Method for improving wear resistance of alloy surface

By performing high-temperature and high-pressure borication treatment in a vacuum environment, the boron elements in the boron dehydrator layer are used to form metal borides and refined grains, which solves the contradiction between the surface hardness and internal toughness of the alloy and significantly improves the resistance of the alloy Grinding performance and life.

CN118979219AActive Publication Date: 2024-11-19SOUTHERN UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410909441.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-19
Estimated Expiration
2044-07-08

AI Technical Summary

Technical Problem

The prior art is difficult to maintain its internal toughness while improving the surface hardness of the alloy, resulting in the material being prone to cracks and fatigue fractures during repeated wear, reducing wear resistance.

Method used

The alloy is placed under high temperature and high pressure conditions in a vacuum environment for boronization treatment. The boron element in the boron dehydrant layer reacts with the alloy to form a variety of metal borides, fine the alloy grains, and form a layered structure to improve the surface Hardness and wear resistance.

Benefits of technology

Effectively improve the wear resistance of the alloy surface, increase its life, while maintaining the toughness inside the alloy to avoid fatigue and fracture.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979219A_ABST
    Figure CN118979219A_ABST
Patent Text Reader

Abstract

The invention discloses a method for improving alloy surface wear resistance and belongs to the field of alloy surface treatment. The method for improving the wear resistance of the alloy surface comprises the steps that the alloy with the boronizing agent layer laid on the surface is placed in a vacuum environment, the temperature is increased to the preset temperature, and boronizing treatment is conducted under the condition that the preset temperature and the preset pressure are kept; wherein the alloy contains transition metal elements, the preset pressure ranges from 30 MPa to 60 MPa, and the preset temperature ranges from 950 DEG C to 1200 DEG C. By boronizing the alloy and the boronizing agent layer at high temperature and high pressure, the wear resistance of the alloy surface can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of alloy surface treatment, and in particular to a method for improving the wear resistance of an alloy surface. Background Art

[0002] Improving the wear resistance of metal alloys can increase the life of friction and wear parts, such as aircraft turbine blades, artificial implant joints, etc. In general, increasing the surface hardness of a material can improve its wear resistance. However, increasing the hardness of a material often reduces its toughness, which in turn causes cracks on the subsurface of the material during repeated wear, leading to fatigue fracture of the material and reducing its wear resistance.

[0003] Therefore, how to effectively improve the wear resistance of the alloy surface is a technical problem that needs to be solved urgently. Summary of the invention

[0004] The present application provides a method for improving the wear resistance of an alloy surface, which can improve the hardness of the alloy surface without substantially affecting the toughness inside the alloy, thereby effectively improving the wear resistance of the alloy surface.

[0005] The embodiment of the present application is implemented as follows:

[0006] The present application example provides a method for improving the wear resistance of an alloy surface, which comprises the following steps:

[0007] The alloy with a boronizing agent layer on the surface is placed in a vacuum environment, heated to a preset temperature, and subjected to a boriding treatment under the conditions of maintaining the preset temperature and the preset pressure;

[0008] Among them, the alloy contains transition metal elements, the preset pressure is 30MPa-60MPa, and the preset temperature is 950℃-1200℃.

[0009] The method for improving the wear resistance of the alloy surface provided in the present application, by reacting the alloy with a boriding agent layer under high temperature and high pressure, can not only make the boron element penetrate into the metal crystal structure to form a variety of metal borides on the alloy surface, and effectively improve the wear resistance of the alloy by compounding a variety of metal borides, but also can effectively refine the alloy grains, making the alloy grain size more uniform to improve the surface hardness and wear resistance of the alloy, and at the same time, the wear-resistant layer forms a layered structure on the sub-surface, further improving the wear resistance of the alloy without affecting the toughness inside the alloy.

[0010] In some embodiments, the preset temperature is 950°C-1100°C.

[0011] In some embodiments, the boronization treatment time is 5 min-60 min.

[0012] In some embodiments, the boronization treatment time is 10 min-20 min.

[0013] In some embodiments, the step of increasing the temperature includes:

[0014] First, the temperature is raised to 600°C at a heating rate of 80°C / min-110°C / min and a heating time of 5.5-6.5min;

[0015] Then, the temperature is raised to 900°C at a heating rate of 80°C / min-120°C / min and a heating time of 2.5-3.8min;

[0016] Finally, the temperature is raised to the preset temperature at a heating rate of 40°C / min-80°C / min and a heating time of 2-4min.

[0017] In some embodiments, the boronizing agent layer includes a boronizing agent, and the boronizing agent includes a powdered B 4 One or more of C, BN, and amorphous boron.

[0018] In some embodiments, the boriding agent layer is composed of powdered amorphous boron.

[0019] In some embodiments, the alloy includes FCC phase, Kappa phase and V 2 O 3 The chemical formula of the Kappa phase is (Co, Ni) 3 V.

[0020] In some embodiments, the thickness of the boriding agent layer is ≥ 1 mm.

[0021] In some embodiments, the particle size of the boronizing agent is ≤ 1 μm. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0023] Figure 1 XRD diagram of the VCoNi medium entropy alloy before and after boriding treatment in Example 1 of the present application;

[0024] Figure 2 This is a schematic diagram of the performance of an alloy sample having a wear-resistant layer on the surface obtained after boronization treatment in Example 1 of the present application;

[0025] Figure 3 This is a schematic diagram of wear comparison between Example 1 of the present application and Comparative Example 1;

[0026] Figure 4 This is a schematic diagram comparing the hardness tests of Examples 1-4 and Comparative Example 1 of the present application. DETAILED DESCRIPTION

[0027] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0028] The following is a specific description of the method for improving the wear resistance of the alloy surface according to the embodiment of the present application:

[0029] The present application provides a method for improving the wear resistance of an alloy surface, which comprises the following steps:

[0030] The alloy with a boronizing agent layer on the surface is placed in a vacuum environment, heated to a preset temperature, and subjected to a boriding treatment under the conditions of maintaining the preset temperature and the preset pressure;

[0031] Among them, the alloy contains transition metal elements, the preset pressure is 30MPa-60MPa, and the preset temperature is 950℃-1200℃.

[0032] It is understood that the boronizing agent layer is used to provide the boron element.

[0033] The vacuum environment avoids interfering impurities during the boronization process.

[0034] The transition metal elements are used to react with the boron element in the boriding agent layer under high temperature and high pressure conditions, thereby generating a wear-resistant layer containing borides on its surface through boriding treatment, thereby greatly enhancing the hardness and wear resistance of the alloy surface. The hardness of the wear-resistant layer decreases from the outside to the inside with increasing depth from the surface. Therefore, the toughness of the alloy will not be greatly reduced while increasing the wear resistance of the alloy surface.

[0035] The boriding treatment is carried out under the condition of a preset temperature of 950℃-1200℃. The alloy surface can be recrystallized and the alloy grains can be refined through heat treatment, which plays a role of fine grain strengthening, thereby effectively improving the hardness and wear resistance of the alloy.

[0036] Exemplarily, the preset temperature is any value of 950°C, 975°C, 1000°C, 1025°C, 1050°C, 1075°C, 1100°C, 1125°C, 1150°C, 1175°C, 1200°C or between any two values.

[0037] The preset pressure used in the controlled boriding treatment is 30MPa-60MPa. By applying pressure to the surface, the residual compressive stress on the alloy surface is increased, causing local plastic deformation around the grain boundary, thereby further promoting grain refinement and reducing the grain size, thereby effectively improving the hardness and wear resistance of the alloy.

[0038] Exemplarily, the preset pressure is any value among 30 MPa, 35 MPa, 40 MPa, 45 MPa, 50 MPa, 55 MPa, 60 MPa or between any two values.

[0039] The boronization treatment can be performed in a furnace that meets the above-mentioned high temperature, high pressure and vacuum environment. For example, the boronization treatment can be performed in an SPS plasma spark sintering furnace.

[0040] In summary, the present application adopts the above-mentioned method, by reacting the alloy with the boriding agent layer under high temperature and high pressure, which not only enables the boron element to penetrate into the metal crystal structure and form a variety of metal borides on the alloy surface, and effectively improves the wear resistance of the alloy through the compounding of multiple metal borides, but also effectively refines the alloy grains, making the alloy grain size more uniform to improve the surface hardness and wear resistance of the alloy. At the same time, the wear-resistant layer forms a layered structure on the sub-surface, further improving the wear resistance of the alloy without affecting the toughness inside the alloy.

[0041] In some optional embodiments, the preset temperature is 950°C-1100°C.

[0042] Controlling the preset temperature of the boriding treatment within the above range is beneficial to improving the wear resistance of the alloy.

[0043] Exemplarily, the preset temperature is any value among 950° C., 1000° C., 1050° C., 1100° C., or between any two values.

[0044] The time of the boronization treatment is greater than 0. Since the thickness of the wear-resistant layer is related to the time of the boronization treatment, the time of the boronization treatment can be selected according to actual needs.

[0045] In some optional embodiments, the boronization treatment time is 5 min-60 min.

[0046] Within the above-mentioned boronization treatment time range, the thickness of the obtained wear-resistant layer is good and meets most usage requirements.

[0047] Exemplarily, the time of the boronization treatment is any value among 5 min, 10 min, 20 min, 30 min, 40 min, 50 min, 60 min, or between any two values.

[0048] Optionally, the boronization treatment time is 10 min-20 min.

[0049] Within the above time range, the thickness of the obtained wear-resistant layer can be greater than 100 μm, and the wear-resistant effect is good.

[0050] Exemplarily, the time of the boronization treatment is any value among 10 min, 13 min, 15 min, 18 min, 20 min, or between any two values.

[0051] In some optional embodiments, the step of heating includes:

[0052] First, the temperature is raised to 600°C at a heating rate of 80°C / min-110°C / min and a heating time of 5.5-6.5min;

[0053] Then, the temperature is raised to 900°C at a heating rate of 80°C / min-120°C / min and a heating time of 2.5-3.8min;

[0054] Finally, the temperature is raised to the preset temperature at a heating rate of 40°C / min-80°C / min and a heating time of 2-4min.

[0055] Heating rate refers to the rate at which the alloy temperature increases from the initial temperature to the preset temperature.

[0056] The above three-step heating method is beneficial to improving the diffusion uniformity of boron atoms.

[0057] For example, the temperature is first raised to 600° C. at a heating rate of 80° C. / min-110° C. / min and a heating time of 6 min;

[0058] Then, the temperature was raised to 900°C at a heating rate of 80°C / min-120°C / min and a heating time of 3 min;

[0059] Finally, the temperature was raised to the preset temperature at a heating rate of 40°C / min-80°C / min and a heating time of 2 min.

[0060] It should be noted that in the three heating stages in the present application, the heating rate of each heating stage remains constant, so in the actual operation process, it is only necessary to determine the temperature difference before and after the heating and limit the heating time.

[0061] It should be noted that the boronizing agent layer includes but is not limited to a boronizing agent, and may also include an activator KBF 4 Etc., can be selected according to actual needs.

[0062] In some optional embodiments, the boronizing agent layer includes a boronizing agent, and the boronizing agent includes powdered B 4 One or more of C, BN, and amorphous boron.

[0063] The above-mentioned boronizing agents can all be used to boronize the surface of the alloy to improve the hardness and wear resistance of the alloy surface.

[0064] In some optional embodiments, the boriding agent layer is composed of powdered amorphous boron.

[0065] That is, the boriding agent layer is composed of only amorphous boron. By selecting the boriding agent layer to be composed of powdered amorphous boron, it is helpful to avoid interference of foreign phases and to improve the hardness and wear resistance of the alloy surface.

[0066] The alloy containing a transition metal element means that the alloy is an alloy consisting of the above transition metal element, or an alloy consisting of the above transition metal element and a non-transition metal element.

[0067] Among them, the transition metal elements include but are not limited to one or more of Fe, Co, Ni, Mg, Al, Cu, Zn, Ti, Zr, Ta, Nb, W, Cr, V and Mn.

[0068] In recent years, medium-entropy alloys, as an important branch of high-entropy alloys, have attracted widespread attention in the field of materials science. Compared with traditional alloys and high-entropy alloys, medium-entropy alloys have more flexible elemental composition and easier to control alloy design. VCoNi isoatomic ratio multi-principal alloys are promising materials due to their excellent mechanical properties, corrosion resistance and high-temperature stability, such as aviation turbine blades. However, the wear resistance of this alloy is currently inferior to that of traditional titanium alloys such as Ti 6 Al 4 V alloy, so the wear resistance needs to be improved, which limits the application of this alloy.

[0069] In some optional embodiments, the alloy includes FCC phase, Kappa phase and V 2 O 3 The chemical formula of the Kappa phase is (Co, Ni) 3 V.

[0070] The above-mentioned medium-entropy alloy has excellent mechanical properties, corrosion resistance and high-temperature stability, and has broad application prospects. At the same time, after the medium-entropy alloy is modified in the above manner, the alloy grain size can be made more uniform while refining the alloy grains, and a V-rich phase can be precipitated, and a gradient metal boride (cobalt boride, nickel boride, etc.) can be formed, which is beneficial to improve the wear resistance of the alloy and further expand its application prospects.

[0071] In some optional embodiments, the thickness of the boronizing agent layer is ≥ 1 mm.

[0072] Controlling the thickness within the above range is beneficial to providing sufficient boron atoms for boriding treatment.

[0073] Optionally, the thickness of the boronizing agent layer is 1 mm-1 cm.

[0074] In some optional embodiments, the particle size of the boronizing agent is ≤1 μm.

[0075] Controlling the particle size of the boronizing agent to ≤1μm is beneficial to ensuring the uniformity of the boronizing of the boronizing agent layer.

[0076] The method for improving the wear resistance of the alloy surface of the present application is further described in detail below in conjunction with embodiments.

[0077] VCoNi medium entropy alloy is prepared by the following method:

[0078] The weighed V, Co and Ni single substance powders are mixed and put into a cemented carbide pot, wherein the atomic percentage of V, Co and Ni is 1:1:1. The purity of V, Co and Ni single substances is higher than 99.9%, and the particle size of V, Co and Ni single substance powders is 8 μm.

[0079] It was placed in an arc melting furnace and arc-melted for 10 minutes under argon protection to melt the metal into an alloy. In order to make the alloy elements uniform, it was remelted 5 times to obtain a VCoNi medium entropy alloy, in which the alloy included FCC phase, Kappa phase and V 2 O 3 The chemical formula of the Kappa phase is (Co, Ni) 3 V.

[0080] The VCoNi medium entropy alloy was cut into 2 mm thick sheet samples, and then polished until there were no obvious scratches on the surface to obtain cast VCoNi medium entropy alloy samples (hereinafter referred to as VCoNi alloy or VCoNi) for implementing the following embodiments and comparative examples.

[0081] Example 1

[0082] Amorphous boron powder with a purity of 99% and a particle size of ≤1 μm produced by Beijing Bailingwei Technology Co., Ltd. was evenly spread on the surface of the alloy sample to form a boronizing agent layer with a thickness of 1 mm.

[0083] A VCoNi alloy sample with a boriding agent layer on the surface was placed in an SPS-211LX spark plasma sintering furnace, and the temperature of the VCoNi alloy sample was first raised to 600°C for 6 minutes; then raised to 900°C for 3 minutes; finally raised to 1000°C for 2 minutes, and then kept at 1000°C and 50 MPa for 10 minutes to obtain an alloy sample with a wear-resistant layer on the surface (recorded as boriding 1000 / 10).

[0084] Figure 1 The XRD diagram of the VCoNi medium entropy alloy before and after boronization treatment in Example 1 of the present application is shown in FIG. Figure 1 It can be seen that the VCoNi alloy is a FCC single phase before boriding. 4 The boride hard phases such as B indicate that a boriding reaction has occurred on the surface of the alloy sample to form metal borides. After the boriding treatment, a wear-resistant layer is prepared on the surface of the alloy sample, which is beneficial to improving the wear resistance of the alloy.

[0085] Figure 2 This is a schematic diagram of the performance of the alloy sample with a wear-resistant layer on the surface obtained after boronization treatment in Example 1. Figure 2 Part (a) shows a cross-sectional SEM image, and part (b) shows a dotted line graph of the hardness change before and after the boronization treatment.

[0086] according to Figure 2 It can be seen from part (a) that the wear-resistant layer (boronized layer + compact layer + ceramic layer formed on the surface of the compact layer) has a depth of about 100 μm (the matrix in the figure represents the VCoNi medium entropy alloy). It can also be seen that the wear-resistant layer is stratified, and it can be seen that the boronized layer has a lot of very fine precipitated phases. Part (b) shows the hardness data of the wear-resistant layer and the matrix. It can be seen that after the boronization treatment shown in Example 1, the surface hardness (average value) of the alloy reaches 21.5 GPa. The surface boronization treatment can greatly improve the surface hardness of the alloy.

[0087] Example 2

[0088] The difference between it and Example 1 is only that:

[0089] A VCoNi alloy sample with a boriding agent layer on the surface was placed in an SPS-211LX spark plasma sintering furnace, and the temperature of the VCoNi alloy sample was first raised to 600°C for 6 minutes; then raised to 900°C for 3 minutes; finally raised to 1000°C for 2 minutes, and then kept at 1000°C and 50 MPa for 5 minutes to obtain an alloy sample with a wear-resistant layer on the surface (recorded as boriding 1000 / 5).

[0090] Example 3

[0091] The difference between it and Example 1 is only that:

[0092] A VCoNi alloy sample with a boriding agent layer on the surface was placed in an SPS-211LX spark plasma sintering furnace, and the temperature of the VCoNi alloy sample was first raised to 600°C with a heating time of 6 minutes; then the temperature was raised to 900°C with a heating time of 3 minutes; finally, the temperature was raised to 1100°C with a heating time of 2 minutes, and then the temperature was kept at 1100°C and a pressure of 50 MPa for 10 minutes to obtain an alloy sample with a wear-resistant layer on the surface (recorded as borided 1100 / 10).

[0093] Example 4

[0094] The difference between it and Example 1 is only that:

[0095] A VCoNi alloy sample with a boriding agent layer on the surface was placed in an SPS-211LX spark plasma sintering furnace, and the temperature of the VCoNi alloy sample was first raised to 600°C for 6 minutes; then raised to 900°C for 3 minutes; finally raised to 1100°C for 2 minutes, and then kept at 1100°C and 50 MPa for 5 minutes to obtain an alloy sample with a wear-resistant layer on the surface (recorded as borided 1100 / 5).

[0096] Example 5

[0097] A VCoNi alloy sample with a boriding agent layer on the surface was placed in an SPS-211LX spark plasma sintering furnace, and the temperature of the VCoNi alloy sample was first raised to 600°C for 6 minutes; then raised to 900°C for 3 minutes; finally raised to 1200°C for 2 minutes, and then kept at 1200°C and 50 MPa for 5 minutes to obtain an alloy sample with a wear-resistant layer on the surface.

[0098] Example 6

[0099] The difference between it and Example 1 is only that:

[0100] A VCoNi alloy sample with a boriding agent layer on the surface was placed in an SPS-211LX spark plasma sintering furnace, and the temperature of the alloy sample was first raised to 600°C with a heating time of 6 minutes; then the temperature was raised to 900°C with a heating time of 3 minutes; finally, the temperature was raised to 950°C with a heating time of 2 minutes, and then the temperature was kept at 950°C and a pressure of 50 MPa for 10 minutes to obtain an alloy sample with a wear-resistant layer on the surface.

[0101] Example 7

[0102] The difference between it and Example 1 is only that:

[0103] A VCoNi alloy sample with a boriding agent layer on the surface was placed in an SPS-211LX spark plasma sintering furnace, and the temperature of the VCoNi alloy sample was first raised to 600°C with a heating time of 6 minutes; then raised to 1000°C with a heating time of 3 minutes; finally raised to 1000°C with a heating time of 2 minutes, and then kept at 1000°C and 60 MPa for 10 minutes to obtain an alloy sample with a wear-resistant layer on the surface.

[0104] Example 8

[0105] The difference between it and Example 1 is only that:

[0106] A VCoNi alloy sample with a boriding agent layer on the surface was placed in an SPS-211LX spark plasma sintering furnace, and the temperature of the VCoNi alloy sample was first raised to 600°C with a heating time of 6 minutes; then raised to 1000°C with a heating time of 3 minutes; finally raised to 1000°C with a heating time of 2 minutes, and then kept at 1000°C and 40 MPa for 10 minutes to obtain an alloy sample with a wear-resistant layer on the surface.

[0107] Example 9

[0108] The difference between it and Example 1 is only that:

[0109] A VCoNi alloy sample with a boriding agent layer on the surface was placed in an SPS-211LX spark plasma sintering furnace, and the temperature of the VCoNi alloy sample was first raised to 600°C with a heating time of 6 minutes; then raised to 1000°C with a heating time of 3 minutes; finally raised to 1000°C with a heating time of 2 minutes, and then kept at 1000°C and 30 MPa for 10 minutes to obtain an alloy sample with a wear-resistant layer on the surface.

[0110] Comparative Example 1

[0111] The VCoNi medium entropy alloy sample prepared as above is directly used as the alloy sample of comparative example 1 (recorded as unborated / VCoNi before boridation / VCoNi RT).

[0112] Test Example 1

[0113] The VCoNi alloy sample after the boronization treatment in Example 1 and the VCoNi alloy sample before the boronization treatment in Comparative Example 1 were subjected to circular (radius 2 mm) sliding friction and wear tests on Anton Paar THT-800 high-temperature friction and wear testing machine. Ball-disc dry sliding wear was adopted, and the grinding material was a Φ6 mm silicon nitride ceramic ball. The wear test was carried out in an atmospheric environment (relative humidity of about 70%) at room temperature (about 25°C). The friction sliding speed was 0.1 m / s, the load was 5 N, and the sliding distance was 1000 m (about 53,000 laps). After the experiment, the friction coefficient curve was recorded; and the wear track morphology was measured using a 3D profilometer. The wear rate was calculated based on the wear volume. The results are shown as follows. Figure 3 shown.

[0114] Figure 3 This is a schematic diagram of wear comparison between Example 1 and Comparative Example 1, where Figure 3 Parts (a), (b) and (c) represent comparative example 1, and parts (d), (e) and (f) represent example 1. Figure 3 Parts (a) and (d) show the friction and wear curves of the VCoNi alloy material before and after boriding treatment, (b) and (e) respectively show the overall view of the wear track, and (c) and (f) are the 3D contours of the wear track before and after boriding treatment, respectively.

[0115] according to Figure 3 It can be seen that the wear rate of Example 1 is significantly reduced by the above-mentioned boronization treatment compared with the alloy of Comparative Example 1 which is not subjected to the boronization treatment, which means that the above-mentioned boronization treatment can effectively improve the wear resistance of the alloy surface.

[0116] The above operation was performed on the above Examples 2-9. Although the wear rates were changed, they were all lower than those of the alloy in Comparative Example 1 which was not subjected to the boronization treatment. This means that the above boronization treatment can effectively improve the wear resistance of the alloy surface.

[0117] Test Example 2

[0118] Hardness comparison chart and average hardness data of the VCoNi alloy samples after boriding treatment in Test Examples 1-4 and the VCoNi alloy sample before boriding treatment in Comparative Example 1, wherein SD represents variance.

[0119] The results are as follows Figure 4 As shown, according to Figure 4 It can be seen that the average hardness of Examples 1-4 is greater than that of Comparative Example 1.

[0120] In summary, the method for improving the wear resistance of the alloy surface provided in the present application can not only allow the boron element to penetrate into the metal crystal structure and form a variety of metal borides on the alloy surface, and effectively improve the wear resistance of the alloy by compounding a variety of metal borides, but also can effectively refine the alloy grains, making the alloy grain size more uniform to improve the surface hardness and wear resistance of the alloy. At the same time, the wear-resistant layer forms a layered structure on the sub-surface, which does not affect the toughness inside the alloy and can further improve the wear resistance of the alloy.

[0121] The above description is only a specific embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A method for improving the wear resistance of alloy surface, It is characterized in that The following steps are involved: The alloy with a boriding agent layer on its surface is placed in a vacuum environment, heated to a preset temperature, and subjected to a boriding treatment under the conditions of maintaining the preset temperature and preset pressure; Wherein, the alloy contains transition metal elements, the preset pressure is 30MPa-60MPa, and the preset temperature is 950°C-1200°C.

2. The method for improving the wear resistance of an alloy surface according to claim 1, It is characterized in that The preset temperature is 950°C-1100°C.

3. The method for improving the wear resistance of an alloy surface according to claim 1, It is characterized in that The time of the boronization treatment is 5 min-60 min.

4. The method for improving the wear resistance of an alloy surface according to claim 1, It is characterized in that The time of the boronization treatment is 10 min-20 min.

5. The method for improving the wear resistance of an alloy surface according to claim 1, It is characterized in that The step of heating up comprises: First, the temperature is raised to 600°C at a heating rate of 80°C / min-110°C / min and a heating time of 5.5-6.5min; Then, the temperature is raised to 900°C at a heating rate of 80°C / min-120°C / min and a heating time of 2.5-3.8min; Finally, the temperature is raised to the preset temperature at a heating rate of 40°C / min-80°C / min and a heating time of 2-4min.

6. The method for improving the wear resistance of an alloy surface according to any one of claims 1 to 5, It is characterized in that The boronizing agent layer includes a boronizing agent, and the boronizing agent includes powdered B 4 One or more of C, BN, and amorphous boron.

7. The method for improving the wear resistance of an alloy surface according to any one of claims 1 to 5, It is characterized in that The boriding agent layer is composed of powdered amorphous boron.

8. The method for improving the wear resistance of an alloy surface according to any one of claims 1 to 5, It is characterized in that The alloy includes FCC phase, Kappa phase and V 2 O 3 The chemical formula of the Kappa phase is (Co, Ni) 3 V.

9. The method for improving the wear resistance of an alloy surface according to any one of claims 1 to 5, It is characterized in that The thickness of the boronizing agent layer is ≥1 mm.

10. The method for improving the wear resistance of an alloy surface according to any one of claims 1 to 5, It is characterized in that The particle size of the boronizing agent is ≤1 μm.

Citation Information

Patent Citations

  • Titanium alloy surface boronizing method

    CN101608296A

  • Magnesium-rare earth-boron alloy with high heat resistance and preparation method thereof

    CN103849802A

  • Boronitriding treatment method for wear-resistance and high hardness, and boronitriding treatment article using the same

    KR1020110111016A

  • Method of boring steel parts under pressure and container with fusible gate for its implementation

    RU2714267C1