Stripping method of hexagonal boron nitride, anticorrosive paint and anticorrosive coating

Through the galli blue assisted ball milling method, the problem of poor dispersion of hexagonal boron nitride in the anticorrosion coating is solved, and its efficient dispersion and barrier properties in the resin are achieved, which significantly enhances the protection effect of the anticorrosion coating, especially in the It exhibits excellent corrosion resistance in marine environments.

CN118978824AActive Publication Date: 2024-11-19NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411139725.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-19
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

In the prior art, hexagonal boron nitride has poor dispersion in the anticorrosion coating, which leads to inability to provide sufficient protection during corrosion, and common peeling strategies cannot effectively reduce the thickness of the layered material, limiting it. Barrier performance in anticorrosion coatings.

Method used

Gallic blue is used as the intercalator, and the ball milling treatment method is used to achieve efficient peeling and dispersion of hexagonal boron nitride, forming a gallic blue-boron nitride hybrid material, and improving its dispersion and barrier properties in the resin.

Benefits of technology

The thickness of the sheet layer of hexagonal boron nitride is significantly reduced, its dispersion and barrier properties in the coating are improved, and the protection effect of the anticorrosion coating is enhanced, especially in marine environments, which show long-term anticorrosion properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978824A_ABST
    Figure CN118978824A_ABST
Patent Text Reader

Abstract

The invention provides a stripping method of hexagonal boron nitride, an anticorrosive paint and an anticorrosive coating. The stripping method of the hexagonal boron nitride comprises the step of carrying out ball milling treatment on a mixture containing the hexagonal boron nitride and an intercalator, wherein the intercalator comprises nutgall blue. Boron nitride is stripped by adopting a nutgall blue auxiliary ball milling method, a boron nitride lamellar material with a good dispersion effect can be obtained, the problem that boron nitride is easy to stack and difficult to disperse in resin is solved, and nutgall blue can also be used as a corrosion inhibitor to further improve the anti-corrosion effect of a coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal surface protection, and specifically relates to a method for stripping hexagonal boron nitride nanosheets, a method for preparing a gallic blue-boron nitride hybrid material, an anticorrosive coating agent and an anticorrosive coating. Background Art

[0002] Metal corrosion is a thorny problem that poses a threat to human safety and causes huge economic losses in various industries. Epoxy coatings stand out for their excellent adhesion, chemical stability and processability. However, cracks and holes are inevitable in the epoxy matrix, which leads to poor long-term corrosion protection of the coating. Corrosive media (such as O2, Cl-, H2O, etc.) will penetrate into the matrix through defects and then react with the metal. To address this problem, it has been proven that adding two-dimensional (2D) materials as nanofillers to the matrix can promote the maze effect to improve the physical barrier properties of the coating, which is an effective means to solve the above problems.

[0003] Hexagonal boron nitride (h-BN) has a sp 2 Hybrid layered structures, where B and N are arranged alternately and uniformly in a honeycomb configuration, continue to attract attention due to their excellent thermal stability, wear resistance under certain conditions, and excellent barrier properties. It is worth noting that h-BN has a perfect combination of the advantages of graphene and insulating properties, making it more promising in long-term corrosion protection. However, weak van der Waals forces always lead to aggregation between adjacent layers, which greatly limits its excellent barrier properties in anti-corrosion coatings. In order to better disperse h-BN nanosheets in aqueous solution, common exfoliation strategies include chemical modification and non-covalent modification. Compared with the former, non-covalent modification provides a very simple and efficient way to achieve uniform dispersion while retaining the original properties of h-BN to the greatest extent. However, the layered materials exfoliated by existing methods mainly play a key role in producing a barrier effect in the initial stage of the corrosion process. In the corrosion reaction stage, they cannot provide sufficient protection. Therefore, existing coatings usually add additional corrosion inhibitors, but this may produce more defects and holes in the epoxy matrix. Summary of the invention

[0004] In order to solve all or part of the above technical problems, the present invention provides the following technical solutions:

[0005] One of the purposes of the present invention is to provide a method for exfoliating hexagonal boron nitride, comprising: ball milling a mixture containing hexagonal boron nitride and an intercalation agent, wherein the intercalation agent comprises gallic blue.

[0006] The structural formula of the gallic acid blue is as follows:

[0007]

[0008] The present invention adopts gallic blue as an intercalant and cooperates with a ball milling method to obtain a hexagonal boron nitride material (h-BN) sheet material with good dispersion effect, thereby solving the problems of poor h-BN dispersion, easy stacking and difficult dispersion in the coating. The coating formed by dispersing the h-BN obtained by peeling in the resin has a good barrier effect.

[0009] In some embodiments, the method specifically includes: uniformly mixing the hexagonal boron nitride, the intercalation agent and the solvent to form a uniform mixture, and then performing the ball milling treatment on the mixture.

[0010] In some embodiments, the mass ratio of hexagonal boron nitride to gallic blue is 1:1 to 1.5.

[0011] In some embodiments, the ball milling process is performed at a rotation speed of 500 to 800 rpm, for a time of 8 to 10 hours, and the diameter of the grinding balls used is 1.6 mm to 1.8 mm.

[0012] In some embodiments, the grinding balls used in the ball milling process include zirconia ceramic balls, silicon dioxide grinding balls, silicon carbide grinding balls, etc., but are not limited thereto.

[0013] In some embodiments, the thickness of the exfoliated hexagonal boron nitride nanosheets obtained by the method is 5 to 10 nm.

[0014] In some embodiments, the hexagonal boron nitride nanosheets obtained by the method after peeling are in the shape of discs, with a size of 1 to 2 μm and a thickness of 5 to 10 nm.

[0015] The stripping method adopted in the present invention can reduce the thickness of the hexagonal boron nitride layer by about 10 times, and the time required for stripping is relatively short (5 to 8 hours). Compared with other intercalation agents based on non-π action, gallic blue exhibits higher stripping efficiency and good stripping effect.

[0016] The second object of the present invention is to provide a method for preparing a gallic blue-boron nitride hybrid material, comprising ball milling a mixture containing hexagonal boron nitride and gallic blue to obtain a gallic blue-boron nitride hybrid material. In the preparation method, gallic blue is used as an intercalation agent to improve the dispersion effect of h-BN, and on the other hand, the gallic blue molecules in the hybrid material can also be adsorbed on the surface of the substrate, and act as a corrosion inhibitor to play an active protective effect, thereby further improving the anti-corrosion performance of the coating.

[0017] In some embodiments, the mass ratio of hexagonal boron nitride to gallic blue is 1:1 to 1.5.

[0018] In some embodiments, the ball milling process is performed at a rotation speed of 500 to 800 rpm, for a time of 8 to 10 hours, and the diameter of the grinding balls used is 1.6 mm to 1.8 mm.

[0019] In some embodiments, the grinding balls used in the ball milling process include zirconia ceramic balls, silicon dioxide grinding balls, silicon carbide grinding balls, etc., but are not limited thereto.

[0020] In some embodiments, the hexagonal boron nitride, gallic blue and solvent are uniformly mixed to form a uniform mixture, and then the mixture is subjected to the ball milling process.

[0021] In some embodiments, after the ball milling treatment is completed, the ball milling product is subjected to solid-liquid separation, and the solid product obtained by the solid-liquid separation is freeze-dried to obtain a gallic blue-boron nitride hybrid material that can be directly dispersed in a resin. The solid-liquid separation is performed, for example, by centrifugation at a speed of 8000 to 10000 rpm, but is not limited thereto.

[0022] The third object of the present invention is to provide a gallic blue-boron nitride hybrid material obtained according to any one of the preparation methods described.

[0023] The fourth object of the present invention is to provide an anticorrosive coating, comprising: 2500-3000 parts by mass of polyetheramine modified epoxy resin, 15-20 parts by mass of the gallic blue-boron nitride hybrid material, 600-1000 parts by mass of a first polyetheramine and 100 parts by mass of a solvent. The first polyetheramine and the solvent have the function of adjusting the viscosity, so that the anticorrosive coating is convenient for application in engineering and more in line with environmental protection requirements.

[0024] In some embodiments, the first polyetheramine includes one of polyetheramine D230 and polyetheramine D400, or a combination of the two, but is not limited thereto.

[0025] In some embodiments, the solvent includes one or a combination of more than one of benzene, toluene, xylene or propylene glycol monomethyl ether acetate, but is not limited thereto.

[0026] In some embodiments, the raw materials of the polyetheramine-modified epoxy resin include 3000-4000 parts by mass of a base epoxy resin and 1000-1500 parts by mass of a second polyetheramine. Compared with directly using epoxy resin to prepare the coating, the viscosity of the oily epoxy resin is greatly reduced by modifying the epoxy resin with the second polyetheramine, which is convenient for application in engineering and more in line with environmental protection requirements.

[0027] In some embodiments, the base epoxy resin includes epoxy resin E51, epoxy resin E20, epoxy resin E44, etc., but is not limited thereto.

[0028] In some embodiments, the second polyetheramine includes polyetheramine M1000, polyetheramine M2070 or polyetheramine M600, but is not limited thereto.

[0029] In some embodiments, the preparation method of the anti-corrosion coating includes: uniformly mixing the mass parts of the polyetheramine-modified epoxy resin, the gallic blue-boron nitride hybrid material and the solvent to form a suspension, and then uniformly mixing the mass parts of the first polyetheramine with the suspension to form the anti-corrosion coating.

[0030] The fifth object of the present invention is to provide an anti-corrosion coating, which comprises the cured product of the anti-corrosion coating described in any of the above technical solutions.

[0031] In some embodiments, the anti-corrosion coating is applicable to substrates including, but not limited to, steel, aluminum, copper-nickel alloy, and magnesium alloy. The gallic blue in the anti-corrosion coating has a good protective effect on the above substrates, and cooperates with the good dispersion effect of h-BN to synergistically improve the barrier performance of the coating.

[0032] In some embodiments, the thickness of the anti-corrosion coating is 50-100 μm, and the coating within the thickness range can achieve good anti-corrosion effect.

[0033] In some embodiments, the method for forming the anti-corrosion coating includes: coating the anti-corrosion coating on a substrate, standing for 1 to 1.5 hours for pre-curing, and then curing at a temperature of 60 to 100° C. for 24 to 48 hours.

[0034] Compared with the prior art, the present invention has at least the following beneficial effects:

[0035] (1) The present invention uses a gallic blue-assisted ball milling method to achieve the exfoliation of h-BN, and can obtain a hexagonal boron nitride sheet material with good dispersion effect, thereby solving the problem that h-BN is easy to stack and difficult to disperse in the resin;

[0036] (2) The gallic blue-boron nitride hybrid material provided by the present invention can be dispersed in a resin to form a coating with excellent barrier properties. The excellent barrier properties are derived from the good dispersibility of h-BN in the resin. On the other hand, gallic blue can also act as a corrosion inhibitor, which has a protective effect on the substrate and further improves the anti-corrosion performance of the coating.

[0037] (3) The anti-corrosion coating provided by the present invention can still reach a low-frequency impedance of 10 after being immersed in simulated seawater for 105 days. 9 Ωcm 2 , indicating that it can exert excellent and long-lasting anti-corrosion performance in the marine environment and is suitable for marine engineering equipment. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0039] Figure 1 is a SEM image of the h-BN@Gallocyanine hybrid material prepared in one embodiment of the present invention;

[0040] Figure 2 is a SEM image of a cross section of an anti-corrosion coating prepared in one embodiment of the present invention;

[0041] Figure 3a , Figure 3b , Figure 3c They are respectively Nyquist diagrams, Bode diagrams, and Bode-phase angle diagrams of the electrode coated with the modified waterborne epoxy resin in Comparative Example 1 immersed in 3.5wt% NaCl for different time periods;

[0042] Figure 4a , Figure 4b , Figure 4c They are respectively the Nyquist diagram, Bode diagram, and Bode-phase angle diagram of the electrode coated with h-BN / WEP in Comparative Example 2 immersed in 3.5wt% NaCl for different time periods;

[0043] Figure 5a , 5b 5c are the Nyquist diagram, Bode diagram, and Bode-phase angle diagram of the electrode coated with h-BN@Gallocyanine / WEP in Example 1 immersed in 3.5wt% NaCl for different time periods, respectively;

[0044] Figure 6 The salt spray photos of the Q235 steel plates coated with h-BN@Gallocyanine / WEP, simple modified waterborne epoxy resin, and h-BN / WEP in Example 1, Comparative Example 1, and Comparative Example 2 placed in a salt spray spray environment for 0 days, 5 days, 11 days, and 16 days;

[0045] Figure 7 The corrosion morphology electron microscope images of the surface of the Q235 steel plates coated with h-BN@Gallocyanine / WEP, simple modified waterborne epoxy resin, and h-BN / WEP in Example 1, Comparative Example 1, and Comparative Example 2 after being immersed in 3.5wt% NaCl for 105 days;

[0046] Figure 8The local electrochemical impedance spectra of the electrodes coated with h-BN@Gallocyanine / WEP coating, simply modified waterborne epoxy resin, and h-BN / WEP in Example 1, Comparative Example 1, and Comparative Example 2, immersed in 3.5wt% NaCl for 4h, 12h, and 24h;

[0047] Fig. 9 Schematic diagram of exfoliating hexagonal boron nitride nanosheets using gallic blue-assisted ball milling in one embodiment of the present invention. DETAILED DESCRIPTION

[0048] The technical solution of the present invention is described in detail below in conjunction with specific embodiments so that those skilled in the art can better understand and implement the technical solution of the present invention. The specific functional details disclosed herein should not be interpreted as limiting, but only as the basis for the claims and as a representative basis for teaching those skilled in the art to adopt the present invention in different ways in any appropriate detailed embodiment.

[0049] Unless otherwise specified, the raw materials and reagents used in the specific embodiments of the present invention are all commercially available. Unless otherwise specified, the number of parts described in the specific embodiments of the present invention is uniform by weight.

[0050] Example 1

[0051] This embodiment provides a method for exfoliating hexagonal boron nitride nanosheets using a gallic blue-assisted ball milling method and obtaining a gallic blue-intercalated boron nitride hybrid material. Fig. 9 Schematic diagram of exfoliating hexagonal boron nitride nanosheets using gallic blue-assisted ball milling in this embodiment.

[0052] 100 parts by mass of h-BN (hexagonal boron nitride) and 100 parts by mass of gallocyanine were mixed in 2000 parts by mass of water, and then ultrasonically treated for 1 hour to obtain a uniform slurry; then, the uniform slurry was transferred into a stainless steel tank, which was filled with zirconia ceramic balls, the total volume of which accounted for 2 / 3 of the volume of the stainless steel tank, and the diameter of each zirconia ceramic ball was 1.7 mm; then, a planetary ball mill was used to perform ball milling at a speed of 500 revolutions per minute for 5 hours at room temperature; after the ball milling, the obtained mixture was centrifuged at a speed of 8000 rpm for 5 minutes, and the centrifuged product was freeze-dried to remove the solvent to obtain a h-BN hybrid material with gallocyanine intercalation, which was recorded as h-BN@Gallocyanine;

[0053] 3000 parts by mass of epoxy resin E51 and 1000 parts by mass of polyetheramine M2070 were mixed, and the mixture was mechanically stirred for 6 hours to obtain a modified waterborne epoxy resin;

[0054] 15 parts by mass of the h-BN@Gallocyanine prepared above were added to 2500 parts by mass of the modified waterborne epoxy resin prepared above, and 100 parts by mass of benzyl alcohol were added as a solvent, ultrasonic dispersion was performed for 30 minutes, and stirring was performed at room temperature for at least 30 minutes to obtain a uniform suspension; then 600 parts by mass of polyetheramine D230 were added to the above suspension, and stirring was continued at room temperature for 30 minutes to obtain an anti-corrosion coating; thereafter, the prepared anti-corrosion coating was transferred to a preheated vacuum oven to remove bubbles, and pre-cured for 30 minutes to obtain h-BN@Gallocyanine / WEP resin.

[0055] Figure 1 is a SEM image of the h-BN@Gallocyanine hybrid material prepared in Example 1. Compared with the untreated h-BN, the sheet thickness of the h-BN@Gallocyanine hybrid material decreases, and the stacking morphology is significantly reduced. Figure 1 A disc-like structure is presented in the results, proving that the h-BN@Gallocyanine hybrid material was successfully prepared. Figure 2 This is a SEM image of the cross section of the coating formed by coating the above h-BN@Gallocyanine / WEP resin on the Q235 electrode, which shows a dense coating, indicating that the barrier effect is better.

[0056] The h-BN@Gallocyanine / WEP resin was applied to the Q235 electrode using a 50μm wire rod to form an anti-corrosion coating, and the electrode containing the anti-corrosion coating was subjected to relevant electrochemical tests to verify the anti-corrosion performance. The h-BN@Gallocyanine / WEP resin was sprayed evenly onto the Q235 steel plate to form an anti-corrosion coating, and relevant tests were performed on it. The test results are as follows.

[0057] Example 2

[0058] 100 parts by mass of h-BN and 100 parts by mass of gallocyanine were mixed in 2000 parts by mass of water, and then ultrasonically treated for 1 hour to obtain a uniform slurry; then, the uniform slurry was transferred into a stainless steel tank, which was filled with zirconia ceramic balls, the total volume of which accounted for 2 / 3 of the volume of the stainless steel tank, and the diameter of each zirconia ceramic ball was 1.6 mm; then, a planetary ball mill was used to perform ball milling treatment at a speed of 800 revolutions per minute for 8 hours at room temperature; after the ball milling, the obtained mixture was centrifuged at a speed of 8000 rpm for 5 minutes, and the centrifuged product was freeze-dried to remove the solvent to obtain a h-BN hybrid material with gallocyanine intercalation, which was recorded as h-BN@Gallocyanine;

[0059] 4000 parts by mass of epoxy resin E51 and 1000 parts by mass of polyetheramine M2070 were mixed, and the mixture was mechanically stirred for 6 hours to obtain a modified waterborne epoxy resin;

[0060] 20 parts by mass of the h-BN@Gallocyanine prepared above were added to 3000 parts by mass of the modified waterborne epoxy resin prepared above, and 100 parts of xylene were added as a solvent, ultrasonic dispersion was performed for 30 minutes, and stirring was performed at room temperature for at least 30 minutes to obtain a uniform suspension; then 1000 parts by mass of polyetheramine D230 were added to the above suspension, and stirring was continued at room temperature for 30 minutes to obtain an anti-corrosion coating; thereafter, the prepared anti-corrosion coating was transferred to a preheated vacuum oven to remove bubbles, and pre-cured for 30 minutes to obtain h-BN@Gallocyanine / WEP resin.

[0061] Example 3

[0062] 100 parts by mass of h-BN and 150 parts by mass of gallocyanine were mixed in 2000 parts by mass of water, and then ultrasonically treated for 1 hour to obtain a uniform slurry; then, the uniform slurry was transferred into a stainless steel tank, which was filled with zirconia ceramic balls, the total volume of which accounted for 2 / 3 of the volume of the stainless steel tank, and the diameter of each zirconia ceramic ball was 1.8 mm; then, a planetary ball mill was used to perform ball milling at a speed of 700 revolutions per minute for 6 hours at room temperature; after the ball milling, the obtained mixture was centrifuged at a speed of 8000 rpm for 5 minutes, and the centrifuged product was freeze-dried to remove the solvent to obtain a h-BN hybrid material with gallocyanine intercalation, which was recorded as h-BN@Gallocyanine;

[0063] 350 parts by mass of epoxy resin E51 and 100 parts by mass of polyetheramine M2070 were mixed, and the mixture was mechanically stirred for 6 hours to obtain a modified waterborne epoxy resin;

[0064] 17.5 parts by mass of the h-BN@Gallocyanine prepared above were added to 2750 parts by mass of the modified waterborne epoxy resin prepared above, and 100 parts by mass of benzyl alcohol were added as a solvent, ultrasonic dispersion was performed for 30 minutes, and stirring was performed at room temperature for at least 30 minutes to obtain a uniform suspension; then 800 parts by mass of polyetheramine D230 were added to the above suspension, and stirring was continued at room temperature for 30 minutes to obtain an anti-corrosion coating; thereafter, the prepared anti-corrosion coating was transferred to a preheated vacuum oven to remove bubbles, and pre-cured for 30 minutes to obtain h-BN@Gallocyanine / WEP resin.

[0065] Comparative Example 1

[0066] The only difference between Comparative Example 1 and Example 1 is that, in Comparative Example 1, a simple modified water-based epoxy resin is evacuated and then applied to a Q235 electrode using a 50 μm wire rod to form a coating, and the modified water-based epoxy resin is the same as that in Example 1; and the modified water-based epoxy resin is sprayed onto a Q235 steel plate using the same spraying method as in Example 1 to form a coating, and the following anti-corrosion performance test is performed.

[0067] Comparative Example 2

[0068] The only difference between Comparative Example 2 and Example 1 is that, in the preparation of the anticorrosion coating, h-BN without gallocyanine intercalation treatment is used to replace h-BN@Gallocyanine, and the rest is the same as Example 1. The h-BN-based coating is applied to a Q235 electrode to form a coating, and the h-BN-based coating is sprayed onto a Q235 steel plate using the same spraying method as Example 1 to form a coating, which is denoted as h-BN / WEP, and the following anticorrosion performance test is performed.

[0069] Comparative Example 3

[0070] The difference between Comparative Example 3 and Example 1 is that the gallic blue in Example 1 is replaced by aniline trimer, and the preparation method of aniline trimer is:

[0071] Add p-phenylenediamine sulfate (8.87g) and aniline (5.56g) to a three-necked flask containing 1M hydrochloric acid solution (500mL) and cool to -5°C. Slowly drop 150mL of ammonium persulfate (13.62g) in hydrochloric acid (1M) into the above reaction flask through a dropping funnel. After the addition is complete, continue to stir and react for 1h. Filter the reaction product and wash it with a large amount of deionized water to obtain a dark green solid product. Then wash the product with a 10% ammonia solution, and then wash it twice with deionized water. Finally, place the product in a vacuum drying oven at 40°C to dry for use.

[0072] The comparison shows that the exfoliation effect of gallic blue is better. The thickness of the exfoliated gallic blue sheet is reduced by nearly 10 times. Through TEM, it can be observed that compared with the unintercalated boron nitride, the intercalated hybrid material has better dispersion in the resin and less agglomeration. Due to the better barrier properties and the active corrosion protection of the excess gallic blue, the coating with the hybrid material has higher corrosion resistance. Its electrochemical impedance can still reach 10 after immersion for 105 days. 9 Ωcm 2 , while the unfilled resin has dropped to 10 7 Ωcm 2 , the protection has been lost. Since the aniline trimer prepared in Comparative Example 3 does not have active protective performance, the coating of the present invention has better anti-corrosion performance than the coating of Comparative Example 3.

[0073] The present invention conducts the following tests on the prepared gallic blue-boron nitride hybrid material, anticorrosive coating and coating:

[0074] (1) Electrochemical test of h-BN@Gallocyanine / WEP composite coating to verify its anti-corrosion performance: h-BN@Gallocyanine / WEP resin was applied to the electrode using a 50 μm wire rod to form a coating, and the electrode containing the coating was immersed in 3.5 wt% NaCl to test the electrochemical impedance after immersion for 10 days, 30 days, 55 days, 80 days, and 105 days. The coating formed by the modified waterborne epoxy resin in Comparative Example 1 and the h-BN@Gallocyanine prepared in Comparative Example 2 were used as controls.

[0075] Figure 3a , 3b 3c are respectively the Nyquist diagram, Bode diagram, and Bode-phase angle diagram of the electrode coated with the modified waterborne epoxy resin in Comparative Example 1 immersed in 3.5wt% NaCl for different time periods; Figure 4a , 4b 4c are respectively the Nyquist diagram, Bode diagram, and Bode-phase angle diagram of the electrode coated with h-BN / WEP in Comparative Example 2 immersed in 3.5wt% NaCl for different time periods; Figure 5a , 5b 5c are the Nyquist plots, Bode plots, and Bode-phase angle plots of the electrode coated with h-BN@Gallocyanine / WEP in Example 1 immersed in 3.5wt% NaCl for different time periods. By comparing these electrochemical impedance spectra, it can be seen that the coating with h-BN@Gallocyanine filler has the best anti-corrosion performance. Its low-frequency impedance can still reach 10 after being immersed in simulated seawater for 105 days. 9 Ωcm 2 The impedance of the coating with unintercalated original boron nitride remained at 10 after 105 days of immersion. 8 Ωcm 2 In contrast, the low-frequency impedance of the epoxy resin without filler has dropped to 10 after 105 days of immersion. 7 Ωcm 2 This shows that the addition of boron nitride increases the barrier properties of the coating, and the intercalated boron nitride of gallocyanine significantly enhances the barrier properties of the coating, so the anti-corrosion properties of the coating based on the h-BN@Gallocyanine hybrid material are greatly improved.

[0076] (2) Salt spray test of h-BN@Gallocyanine / WEP composite coating To verify its long-term anticorrosion performance, the coating samples were subjected to salt spray test according to GB6458-86: h-BN@Gallocyanine / WEP resin was sprayed evenly onto Q235 steel plate to form a coating, a 3mm long scratch was introduced on the coating surface with a scalpel, and the steel plate containing the coating was placed in a 5wt% salt spray environment for several days. The modified waterborne epoxy resin of Comparative Example 1 and the coating formed by preparing h-BN@Gallocyanine in Comparative Example 2 were used as controls.

[0077] Figure 6 The following are salt spray photos of Q235 steel plates coated with h-BN@Gallocyanine / WEP coating, simple modified waterborne epoxy resin, and h-BN / WEP coating in Example 1, Comparative Example 1, and Comparative Example 2 after being placed in a salt spray environment for 0 days, 5 days, 11 days, and 16 days. Figure 6 It can be seen that compared with the simple modified water-based epoxy resin and h-BN / WEP coating, the h-BN@Gallocyanine / WEP coating in Example 1 did not show obvious corrosion at the scratches in a long-term salt spray environment, and its barrier performance was better than that of the coatings in Comparative Examples 1 and 2.

[0078] (3) Electron microscope image of the corrosion morphology of the steel block surface after immersion for 105 days under the protection of h-BN@Gallocyanine / WEP composite coating. The h-BN@Gallocyanine / WEP resin was sprayed evenly onto the Q235 steel plate to form a coating, and the steel block containing the coating was immersed in 3.5wt% NaCl for 105 days. The epoxy ab glue encapsulating the outside of the steel block was peeled off, and the corrosion morphology of the steel block surface was observed using a scanning electron microscope. The coating formed by the water-based epoxy resin modified in Comparative Example 1 and the h-BN@Gallocyanine in Comparative Example 2 were used as controls.

[0079] Figure 7The corrosion morphology electron microscope images of the surface of Q235 steel plates coated with h-BN@Gallocyanine / WEP coating, simple modified waterborne epoxy resin, and h-BN / WEP coating in Example 1, Comparative Example 1, and Comparative Example 2 after being immersed in 3.5wt% NaCl for 105 days are shown. By comparison, it can be seen that a large amount of corrosion products are accumulated on the surface of the coating without adding fillers, indicating that the corrosive medium has reached the substrate and a corrosion reaction has occurred, while the accumulation of corrosion products coated with h-BN / WEP coating is significantly reduced, indicating that the addition of boron nitride has a certain effect of blocking the corrosive medium. However, there is basically no accumulation of corrosion products on the surface coated with h-BN@Gallocyanine / WEP coating, and the scratches of the grinding are clearly visible, which has the best corrosion protection effect.

[0080] (4) Local electrochemical impedance test of h-BN@Gallocyanine / WEP composite coating to verify its dynamic protection performance. A scalpel was used to introduce a scratch of about 2 mm in length on the surface of the h-BN@Gallocyanine / WEP coating, and the local electrochemical impedance was tested after immersion in 3.5wt% NaCl for different times. The coating formed by the modified waterborne epoxy resin of Comparative Example 1 and the h-BN@Gallocyanine prepared in Comparative Example 2 were used as controls.

[0081] Figure 8 The local electrochemical impedance spectra of the electrodes coated with h-BN@Gallocyanine / WEP coating, simple modified waterborne epoxy resin, and h-BN / WEP in Example 1, Comparative Example 1, and Comparative Example 2, immersed in 3.5wt% NaCl for 4h, 12h, and 24h are shown. The impedance of the epoxy coating without filler decreases rapidly with the immersion time, and the corrosion area rapidly expands along the scratch to the surrounding area. In contrast, the corrosion of the h-BN@Gallocyanine / WEP coating expands most slowly with the extension of the immersion time, and a slight upward trend in the impedance at the scratch can be observed from 4 to 12 hours, indicating that the residual gallic blue molecules have good active corrosion inhibition ability.

[0082] The effects of the above-mentioned Embodiment 2 and Embodiment 3 are equivalent to those of Embodiment 1.

[0083] The various aspects, embodiments, features and examples of the present invention should be considered as illustrative in all aspects and are not intended to limit the present invention, the scope of the present invention is defined only by the claims. Other embodiments, modifications and uses will be apparent to those skilled in the art without departing from the spirit and scope of the claimed invention.

[0084] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.

[0085] Although the present invention has been described with reference to illustrative embodiments, it will be appreciated by those skilled in the art that various other changes, omissions and / or additions may be made without departing from the spirit and scope of the present invention and that the elements of the embodiments may be replaced by substantial equivalents. In addition, many modifications may be made without departing from the scope of the present invention to adapt specific circumstances or materials to the teachings of the present invention. Therefore, it is not intended herein to limit the present invention to the disclosed specific embodiments for performing the present invention, but it is intended that the present invention will include all embodiments within the scope of the appended claims. In addition, unless specifically stated, any use of the terms first, second, etc. does not indicate any order or importance, but rather uses the terms first, second, etc. to distinguish one element from another.

Claims

1. A method for exfoliating hexagonal boron nitride, characterized in that: include: A mixture containing hexagonal boron nitride and an intercalation agent is ball-milled, wherein the intercalation agent comprises gallic blue.

2. The method for exfoliating hexagonal boron nitride according to claim 1, characterized in that: include: The hexagonal boron nitride, the intercalation agent and the solvent are uniformly mixed to form a uniform mixture, and then the mixture is subjected to the ball milling treatment; And / or, the mass ratio of hexagonal boron nitride to gallic blue is 1:1-1.5; And / or, the rotation speed of the ball milling treatment is 500-800 rpm, the time is 5-8 hours, and the diameter of the grinding balls used is 1.6 mm-1.8 mm; And / or, the thickness of the hexagonal boron nitride after exfoliation obtained by the method is 5 to 10 nm.

3. A method for preparing a gallic blue-boron nitride hybrid material, characterized in that: The method comprises subjecting a mixture containing hexagonal boron nitride and gallic blue to ball milling to obtain a gallic blue-boron nitride hybrid material.

4. The preparation method according to claim 3, characterized in that: The mass ratio of hexagonal boron nitride to gallic blue is 1:1-1.5; And / or, the rotation speed of the ball milling treatment is 500-800 rpm, the time is 5-8 hours, and the diameter of the grinding balls used is 1.6 mm-1.8 mm; and / or, uniformly mixing the hexagonal boron nitride, gallic blue and solvent to form a uniform mixture, and then subjecting the mixture to the ball milling treatment; And / or, the method further comprises performing solid-liquid separation on the product obtained by ball milling, and freeze-drying the gallic blue-boron nitride hybrid material obtained by the solid-liquid separation.

5. The gallic blue-boron nitride hybrid material obtained according to the preparation method according to claim 3 or 4.

6. A gallic blue-boron nitride hybrid material, characterized in that: It includes hexagonal boron nitride sheet material and gallic blue combined with the hexagonal boron nitride sheet material; Preferably, the mass ratio of hexagonal boron nitride to gallic blue in the gallic blue-boron nitride hybrid material is 1:1 to 1.

5.

7. An anticorrosive coating, characterized in that: include: 2500-3000 parts by mass of a polyetheramine-modified epoxy resin, 15-20 parts by mass of the gallic blue-boron nitride hybrid material according to any one of claims 5-6, 600-1000 parts by mass of a first polyetheramine and 100 parts by mass of a solvent.

8. The anticorrosive coating according to claim 7, characterized in that: The first polyetheramine includes one or a combination of polyetheramine D230 and polyetheramine D400; And / or, the raw materials of the polyetheramine-modified epoxy resin include 3000-4000 parts by mass of a base epoxy resin and 1000-1500 parts by mass of a second polyetheramine; And / or, the solvent includes one or a combination of more than one of benzene, toluene, xylene or propylene glycol monomethyl ether acetate.

9. The anticorrosive coating according to claim 8, characterized in that: The matrix epoxy resin includes one or more of epoxy resin E51, epoxy resin E20, and epoxy resin E44; And / or, the second polyetheramine includes one or a combination of polyetheramine M1000, polyetheramine M2070 or polyetheramine M600.

10. An anti-corrosion coating, characterized in that: A cured product comprising the anticorrosive coating according to any one of claims 7 to 9.

Citation Information

Patent Citations

  • Epoxy resin and boron nitride nanocomposite and preparation method thereof

    CN107033539A

  • Gallic acid intercalated zinc-aluminum hydrotalcite anticorrosive filler as well as preparation method and application thereof

    CN116770298A

  • Hydrophilic boron nitride nanosheet as well as preparation method and application thereof

    CN118221079A

  • process for applying a resist to goods to be dyed with chromium-intensive dyes, such as gallocyanins, leucogallocyanins, bisulphite gallocyanins, bisulphite alizarin blue, bisulphite cerulein, etc., with the addition of a chrome mordant

    FR481867A

  • Hexagonal Boron Nitride Epoxy Compound Anticorrosive Paint, and Preparation Method and Use Thereof

    US20200095432A1