Protective coating as well as preparation method and application thereof
Through specific proportions of chemical raw materials and spraying processes, protective coatings with good mechanical strength, corrosion resistance and antistatic properties are prepared, which solves the problems of complexity of traditional coating processes and insufficient protection, and realizes the application of multiple models of spacecraft efficient protection effect.
Patent Information
- Application Number
- CN202411128979.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-19
AI Technical Summary
The protective coating of traditional spacecraft coats is complex and has limited protection. It is difficult to be suitable for applications of multiple spacecraft models, and it lacks good mechanical strength, corrosion resistance and antistatic properties.
Protective coatings made of isocyanate, amino resin, chain extender, anti-mold agent, defoaming agent, light stabilizer and antistatic agent in a specific proportion, form coatings through mixing and spraying processes, combining high-speed dispersers and thermal spraying Curing technology to achieve rapid curing and good adhesion of the coating.
It provides a coating with good weather resistance, anti-static properties and anti-collision. It has a wide range of applications, is easy to construct and is easy to tear. It replaces the traditional protection method of tinting polytetrafluoroethylene film to ensure that the elastic body is not subject to wear and corrosion. and oxidative effects.
Smart Images

Figure CN118978854A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of coatings, and in particular to a protective coating and a preparation method and application thereof. Background Art
[0002] As a strategic weapon, the leakage of spacecraft may lead to various accidents during transportation and storage, such as oxidation, corrosion, impact, etc. Therefore, in order to ensure the service life and safety performance of the spacecraft, it is extremely important to protect the spacecraft. The antistatic protective coating of the spacecraft outer coat can protect the surface of the missile body and avoid static electricity caused by the removal of the coating. However, the traditional protective coating process of the outer coat of the spacecraft is complicated and the degree of protection is limited, which is not suitable for large-scale and multi-model applications. The development of protective coatings suitable for the outer coats of multiple models of spacecraft is one of the current efficient technologies for the protection of spacecraft.
[0003] Chinese patent CN214842773U discloses a gas phase anti-rust coat, which mainly adopts the outer part of the spacecraft body to be provided with anti-rust coat 1 and anti-rust coat 2, which is used to solve the overall shielding protection of the spacecraft. However, due to the many operation procedures of the gas phase anti-rust coat and the limited protection degree, the performance of the spacecraft surface coating is affected. Summary of the invention
[0004] The purpose of the present invention is to provide a protective coating with suitable mechanical strength, good corrosion resistance and antistatic properties, fast coating curing, strong design, and tearable operation, which can meet the performance requirements of aerospace vehicle outer coatings in many aspects.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a protective coating, which is made of the following raw materials in parts by weight:
[0007] 40-55 parts of isocyanate, 40-50 parts of amino resin, 5-10 parts of chain extender, 1-2 parts of mildewproof agent, 0.5-1 part of defoamer, 5-10 parts of antistatic agent, 1-2 parts of light stabilizer, and 80-300 parts of diluent.
[0008] Preferably, the isocyanate is an aliphatic isocyanate and / or an aromatic isocyanate.
[0009] Preferably, the amino resin is an amino-terminated polyether.
[0010] Preferably, the chain extender is selected from isophorone diamine, Clearlink TM Series of fatty amines, Versalink TMOne or more of a series of fatty amines.
[0011] Preferably, the mildew inhibitor is 8-hydroxyquinolinone and / or tributyltin oxide.
[0012] Preferably, the defoaming agent is selected from one or more of isopropyl alcohol, silicone resin and oleic acid.
[0013] Preferably, the antistatic agent is imidazole bis(trifluoromethanesulfonyl)imide salt.
[0014] Preferably, the light stabilizer is a benzotriazole ultraviolet absorber.
[0015] The present invention also provides a method for preparing the protective coating, comprising the following steps:
[0016] Mixing the other components except isocyanate to obtain solution A;
[0017] The solution A is mixed with isocyanate and a diluent to obtain the protective coating.
[0018] The present invention also provides the use of the protective coating in preparing aerospace vehicle outerwear, oil storage and transportation equipment coatings, and floor coatings.
[0019] Beneficial effects of the present invention:
[0020] The protective coating provided by the present invention uses isocyanate, amino resin, chain extender, mildewproof agent, defoamer, light stabilizer, and antistatic agent as raw materials in a specific ratio. The prepared protective coating has the characteristics of good weather resistance, antistatic property, anti-collision, wide application range, convenient construction, and easy tearing and removal. It can replace the current conventional protective method of wrapping the "outer coat" of aerospace vehicles with polytetrafluoroethylene film. The protective coating can ensure that the projectile is not affected by wear, corrosion, oxidation, etc., and the protective coating and the substrate achieve a balance between adhesion and peelability, which is more convenient to use. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a photograph of the surface state of the coating of the present invention after spraying. DETAILED DESCRIPTION
[0022] The present invention provides a protective coating, which is made of the following raw materials in parts by weight:
[0023] 40-55 parts of isocyanate, 40-50 parts of amino resin, 5-10 parts of chain extender, 1-2 parts of mildewproof agent, 0.5-1 part of defoamer, 5-10 parts of antistatic agent, 1-2 parts of light stabilizer, and 80-300 parts of diluent.
[0024] In the present invention, the isocyanate is preferably an aliphatic isocyanate and / or an aromatic isocyanate, and more preferably an aliphatic isocyanate; the amino resin is preferably an amino-terminated polyether; the chain extender is preferably selected from isophorone diamine, Clearlink TM Series of fatty amines, Versalink TM The invention discloses a novel polyol-based polyol, wherein the polyol-based polyol is selected from one or more of a series of fatty amines; the mildew inhibitor is 8-hydroxyquinolinone and / or tributyltin oxide; the defoamer is preferably selected from one or more of isopropyl alcohol, silicone resin, and oleic acid; the antistatic agent is preferably imidazole bistrifluoromethanesulfonyl imide salt; and the light stabilizer is preferably a benzotriazole ultraviolet absorber.
[0025] The present invention also provides a method for preparing the above-mentioned protective coating, comprising the following steps: mixing the other components except isocyanate to obtain solution A; mixing solution A with isocyanate and a diluent to obtain the protective coating; the mixing is preferably carried out using a high-speed disperser, the mixing speed is preferably 1000-1500 r / min, and the mixing time is preferably 0.5-2h.
[0026] The present invention also provides the use of the above-mentioned protective coating in the preparation of aerospace vehicle outerwear, oil storage and transportation equipment coatings, and floor coatings. The protective coating is preferably applied by spraying. The spraying environment temperature is preferably 18-30°C, and the relative air humidity is preferably less than 50%. The spraying is preferably performed by thermal spraying with 1.0MPa compressed air. After 4 hours after spraying, the coating is preferably cured in a dust-free spray room at a temperature not higher than 45°C to obtain a protective coating.
[0027] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0028] The main raw materials used in the examples are purchased from the following sources:
[0029] Isocyanate was purchased from Wanhua Chemical Group Co., Ltd.; brand HT-600;
[0030] Amino resin was purchased from Zhuhai Feiyang New Materials Co., Ltd.; the brand number is F520.
[0031] Example 1
[0032] Raw materials: 40 parts of isocyanate, 40 parts of amino resin, chain extender Clearlink TM 5 parts of series fatty amines, 1 part of mildew preventer 8-hydroxyquinolinone, 0.5 parts of defoamer silicone resin, 5 parts of antistatic agent imidazole bistrifluoromethanesulfonyl imide salt, 1 part of light stabilizer benzotriazole ultraviolet absorber.
[0033] A chain extender, a mildew preventer, a defoamer, an antistatic agent and a light stabilizer are sequentially added to the amino resin, and mixed in a high-speed disperser at a speed of 800 r / min for 0.5 h to form a mixed solution, which is component A.
[0034] Isocyanate is used as the B component.
[0035] The component A: ethyl acetate diluent: component B were mixed in a mass ratio of 1:1:1.5 in a high-speed disperser with a rotation speed of 1000 r / min for 15 minutes to obtain a protective coating.
[0036] Example 2
[0037] Raw materials: 45 parts of isocyanate, 50 parts of amino resin, 8 parts of chain extender isophorone diamine, 1 part of mildew inhibitor 8-hydroxyquinolinone, 0.5 parts of defoamer silicone resin, 8 parts of antistatic agent imidazole bis trifluoromethanesulfonyl imide salt, 2 parts of light stabilizer benzotriazole ultraviolet absorber.
[0038] Chain extender, mildewproof agent, defoamer, antistatic agent and light stabilizer were added to the amino resin in sequence, and mixed in a high-speed disperser for 0.5 hours at a speed of 1000 r / min to form a mixed solution, which is component A. Isocyanate is component B. Component A: ethyl acetate diluent: component B = 1:1:1.5 mass ratio, and mixed in a high-speed disperser for 15 minutes at a speed of 1200 r / min to obtain a protective coating.
[0039] Example 3
[0040] Raw materials: 45 parts of isocyanate, 50 parts of amino resin, 10 parts of chain extender isophorone diamine, 1 part of mildew preventer 8-hydroxyquinolinone, 1 part of defoamer isopropyl alcohol, 8 parts of antistatic agent imidazole bis trifluoromethanesulfonyl imide salt, 1 part of light stabilizer benzotriazole ultraviolet absorber.
[0041] Chain extender, mildewproof agent, defoamer, antistatic agent and light stabilizer were added to the amino resin in sequence, and mixed in a high-speed disperser at a speed of 1000 r / min for 1.0 h to form a mixed solution, which is component A. Isocyanate is component B. Component A: ethyl acetate diluent: component B = 1:1:1.5 mass ratio, and mixed in a high-speed disperser at a speed of 1200 r / min for 15 min to obtain a protective coating.
[0042] Comparative Example 1
[0043] The only difference from Example 1 is that the raw materials do not contain defoaming agent and chain extender.
[0044] Comparative Example 2
[0045] The only difference from Example 2 is that the raw materials do not contain an antistatic agent.
[0046] Comparative Example 3
[0047] The only difference from Example 2 is that the raw materials do not contain mildew inhibitors and light stabilizers.
[0048] Comparative Example 4
[0049] The only difference from Example 1 is that the amount of isocyanate is replaced by 60 parts.
[0050] The antistatic protective coating materials prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were subjected to the following performance tests, and the test results are shown in Table 1.
[0051] Table 1 Coating performance test results
[0052]
[0053]
[0054] As shown in Table 1, the coating provided by the present invention has a tensile strength of 1.0-2.5 MPa, a tear elongation of 200-250%, has suitable mechanical strength, is easy to tear, and has a surface resistivity of 10 5 ~10 8 Ω·cm, excellent antistatic effect.
[0055] The coating provided in Example 1 of the present invention is thermally sprayed onto a substrate test plate (the material of the substrate test plate is aluminum / carbon fiber) using 1.0 MPa compressed air under the conditions of an ambient temperature of 20°C and an air relative humidity of 30%. After spraying, the coating is heated and cured in a dust-free spray room at 30°C for 4 hours to obtain a protective coating for the outer shell of a spacecraft.
[0056] After spraying, record the apparent state, such as Figure 1 As shown;
[0057] Depend on Figure 1 It can be seen that the coating provided by the present invention is closely attached to the substrate after spraying, has no pores, and has excellent surface effect.
[0058] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A protective coating, It is characterized in that Made from the following raw materials in parts by weight: 40-55 parts of isocyanate, 40-50 parts of amino resin, 5-10 parts of chain extender, 1-2 parts of mildewproof agent, 0.5-1 part of defoamer, 5-10 parts of antistatic agent, 1-2 parts of light stabilizer, and 80-300 parts of diluent.
2. The protective coating according to claim 1, It is characterized in that The isocyanate is an aliphatic isocyanate and / or an aromatic isocyanate.
3. The protective coating according to claim 1, It is characterized in that The amino resin is an amino-terminated polyether.
4. The protective coating according to claim 1, It is characterized in that The chain extender is selected from isophorone diamine, Clearlink TM Series of fatty amines, Versalink TM One or more of a series of fatty amines.
5. The protective coating according to claim 1, It is characterized in that The mildew preventer is 8-hydroxyquinolinone and / or tributyltin oxide.
6. The protective coating according to claim 1, It is characterized in that The defoaming agent is selected from one or more of isopropyl alcohol, silicone resin and oleic acid.
7. The protective coating according to claim 1, It is characterized in that The antistatic agent is imidazole bis(trifluoromethanesulfonyl)imide salt.
8. The protective coating according to claim 1, It is characterized in that The light stabilizer is a benzotriazole ultraviolet absorber.
9. The method for preparing the protective coating according to any one of claims 1 to 8, It is characterized in that The following steps are involved: Mixing the other components except isocyanate to obtain solution A; The solution A is mixed with isocyanate and a diluent to obtain the protective coating.
10. Use of the protective coating according to any one of claims 1 to 8 in the preparation of aerospace vehicle outerwear, oil storage and transportation equipment coatings, and floor coatings.
Citation Information
Patent Citations
Anti-static wear-resistant polyurea elastomer paint and preparation method thereof
CN108264830A
Short-term protective polyurethane urea coating as well as preparation and use methods thereof
CN114854291A
Strippable anticorrosive paint for friction surface of high-strength bolt
CN114921161A
Solvent-free peelable efficient protective material and preparation method thereof
CN117567934A
Sealing protective coating as well as preparation method and application thereof