 80℃;
[0062] S9, demoulding the gloves and sealing and packaging the prepared gloves in a light-proof manner.
[0063] Example 4
[0064] like Figure 1 The preparation process of a highly wear-resistant nitrile scrub mosquito repellent gloves shown comprises the following steps:
[0065] S1, preparing ethyl butyl acetylaminopropionate emulsion: taking 80 parts by weight of deionized water and 20 parts by weight of ethyl butyl acetylaminopropionate, mixing and stirring for 5 minutes, adding 3 parts of emulsifier sodium dodecylbenzene sulfonate, and using a high-speed emulsifier to whip and emulsify at a high speed of 7500 rpm. The preparation is completed after 15 minutes;
[0066] S2, preparing modified nitrile foaming frosted latex: the modified nitrile foaming frosted latex includes the following components in parts by weight: 100 parts of nitrile latex, 1 part of potassium hydroxide, 2 parts of sulfur, 2 parts of zinc oxide, 1 part of accelerator ZDEC, 4 parts of sodium dodecylbenzene sulfonate as a foaming agent, 1 part of titanium dioxide, 20 parts of ethyl butyl acetylaminopropionate emulsion, and 1 part of color paste, and the specific steps are: gradually adding potassium hydroxide, sulfur, zinc oxide, accelerator, titanium dioxide and foaming agent to the nitrile latex solution and mixing them evenly, and then slowly adding ethyl butyl acetylaminopropionate emulsion and color paste under stirring, stirring at a uniform speed for 15 minutes, and then using a foamer to whip and foam at high speed, the foaming ratio is controlled at 1.2 times, and after stirring for another 8 hours at room temperature, the viscosity is thickened to 4500mpa·s, and the modified nitrile foaming frosted latex is obtained;
[0067] S3, put the nylon glove core on the hand mold and put it into a 60℃ oven for preheating;
[0068] S4, immersing the preheated nylon glove core in a methanol solution containing 3% glacial acetic acid as a coagulant;
[0069] S5, after homogenizing the glove core for 50 seconds, immerse it in modified nitrile foaming frosted latex;
[0070] S6, after 20s of glue spreading at room temperature, salt spraying and sanding treatment is performed;
[0071] S7, after the salt spraying and sanding treatment, the product is placed in an oven for pre-vulcanization treatment for 1 hour, and the pre-vulcanization temperature is set at 95°C;
[0072] S8, pre-vulcanization is completed, soak, wash, desalt and wring, then vulcanize for 40 minutes, and the vulcanization temperature is set to 80℃;
[0073] S9, demoulding the gloves and sealing and packaging the prepared gloves in a light-proof manner.
[0074] Comparative Example 1
[0075] A process for preparing common nylon nitrile frosted gloves comprises the following steps:
[0076] S1, preparing nitrile foaming frosted latex: the nitrile foaming frosted latex comprises the following components in parts by weight: 100 parts of nitrile latex, 1 part of potassium hydroxide, 1 part of sulfur, 1 part of zinc oxide, 1 part of accelerator ZDEC, 3 parts of sodium dodecylbenzene sulfonate as a foaming agent, 1 part of titanium dioxide, and 1 part of color paste, and the specific steps are: gradually adding potassium hydroxide, sulfur, zinc oxide, accelerator, titanium dioxide and foaming agent to the nitrile latex solution and mixing them evenly, and then slowly adding the color paste under stirring, stirring at a uniform speed for 15 minutes, and then using a foamer to whip and foam at a high speed, the foaming ratio is controlled at 1.2 times, and after stirring for another 7 hours at room temperature, the viscosity is thickened to 4500mpa·s, so as to obtain the modified nitrile foaming frosted latex;
[0077] S3, put the nylon glove core on the hand mold and put it into a 60℃ oven for preheating;
[0078] S4, immersing the preheated nylon glove core in a methanol solution containing 3% glacial acetic acid as a coagulant;
[0079] S5, after homogenizing the glove core for 50 seconds, immerse it in modified nitrile foaming frosted latex;
[0080] S6, after 20s of glue spreading at room temperature, salt spraying and sanding treatment is performed;
[0081] S7, after the salt spraying and sanding treatment, the product is placed in an oven for pre-vulcanization treatment for 1 hour, and the pre-vulcanization temperature is set at 95°C;
[0082] S8, pre-vulcanization is completed, soak, wash, desalt and wring, then vulcanize for 40 minutes, and the vulcanization temperature is set to 80℃;
[0083] S9, demoulding the gloves and sealing and packaging the prepared gloves in a light-proof manner.
[0084] Comparative Example 2
[0085] A preparation process of highly wear-resistant nitrile frosted mosquito repellent gloves, comprising the following steps:
[0086] S1, preparing ethyl butyl acetylaminopropionate emulsion: taking 80 parts by weight of deionized water and 20 parts by weight of ethyl butyl acetylaminopropionate, mixing and stirring for 5 minutes, adding 3 parts of emulsifier sodium dodecylbenzene sulfonate, and using a high-speed emulsifier to whip and emulsify at a high speed of 7500 rpm. The preparation is completed after 15 minutes;
[0087] S2, preparing modified nitrile foaming frosted latex: the modified nitrile foaming frosted latex includes the following components in parts by weight: 100 parts of nitrile latex, 1 part of potassium hydroxide, 2 parts of sulfur, 2 parts of zinc oxide, 1 part of accelerator ZDEC, 4 parts of sodium dodecylbenzene sulfonate as a foaming agent, 1 part of titanium dioxide, 25 parts of ethyl butyl acetylaminopropionate emulsion, and 1 part of color paste, and the specific steps are: gradually adding potassium hydroxide, sulfur, zinc oxide, accelerator, titanium dioxide and foaming agent to the nitrile latex solution and mixing them evenly, and then slowly adding ethyl butyl acetylaminopropionate emulsion and color paste under stirring, stirring at a uniform speed for 15 minutes, and then using a foamer to whip and foam at high speed, the foaming ratio is controlled at 1.2 times, and after stirring for another 6 hours at room temperature, the viscosity is thickened to 4500mpa·s, and the modified nitrile foaming frosted latex is obtained;
[0088] S3, put the nylon glove core on the hand mold and put it into a 60℃ oven for preheating;
[0089] S4, immersing the preheated nylon glove core in a methanol solution containing 3% glacial acetic acid as a coagulant;
[0090] S5, after homogenizing the glove core for 50 seconds, immerse it in modified nitrile foaming frosted latex;
[0091] S6, after 20s of glue spreading at room temperature, salt spraying and sanding treatment is performed;
[0092] S7, after the salt spraying and sanding treatment, the product is placed in an oven for pre-vulcanization treatment for 1 hour, and the pre-vulcanization temperature is set at 95°C;
[0093] S8, pre-vulcanization is completed, soak, wash, desalt and wring, then vulcanize for 40 minutes, and the vulcanization temperature is set to 80℃;
[0094] S9, demoulding the gloves and sealing and packaging the prepared gloves in a light-proof manner.
[0095] Comparative Example 3
[0096] A preparation process of highly wear-resistant nitrile frosted mosquito repellent gloves, comprising the following steps:
[0097] S1, preparing ethyl butyl acetylaminopropionate emulsion: taking 80 parts by weight of deionized water and 20 parts by weight of ethyl butyl acetylaminopropionate, mixing and stirring for 5 minutes, adding 3 parts of emulsifier sodium dodecylbenzene sulfonate, and using a high-speed emulsifier to whip and emulsify at a high speed of 7500 rpm. The preparation is completed after 15 minutes;
[0098] S2, preparing modified nitrile foaming frosted latex: the modified nitrile foaming frosted latex includes the following components in parts by weight: 100 parts of nitrile latex, 1 part of potassium hydroxide, 2 parts of sulfur, 2 parts of zinc oxide, 1 part of accelerator ZDEC, 4 parts of sodium dodecylbenzene sulfonate as a foaming agent, 1 part of titanium dioxide, 30 parts of ethyl butyl acetylaminopropionate emulsion, and 1 part of color paste, and the specific steps are: gradually adding potassium hydroxide, sulfur, zinc oxide, accelerator, titanium dioxide and foaming agent to the nitrile latex solution and mixing them evenly, and then slowly adding ethyl butyl acetylaminopropionate emulsion and color paste under stirring, stirring at a uniform speed for 15 minutes, and then using a foamer to whip and foam at high speed, the foaming ratio is controlled at 1.2 times, and after stirring for another 8 hours at room temperature, the viscosity is thickened to 4500mpa·s, and the modified nitrile foaming frosted latex is obtained;
[0099] S3, put the nylon glove core on the hand mold and put it into a 60℃ oven for preheating;
[0100] S4, immersing the preheated nylon glove core in a methanol solution containing 3% glacial acetic acid as a coagulant;
[0101] S5, after homogenizing the glove core for 50 seconds, immerse it in modified nitrile foaming frosted latex;
[0102] S6, after 20s of glue spreading at room temperature, salt spraying and sanding treatment is performed;
[0103] S7, after the salt spraying and sanding treatment, the product is placed in an oven for pre-vulcanization treatment for 1 hour, and the pre-vulcanization temperature is set at 95°C;
[0104] S8, pre-vulcanization is completed, soak, wash, desalt and wring, then vulcanize for 40 minutes, and the vulcanization temperature is set to 80℃;
[0105] S9, demoulding the gloves and sealing and packaging the prepared gloves in a light-proof manner.
[0106] In order to detect the mosquito repellent effect of gloves, a set of test standards for mosquito repellent effect is designed. After data analysis, the mosquito repellent rate is reasonably calculated. The following Table 1 is the designed mosquito repellent gloves test standard:
[0107] Table 1 Testing standards for mosquito repellent gloves
[0108]
[0109] The wear resistance and mosquito repellent effect tests of the above-mentioned Examples 1-4 and Comparative Examples 1-3 were conducted. The mechanical properties of the gloves were tested using the European standard EN-388 test method. The specific test results are shown in Table 2 below:
[0110] Table 2 Wear resistance and mosquito repellent effect test results of each embodiment and comparative example
[0111] Test No. Number of bites Mosquito repellent rate (%) Wear-resistant (r) Tear resistance Puncture resistance Example 1 4 80 11200 Level 3 Level 1 Example 2 5 75 12600 Level 3 Level 1 Example 3 2 90 15600 Level 3 Level 1 Example 4 1 95 15000 Level 3 Level 1 Comparative Example 1 20 / 8300 Level 3 Level 1 Comparative Example 2 2 90 7300 Level 3 Level 1 Comparative Example 3 2 90 7000 Level 3 Level 1
[0112] It can be seen from the above experimental data that the treatment method provided by the present invention can indeed increase the mosquito repellent effect of the scrub gloves. However, analysis shows that although adding ethyl butyl acetylaminopropionate to the formula of nitrile scrub gloves is effective, if the added amount is insufficient or absent, the mosquito repellent effect will be greatly reduced and the ideal mosquito repellent rate cannot be achieved, as shown in Comparative Example 1. Of course, it is not the case that the more the amount added, the better. When the amount of ethyl butyl acetylaminopropionate added exceeds 20 parts, although the mosquito repellent effect does not change much, the wear resistance of the gloves is greatly affected. As shown in Comparative Examples 2 and 3, the reason is that excessive addition of ethyl butyl acetylaminopropionate will significantly weaken the interaction between the polymer molecular chains and significantly reduce the overall strength of the material. Within a certain range, adding ethyl butyl acetylaminopropionate will make the gloves more flexible and produce beneficial effects. Once excessive, it will cause excessive softening of the coating surface material and reduce its ability to resist external deformation. Therefore, considering comprehensively, in order to have both mosquito repellent and wear-resistant effects, 10-20 parts of ethyl butyl acetylaminopropionate emulsion addition is the most suitable range.
[0113] The ethyl butyl acetylaminopropionate added in the present invention can be used as a broad-spectrum and highly effective insect repellent. Its main working principle is to directly affect the tactile organs and chemical receptors of mosquitoes, act on the nervous system of mosquitoes during the mosquito repelling process, interfere with its nerve conduction, and thus achieve the effect of repelling mosquitoes. Compared with other similar repellents, ethyl butyl acetylaminopropionate has the characteristics of lower toxicity, less irritation, longer repelling time, etc., has the advantages of no toxic side effects on skin and mucous membranes, no allergy, no skin permeability, etc., has a high safety factor, and has a high matching degree with the formula system of nitrile latex, and will not affect the stability of the latex.
[0114] In addition, ethyl butyl acetylaminopropionate itself can also be used as a plasticizer. The appropriate addition has a significant effect on the wear resistance of the glove coating surface. The mechanism of ethyl butyl acetylaminopropionate in increasing the wear resistance of latex coatings mainly involves the following two aspects: First, reducing stress concentration. By inserting between the molecular chains of latex polymers, the mutual friction between the molecular chains is reduced, so that the material can be better deformed when subjected to external forces, thereby reducing stress concentration points. Second, improving flexibility. Once the flexibility of the latex coating is increased, the coating can better absorb energy when subjected to friction or impact, rather than directly causing material damage. The coating with good flexibility is less likely to crack and fall off during friction, thereby improving wear resistance.
[0115] The invention adopts an emulsification method to process ethyl butyl acetylaminopropionate, utilizes the high-speed shear force when the emulsifier is running, and forces the ethyl butyl acetylaminopropionate as a plasticizer to be dispersed to form an emulsion liquid. The hydrophobic groups in the ethyl butyl acetylaminopropionate cause dispersion and adsorption, and the charge distribution inside the molecules is uneven, forming polar regions and non-polar regions, so that the plasticizer molecules can be self-assembled in the solution to form a dispersed state, so that the plasticizer molecules are soluble in water or an organic solvent. When the ethyl butyl acetylaminopropionate is added into the latex formula in the form of an emulsion, the effect is better, and the emulsified ethyl butyl acetylaminopropionate can improve the physical and mechanical properties of the latex coating, thereby improving its wear resistance.
[0116] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Those skilled in the art may make various modifications or equivalent substitutions to the present invention within the essence and protection scope of the present invention, and such modifications or equivalent substitutions should also be deemed to fall within the protection scope of the technical solution of the present invention.
Claims
1. A preparation process of highly wear-resistant nitrile frosted mosquito repellent gloves, characterized in that: The steps include: S1, preparing ethyl butyl acetylaminopropionate emulsion; S2, preparing modified nitrile foaming frosted latex; S3, put the nylon glove core on the hand mold and put it into the oven for preheating; S4, the preheated nylon glove core is immersed in the coagulant; S5, after homogenizing the glove core, immersing it in modified nitrile foaming frosted latex; S6, after the glue is evenly coated at room temperature, a salt spraying and sanding treatment is performed; S7, after the salt spraying and sanding treatment, the product is placed in an oven for pre-sulfurization treatment; S8, pre-vulcanization is completed, soaking, washing, desalting and wringing, and then vulcanization is carried out; S9, demoulding the gloves and sealing and packaging the prepared gloves in a light-proof manner.
2. The process for preparing a highly wear-resistant nitrile frosted mosquito repellent gloves according to claim 1, characterized in that: The specific steps of preparing the ethyl butyl acetylaminopropionate emulsion in S1 are as follows: 80 parts by weight of deionized water and 20 parts by weight of ethyl butyl acetylaminopropionate are mixed and stirred for 5 minutes, 3 parts of an emulsifier sodium dodecylbenzene sulfonate are added, and a high-speed emulsifier is used for high-speed whipping and emulsification at a speed of 7500 rpm. The preparation is completed after 15 minutes.
3. The process for preparing a highly wear-resistant nitrile frosted mosquito repellent gloves according to claim 1, characterized in that: The modified nitrile foamed frosted latex in S2 includes the following components in parts by weight: 100 parts of nitrile latex, 1 part of potassium hydroxide, 1-2 parts of sulfur, 1-2 parts of zinc oxide, 1 part of accelerator ZDEC, 3-4 parts of foaming agent sodium dodecylbenzene sulfonate, 1 part of titanium dioxide, 10-20 parts of ethyl butyl acetylaminopropionate emulsion, and 1 part of color paste.
4. The process for preparing a highly wear-resistant nitrile frosted mosquito repellent gloves according to claim 3, characterized in that: The specific steps of preparing the modified nitrile foamed frosted latex are: gradually adding potassium hydroxide, sulfur, zinc oxide, accelerator, titanium dioxide and foaming agent into the nitrile latex solution and mixing them evenly, then slowly adding ethyl butyl acetylaminopropionate emulsion and color paste under stirring, stirring at a uniform speed for 15 minutes, and then using a foamer to whip and foam at high speed, the foaming ratio is controlled at 1.2 times, and then stirring at room temperature for 5-8 hours to thicken to a viscosity of 4500mpa·s, so as to obtain the modified nitrile foamed frosted latex.
5. The process for preparing a highly wear-resistant nitrile frosted mosquito repellent gloves according to claim 1, characterized in that: In S3, the oven is preheated to 60°C.
6. The process for preparing a highly wear-resistant nitrile frosted mosquito repellent gloves according to claim 1, characterized in that: The coagulant in S4 is a methanol solution of 3% by mass glacial acetic acid.
7. The process for preparing a highly wear-resistant nitrile frosted mosquito repellent gloves according to claim 1, characterized in that: The homogenization time of the glove core in S5 is 50s.
8. The process for preparing a highly wear-resistant nitrile frosted mosquito repellent gloves according to claim 1, characterized in that: In S6, the gelling time under room temperature is 20 seconds.
9. The process for preparing a highly wear-resistant nitrile frosted mosquito repellent gloves according to claim 1, characterized in that: The pre-vulcanization treatment time in S7 is 1 hour, and the pre-vulcanization temperature is set to 95°C.
10. The process for preparing a highly wear-resistant nitrile frosted mosquito repellent gloves according to claim 1, characterized in that: In the S8, the vulcanization time is 40 minutes and the vulcanization temperature is set to 80°C.