Purification method of carbon fiber material

Through the combined purification method of sodium hydroxide and sodium metaborate, the phosphorus sulfur and metal elements in carbon fiber materials are removed at a low temperature, solving the problems of low purification efficiency and high energy consumption in the prior art, and realizing the high-purity carbon fiber materials Low cost and efficient production.

CN118979376APending Publication Date: 2024-11-19JILIN LIANKE SPECIAL GRAPHITE MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411187243.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing carbon fiber material purification methods have problems such as low purification efficiency, serious environmental pollution and high energy consumption, especially when removing phosphorus sulfur and metal ions, it requires a two-step method and has a high energy consumption.

Method used

Using sodium hydroxide aqueous solution and sodium metaborate as purification reagents and auxiliary purification agents, the steps of ultrasonic treatment, alkali calcination treatment, water washing treatment and acid leaching treatment can be achieved in one step to remove phosphorus sulfur and metal elements at low temperatures, reducing purification temperature and time.

Benefits of technology

The impurity content of carbon fiber materials is less than 10ppm, which shortens purification time, reduces energy consumption, and meets the industrial needs of high-purity carbon fiber materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979376A_ABST
    Figure CN118979376A_ABST
Patent Text Reader

Abstract

The invention is suitable for the technical field of carbon fiber materials, and provides a carbon fiber material purification method, which comprises: dipping a carbon fiber material in a purification reagent sodium hydroxide aqueous solution, adding an auxiliary purification agent sodium metaborate, and stirring; performing ultrasonic treatment on the mixture; roasting the mixture subjected to ultrasonic treatment in a vacuum atmosphere furnace, immediately removing the mixture after roasting, and cooling to room temperature; transferring the mixture cooled to room temperature into a container filled with water, blowing air into the solution, and repeating the screening process for multiple times until the mixture is washed to be neutral; and mixing the mixture washed to be neutral with a hydrochloric acid solution, stirring, extracting the carbon fiber material, filtering, washing to be neutral, and drying. According to the method, the purpose of removing phosphorus, sulfur and metal elements in one step is achieved by utilizing the auxiliary purification reagent in the low-temperature section, the purposes of shortening the purification time and reducing the energy consumption are achieved, and the requirement for import and substitution of similar products in the industry is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of carbon fiber materials, and in particular relates to a method for purifying carbon fiber materials. Background Art

[0002] In recent years, with the rapid development of the aerospace and semiconductor industries, the demand for high-purity carbon fiber materials has continued to rise, especially in the semiconductor heating furnaces of the electronics industry, graphite heaters that act as heating elements, and carbon-carbon composite materials that serve as support and protection, which have put forward more stringent purity standards for carbon fiber materials. However, at present, the carbon materials used by most domestic semiconductor manufacturers are almost all imported products, and domestic companies account for a very small share. Even so, the impurity content of domestically produced thermal insulation carbon felt is still far more than 10ppm, which can only meet the needs of some parts with lower requirements for the impurity content of carbon materials.

[0003] Traditional carbon material purification methods include flotation, alkaline acid method, high temperature purification method and halogen gas purification method, etc. However, these methods all have inherent defects, such as low purification efficiency and serious environmental pollution, which restrict the large-scale production of high-purity carbon materials. The high temperature purification method uses the high boiling point characteristics of carbon and graphite materials to remove all impurity salts by high temperature evaporation. This method is widely used in various types of graphite materials and carbon materials, but it has high energy consumption and long purification time; the principle and process of the halogen gas purification method is to allow the metal ions (such as iron, magnesium, calcium, aluminum, chromium, manganese, zinc and other metal elements) and silicon elements in the carbon material to react with the halogen atoms decomposed by high temperature to generate compounds with lower boiling points, and then remove various impurities from the carbon material by high temperature volatilization, but it is prohibited due to its high pollution and high risk; the existing technical solutions usually replace chlorine and fluorine (such as chlorofluorocarbons, etc.) with chlorine-containing organic matter and fluorine-containing organic matter. , still relying on the chlorine atoms and fluorine atoms produced by high-temperature decomposition to react with metal elements and silicon to generate low-boiling point substances to remove impurities. For example, the patent application with publication number CN116621606A discloses a carbon fiber thermal insulation felt and a purification method thereof, which uses chlorine-containing and fluorine-containing alkanes as purification reagents to achieve metal ion purification. Although this purification method reduces the purification time and reduces energy consumption, since the purification reagents are mainly used to remove metal impurities and silicon impurities, the phosphorus and sulfur in the carbon material still need to be removed by high-temperature purification method, so the energy consumption is still very high, especially the phosphorus and sulfur in the carbon material are very easy to enter the lattice during the carbonization process and firmly combine with the carbon.

[0004] At present, in order to simultaneously solve the problem of removing phosphorus and sulfur and metal ions in purified carbon materials, a two-step purification method is often adopted, that is, the first step is to remove phosphorus and sulfur, and the second step is to remove metal elements. The purification time is relatively long, and the current method of removing phosphorus and sulfur mostly uses high-temperature purification method to remove phosphorus and sulfur in the lattice, which has high energy consumption. Summary of the invention

[0005] The purpose of the embodiments of the present invention is to provide a method for purifying carbon fiber materials, aiming to solve the problems raised in the above background technology.

[0006] The embodiment of the present invention is implemented as follows: a method for purifying carbon fiber material comprises the following steps:

[0007] (1) Preparation stage: treating the carbon fiber material to be purified, immersing it in a purification reagent sodium hydroxide aqueous solution, and then adding an auxiliary purification agent sodium metaborate and stirring to obtain a mixture;

[0008] (2) Ultrasonic treatment stage: The mixture is subjected to ultrasonic treatment to ensure that the carbon fiber material, purification reagent and auxiliary purification agent are evenly mixed;

[0009] (3) Alkali calcination stage: the mixture after ultrasonic treatment is placed in a vacuum atmosphere furnace for calcination, and the mixture is immediately removed and cooled to room temperature after the calcination is completed;

[0010] (4) Water washing treatment stage: the mixture cooled to room temperature is transferred into a container filled with water, air is blown into the solution to promote the flow of solution between the carbon fiber materials, and leaching and screening are performed. The screening process is repeated multiple times until the mixture is washed to neutrality;

[0011] (5) Acid leaching stage: The mixture washed to neutrality is mixed and stirred with a hydrochloric acid solution. After the acid leaching, the carbon fiber material is extracted and filtered, and then washed to neutrality and dried.

[0012] Preferably, in step (1), the concentration of sodium hydroxide is 20%-60%wt, and the mass ratio of the carbon fiber material to the sodium hydroxide solution is 1:1.5-2.5.

[0013] Preferably, in step (1), the amount of sodium metaborate added is 2%-4% of the mass of the carbon fiber material.

[0014] Preferably, in step (2), the ultrasonic treatment is carried out at 40-80°C, with a power of 200-800W and a treatment time of 25-35min.

[0015] Preferably, in step (3), the set temperature of the vacuum atmosphere furnace is 500-700° C., and the calcination time is 1.8-3 h.

[0016] Preferably, in step (4), the step of blowing air into the solution to promote the flow of the solution between the carbon fiber materials is specifically to use an aerator at 45-50°C at a speed of 10-50m 3Air is blown into the solution at a flow rate of / h to promote the flow of solution between fibers, and the leaching and screening time is 30-35min.

[0017] Preferably, in step (5), the concentration of the hydrochloric acid solution is 0.5-1.5 mol / L, and the solid-liquid ratio of the mixture to the hydrochloric acid solution is 1:15-20.

[0018] Preferably, in step (5), the stirring is carried out at 78-82° C., the stirring speed is 750 rpm, and the stirring time is 75-80 min.

[0019] A method for purifying carbon fiber materials provided in an embodiment of the present invention optimizes purification reagents and achieves the purpose of removing phosphorus, sulfur and metal elements in one step by utilizing auxiliary purification reagents in a low temperature section, thereby improving the purification method in the prior art that requires high temperatures of 2800°C and 3000°C and reducing the temperature required for purification. The two-step purification method in the prior art is shortened to one step, reducing the reaction time and allowing the impurity content of the carbon fiber felt to be less than 10ppm, thereby achieving the purpose of shortening the purification time and reducing energy consumption and meeting the demand for import substitution of similar products in the industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 A flow chart of a method for purifying a carbon fiber material provided by an embodiment of the present invention;

[0021] Figure 2 The purification effects of auxiliary purifying agents of different concentrations provided in the embodiments of the present invention are shown. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0023] A method for purifying carbon fiber material, the process is as follows Figure 1 As shown, the following steps are included:

[0024] (1) Preparation stage:

[0025] Treat the carbon fiber material to be purified, immerse the carbon fiber material in a sodium hydroxide aqueous solution, the mass ratio of the two is 1:1.5-2.5, the concentration of sodium hydroxide is 20%-60%wt, and then add an auxiliary purification agent sodium metaborate and stir, the mass of sodium metaborate is about 2%-4% of the mass of the carbon fiber;

[0026] The carbon fiber material includes but is not limited to PAN-based carbon fiber soft felt, asphalt-based carbon fiber soft felt, viscose-based carbon fiber soft felt and carbon fiber hard felt prepared using the above raw materials;

[0027] (2) Ultrasonic treatment stage:

[0028] The mixture is treated at 40-80°C with an ultrasonic power of 200-800W for 30 minutes to ensure uniform mixing of the carbon fiber material, the purification reagent and the auxiliary purification agent;

[0029] (3) Alkali calcination stage:

[0030] The mixture after ultrasonic treatment is placed in a vacuum atmosphere furnace at a set temperature (500-700°C) and calcined. The calcination process lasts for about 2 hours. After the calcination is completed, the mixture is immediately removed and cooled to room temperature.

[0031] (4) Water washing stage:

[0032] After the reaction is completed, the product of step (3) is transferred into a container filled with water and aerated at 50°C at 10-50 m / s. 3 Blow air into the solution at a flow rate of / h to promote the flow of solution between fibers, leaching and screening for 30 minutes, and repeating the above screening steps until the mixture is washed to neutrality;

[0033] (5) Acid leaching stage:

[0034] The washed mixture was mixed with a hydrochloric acid solution (concentration of 0.5-1.5 mol / L) at a solid-liquid ratio of 1:15-20, and stirred at 80°C at a speed of 750 rpm for 80 min. After the reaction was completed, the carbon fiber material after acid leaching was extracted and filtered, and then the carbon fiber material was washed to neutrality and then dried.

[0035] The specific implementation of the present invention is described in detail below in conjunction with specific embodiments.

[0036] Example 1

[0037] A method for purifying a carbon fiber material, wherein the carbon fiber material is 50 kg of asphalt-based carbon fiber felt, comprising the following steps:

[0038] (1) Preparation stage:

[0039] 50 kg of asphalt-based carbon fiber felt, weigh 20-25 kg of purifying agent sodium hydroxide and 1-2 kg of auxiliary purifying agent sodium metaborate, and mix them at a solid-liquid ratio of 2:3;

[0040] (2) Ultrasonic treatment stage:

[0041] The mixture was treated at 80°C with an ultrasonic power of 600 W for 30 min to ensure uniform mixing of the carbon fiber material, the purification reagent and the auxiliary purification agent;

[0042] (3) Alkali calcination stage:

[0043] The mixture after ultrasonic treatment was placed in a vacuum atmosphere furnace at 700°C and calcined. The calcination process lasted for about 3 hours. After the calcination was completed, the mixture was immediately removed and cooled to room temperature.

[0044] (4) Water washing stage:

[0045] After the reaction is completed, the product of step (3) is transferred into a container filled with water and aerated at 50°C with 50m 3 Blow air into the solution at a flow rate of / h to promote the flow of solution between fibers, leaching and screening for 30 minutes, and repeating the above screening steps until the mixture is washed to neutrality;

[0046] (5) Acid leaching stage:

[0047] The washed mixture was mixed with a hydrochloric acid solution (concentration of 1.5 mol / L) at a solid-liquid ratio of 1:15, and stirred at 80°C at a speed of 750 rpm for 80 min. After the reaction was completed, the carbon fiber material after acid leaching was extracted and filtered, and then the carbon fiber material was washed to neutrality and then dried.

[0048] Example 2

[0049] A method for purifying a carbon fiber material, wherein the carbon fiber material is 20 kg of soft carbon fiber felt, comprising the following steps:

[0050] (1) Preparation stage:

[0051] 20 kg of soft carbon fiber felt, weigh 5-10 kg of purifying agent sodium hydroxide and 0.5-1 kg of auxiliary purifying agent sodium metaborate, and mix them at a solid-liquid ratio of 1:2;

[0052] (2) Ultrasonic treatment stage:

[0053] The mixture was treated with an ultrasonic power of 400 W at 40° C. for 30 min to ensure uniform mixing of the carbon fiber material, the purification reagent, and the auxiliary purification agent;

[0054] (3) Alkali calcination stage:

[0055] The mixture after ultrasonic treatment is placed in a vacuum atmosphere furnace at 500°C and calcined. The calcination process lasts for about 1.8-2 hours. After the calcination is completed, the mixture is immediately removed and cooled to room temperature.

[0056] (4) Water washing stage:

[0057] After the reaction is completed, the product of step (3) is transferred into a container filled with water and aerated at 50°C at 15 m / s. 3 Blow air into the solution at a flow rate of / h to promote the flow of solution between fibers, leaching and screening for 30 minutes, and repeating the above screening steps until the mixture is washed to neutrality;

[0058] (5) Acid leaching stage:

[0059] The washed mixture was mixed with a hydrochloric acid solution (concentration of 1 mol / L) at a solid-liquid ratio of 1:18, and stirred at 750 rpm at 80°C for 80 min. After the reaction was completed, the carbon fiber material after acid leaching was extracted and filtered, and then the carbon fiber material was washed to neutrality and then dried.

[0060] The concentration of the auxiliary purifying agent sodium metaborate used in the purification process of the carbon fiber material in Example 1 and Example 2 was controlled to be about 0%, 2%, 4%, 6%, 8%, and 10%, respectively. The other steps were the same as in Example 1 and Example 2. An orthogonal test was performed, and the impurity content of the purified carbon fiber material was detected. The results were as follows: Figure 2 As shown, according to Figure 2 It can be seen that by adding the auxiliary purification agent sodium metaborate, the purpose of removing phosphorus, sulfur and metal elements in one step can be achieved, shortening the purification time and greatly reducing energy consumption.

[0061] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for purifying a carbon fiber material, characterized in that: The following steps are involved: (1) Preparation stage: treating the carbon fiber material to be purified, immersing it in a purification reagent sodium hydroxide aqueous solution, and then adding an auxiliary purification agent sodium metaborate and stirring to obtain a mixture; (2) Ultrasonic treatment stage: The mixture is subjected to ultrasonic treatment to ensure that the carbon fiber material, purification reagent and auxiliary purification agent are evenly mixed; (3) Alkali calcination stage: the mixture after ultrasonic treatment is placed in a vacuum atmosphere furnace for calcination, and the mixture is immediately removed and cooled to room temperature after the calcination is completed; (4) Water washing treatment stage: the mixture cooled to room temperature is transferred into a container filled with water, air is blown into the solution to promote the flow of solution between the carbon fiber materials, and leaching and screening are performed. The screening process is repeated multiple times until the mixture is washed to neutrality; (5) Acid leaching stage: The mixture washed to neutrality is mixed and stirred with a hydrochloric acid solution. After the acid leaching, the carbon fiber material is extracted and filtered, and then washed to neutrality and dried.

2. The method for purifying carbon fiber material according to claim 1, characterized in that: In step (1), the concentration of sodium hydroxide is 20%-60%wt, and the mass ratio of the carbon fiber material to the sodium hydroxide solution is 1:1.5-2.

5.

3. The method for purifying carbon fiber material according to claim 1, characterized in that: In step (1), the amount of sodium metaborate added is 2%-4% of the mass of the carbon fiber material.

4. The method for purifying carbon fiber material according to claim 1, characterized in that: In step (2), the ultrasonic treatment is carried out under the conditions of 40-80°C, 200-800W of power and 25-35min of treatment time.

5. The method for purifying carbon fiber material according to claim 1, characterized in that: In step (3), the set temperature of the vacuum atmosphere furnace is 500-700° C., and the calcination time is 1.8-3 hours.

6. The method for purifying carbon fiber material according to claim 1, characterized in that: In step (4), the step of blowing air into the solution to promote the flow of the solution between the carbon fiber materials is specifically to use an aerator at 45-50°C at a speed of 10-50m 3 Air is blown into the solution at a flow rate of / h to promote the flow of solution between fibers, and the leaching and screening time is 30-35min.

7. The method for purifying carbon fiber material according to claim 1, characterized in that: In step (5), the concentration of the hydrochloric acid solution is 0.5-1.5 mol / L, and the solid-to-liquid ratio of the mixture to the hydrochloric acid solution is 1:15-20.

8. The method for purifying carbon fiber material according to claim 1, characterized in that: In step (5), the stirring is carried out at 78-82° C., the stirring speed is 750 rpm, and the stirring time is 75-80 min.