HEMT epitaxial structure and epitaxial method of GaN single crystal substrate

By growing buffer layer and low-temperature stress control layer on GaN single crystal substrate, the problems of high warpage and vertical leakage in the HEMT epitaxial structure are solved, the consistency and voltage resistance of the device are improved, and suitable for high-performance power and RF devices.

CN118983336APending Publication Date: 2024-11-19SINO NITRIDE SEMICON
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411069694.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

GaN single crystal substrates have problems of large warpage and serious vertical leakage in the HEMT epitaxial structure, which affects the performance consistency and voltage resistance of the device.

Method used

GaN buffer layer, low temperature stress control layer, GaN high resistance layer, AlyGa1-yN back barrier layer, GaN channel layer and AlzGa1-zN barrier layer are grown on GaN single crystal substrate, and the InxGa1-xN solid solution film layer or The combined structure of the InN/GaN superlattice layer regulates the epitaxial growth process, reduces warpage and improves vertical pressure resistance.

Benefits of technology

Effectively reduce the warpage of the HEMT epitaxial structure, improve the thickness and component uniformity of the device, reduce vertical leakage current, and improve vertical voltage withstand performance. It is suitable for power devices with high current density and radio frequency with high operating frequency. Device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983336A_ABST
    Figure CN118983336A_ABST
Patent Text Reader

Abstract

The HEMT epitaxial structure comprises the GaN single crystal substrate, and a GaN buffer layer, a low-temperature stress regulation and control layer, a GaN high-resistance layer, an AlyGa1-yN back barrier layer, a GaN channel layer, an AlzGa1-zN barrier layer and a GaN cap layer which are sequentially grown on the GaN single crystal substrate, the low-temperature stress regulation and control layer is an InxGa1-xN solid solution film layer or an InN / GaN superlattice layer, 0 < = x < = 0.1, 0.05 < = y < = 0.15, and 0.2 < = z < = 0.3. The low-temperature stress regulation and control layer is arranged on the GaN buffer layer to regulate and control the warping degree in the epitaxial growth process, especially in the growth process of the Al < z > Ga < 1-z > N barrier layer, so that the HEMT epitaxial structure with more excellent thickness and component uniformity is obtained, especially the HEMT epitaxial structure with a large size is obtained, and the HEMT device is good in consistency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of HEMT chips, and in particular to a HEMT epitaxial structure and an epitaxial method of a GaN single crystal substrate. Background Art

[0002] At present, the device application of GaN materials mainly relies on heteroepitaxial growth. In the field of light-emitting diodes (LEDs), the technical route of growing GaN materials on sapphire substrates has achieved great success and has become the mainstream of the current LED industry. In the field of power semiconductor devices, growing GaN epitaxial layers on Si and SiC has become the main technical route, especially Si substrates, which have obvious advantages in price and process manufacturing. The disadvantages of GaN single crystal substrates in price and size have prevented them from receiving much attention in the field of power semiconductor devices.

[0003] However, the defect density of GaN layer grown on heterogeneous substrates (Si, SiC) is much higher than that of homogeneous epitaxy. For example, the 0002 half-width of heterogeneous epitaxial GaN on Si substrate is generally greater than 300 arcsec, while the half-width of epitaxial GaN on GaN self-supporting substrate is less than 50 arcsec. Therefore, whether it is a laser chip or a power or RF device, GaN single crystal substrate will be the best choice for high-performance, high-stability high-end products.

[0004] At present, most commercial GaN self-supporting substrates are obtained by grinding and polishing after HVPE epitaxy. Due to technical and cost limitations, the thickness of GaN single crystal substrates is not large, generally less than 500um. Therefore, when using HVPE-GaN single crystals as substrates, especially large-sized GaN single crystals, the bottom of the substrate is usually heated for epitaxial growth during the epitaxial growth of thin films. In the process of heating the substrate from room temperature to the temperature of epitaxial growth, a very large bowl-shaped negative warp will be formed, which will affect the thickness and component ratio of the epitaxial film layer, and thus affect the consistency of device performance; in addition, undoped GaN often behaves as n-type (silicon-based gallium nitride epitaxy often uses p-type Si), so no depletion region is formed in the vertical direction. If the vertical leakage is completely blocked by self-doped C-GaN high-resistance layer, the effect is very poor. For example, 1um thick C-GaN (C content>1E9cm -3 ), the withstand voltage in the vertical direction shall not exceed 200V. Summary of the invention

[0005] The object of the present invention is to provide a HEMT epitaxial structure and an epitaxial method for a GaN single crystal substrate, so as to reduce the warping degree and vertical leakage of the HEMT epitaxial structure.

[0006] In order to achieve the above object, the present invention provides a HEMT epitaxial structure of a GaN single crystal substrate, comprising a GaN single crystal substrate and a GaN buffer layer, a low temperature stress regulating layer, a GaN high resistance layer, an Al y Ga 1-y N back barrier layer, GaN channel layer, Al z Ga 1-z N barrier layer and GaN cap layer, the low temperature stress regulating layer is In x Ga 1-x N solid solution thin film layer and / or InN / GaN superlattice layer, wherein 0≤x≤0.1, 0.05≤y≤0.15, 0.2≤z≤0.3.

[0007] Preferably, the In x Ga 1-x The solvent in the N solid solution thin film layer is GaN crystal, and the solute is In atoms.

[0008] Preferably, the thickness of the GaN single crystal substrate is greater than or equal to 400 microns and less than or equal to 500 microns; and / or the resistivity of the GaN single crystal substrate is greater than 1E7 ohm-centimeter; and / or the thickness of the GaN buffer layer is greater than or equal to 200 nanometers and less than or equal to 500 nanometers.

[0009] Preferably, the In x Ga 1-x The thickness of the N solid solution thin film layer is greater than or equal to 1.5 micrometers and less than or equal to 3 micrometers.

[0010] Preferably, the thickness of each InN layer in the InN / GaN superlattice layer is greater than 0 nanometers and less than or equal to 10 nanometers and the thickness of each GaN layer is greater than or equal to 50 nanometers and less than or equal to 100 nanometers, and the number of cycles of the InN / GaN superlattice is greater than or equal to 15 and less than or equal to 30.

[0011] Preferably, the GaN high resistance layer is an externally doped C-GaN layer, and the C doping concentration in the C-GaN layer is greater than or equal to 5E18cm -3 and less than or equal to 1E19cm -3 , the thickness of the C-GaN layer is greater than or equal to 500 nanometers and less than or equal to 1500 nanometers; or, the GaN high resistance layer is a Mg-doped P-GaN layer, and the hole concentration of the P-GaN layer is greater than or equal to 5E16cm -3 and less than or equal to 5E17cm -3 , the thickness of the P-GaN layer is greater than or equal to 500 nanometers and less than or equal to 1000 nanometers.

[0012] Preferably, the Al y Ga 1-y The thickness of the N back barrier layer is greater than or equal to 50 nanometers and less than or equal to 150 nanometers; and / or the thickness of the GaN channel layer is greater than or equal to 150 nanometers and less than or equal to 300 nanometers; and / or the Al z Ga 1-z The thickness of the N barrier layer is greater than or equal to 15 nanometers and less than or equal to 30 nanometers; and / or the thickness of the GaN cap layer is greater than or equal to 1 nanometer and less than or equal to 3 nanometers.

[0013] The embodiment of the present invention also provides a HEMT epitaxial growth method of a GaN single crystal substrate, comprising the following steps: S1, providing a GaN single crystal substrate, and epitaxially growing a GaN buffer layer on the GaN single crystal substrate; S2, epitaxially growing a low-temperature stress regulation layer on the GaN buffer layer, wherein the low-temperature stress regulation layer is In x Ga 1-x N solid solution thin film layer and / or InN / GaN superlattice layer, wherein 0≤x≤0.1; S3, epitaxially growing a GaN high resistance layer on the low temperature stress regulation layer; S4, growing an Al y Ga 1-y N back barrier layer, wherein 0.05≤y≤0.15; S5, in the Al y Ga 1-y Growing a GaN channel layer on the N back barrier layer; S6, growing an Al z Ga 1-z N barrier layer, wherein 0.2≤z≤0.3; S7, in the Al z Ga 1-z A GaN cap layer is grown on the N barrier layer.

[0014] Preferably, the growth pressure of the low-temperature stress regulation layer is greater than or equal to 100 mbar and less than or equal to 300 mbar, and the growth temperature of the low-temperature stress regulation layer is greater than or equal to 750 degrees Celsius and less than or equal to 850 degrees Celsius; the GaN high resistance layer has a first growth setting pressure, the first growth setting pressure is greater than or equal to 50 mbar and less than or equal to 200 mbar, and the GaN high resistance layer has a first growth setting temperature, the first growth setting temperature is greater than or equal to 900 degrees Celsius and less than or equal to 1050 degrees Celsius; the Al y Ga 1-y The N back barrier layer has a second growth setting pressure, which is greater than or equal to 50 mbar and less than or equal to 100 mbar. y Ga 1-yThe N back barrier layer has a second growth setting temperature, which is greater than or equal to 1050 degrees Celsius and less than or equal to 1150 degrees Celsius.

[0015] Preferably, the In x Ga 1-x The N solid solution thin film layer is formed by simultaneously introducing ammonia, trimethylgallium and trimethylindium into the GaN buffer layer; the InN / GaN superlattice layer is formed by alternately introducing trimethylgallium and trimethylindium into the GaN buffer layer while introducing ammonia.

[0016] Preferably, the GaN high resistance layer is an externally doped C-GaN layer, and step S3 includes: growing the GaN high resistance layer by introducing ammonia, trimethylgallium and hexene into the low-temperature stress regulation layer; or, the GaN high resistance layer is a Mg-doped P-GaN layer, and step S3 includes: growing the GaN high resistance layer by introducing ammonia, trimethylgallium and bis(cyclopentadienyl)magnesium into the low-temperature stress regulation layer.

[0017] Compared with the prior art, the present invention arranges a low-temperature stress regulating layer on the GaN buffer layer. During the growth process, the low-temperature stress regulating layer is more inclined to convex warping because the lattice constant of InN is larger than that of GaN and low-temperature gallium nitride has more grain boundaries, thereby resisting the concave warping of the GaN single crystal substrate, thereby regulating the epitaxial growth process, especially Al z Ga 1-z The warpage of the N barrier layer during growth is used to obtain a HEMT epitaxial structure with better thickness and composition uniformity, especially a large-sized HEMT epitaxial structure to make the HEMT device consistent. In addition, by setting Al on the GaN high-resistance layer y Ga 1-y The N back barrier layer can effectively reduce the leakage current in the vertical direction and improve the vertical withstand voltage performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a structural schematic diagram of the HEMT epitaxial structure of the GaN single crystal substrate of the present invention. DETAILED DESCRIPTION

[0019] In order to explain the technical content, structural features and achieved effects of the present invention in detail, the following is a detailed description in conjunction with the implementation methods and the accompanying drawings.

[0020] Embodiment 1

[0021] like Figure 1As shown, the embodiment of the present invention provides a HEMT epitaxial structure of a GaN single crystal substrate, comprising a GaN single crystal substrate 1 and a GaN buffer layer 2, a low temperature stress regulating layer 3, a GaN high resistance layer 4, an Al y Ga 1-y N back barrier layer 5, GaN channel layer 6, Al z Ga 1-z N barrier layer 7 and GaN cap layer 8, the low temperature stress regulation layer 3 is an InN / GaN superlattice layer, wherein 0.05≤y≤0.15, 0.2≤z≤0.3, specifically, the growth temperature of the low temperature stress regulation layer 3 is lower than that of the GaN buffer layer 2, the GaN high resistance layer 4, and the Al y Ga 1-y N back barrier layer 5, GaN channel layer 6, Al z Ga 1-z The growth temperature of the N barrier layer 7 and the GaN cap layer 8 is set to ensure that In is well grown and prepared. It should be noted that in some other specific embodiments, the low temperature stress regulating layer 3 can also be In x Ga 1-x N solid solution thin film layer, In x Ga 1-x The solvent in the N solid solution film layer is GaN crystal, and the solute is In atom, where 0≤x≤10. It should be noted that the low temperature stress regulation layer can also be In x Ga 1-x The stack of N solid solution thin film layer and InN / GaN superlattice layer can be x Ga 1-x An InN / GaN superlattice layer is provided on the N solid solution thin film layer, or two layers of In x Ga 1-x A sandwich structure in which an InN / GaN superlattice layer is sandwiched between a N solid solution thin film layer.

[0022] In the embodiment of the present invention, a low-temperature stress regulating layer 3 is arranged on the GaN buffer layer 2. During the growth process of the low-temperature stress regulating layer 3, since the lattice constant of InN is larger than that of GaN and low-temperature gallium nitride has more grain boundaries, the low-temperature stress regulating layer 3 is more inclined to convex warping, thereby resisting the concave warping of the GaN single crystal substrate 1, thereby regulating the epitaxial growth process, especially Al z Ga 1-z The warpage of the N barrier layer 7 during growth is used to obtain a HEMT epitaxial structure with better thickness and composition uniformity, especially a large-sized HEMT epitaxial structure to make the HEMT device consistent. In addition, by setting Al on the GaN high resistance layer 4 y Ga 1-yThe N back barrier layer 5 can effectively reduce the leakage current in the vertical direction and improve the vertical withstand voltage performance.

[0023] In the embodiment of the present invention, the thickness of the GaN single crystal substrate 1 is greater than or equal to 400 microns and less than or equal to 500 microns; the resistivity of the GaN single crystal substrate 1 is greater than 1E7 ohm-cm; the thickness of the GaN buffer layer 2 is greater than or equal to 200 nanometers and less than or equal to 500 nanometers. Of course, the thickness and resistivity of the GaN single crystal substrate 1 and the thickness of the GaN buffer layer 2 can be selected according to actual needs.

[0024] In an embodiment of the present invention, the thickness of each InN layer in the InN / GaN superlattice layer is greater than 0 nanometers and less than or equal to 10 nanometers, and the thickness of each GaN layer is greater than or equal to 50 nanometers and less than or equal to 100 nanometers, and the number of cycles of the InN / GaN superlattice is greater than or equal to 15 and less than or equal to 30.

[0025] In some other specific embodiments of the present invention, when the low temperature stress regulating layer 3 is In x Ga 1-x N solid solution film layer, In x Ga 1-x The thickness of the N solid solution thin film layer is greater than or equal to 1.5 micrometers and less than or equal to 3 micrometers.

[0026] In the embodiment of the present invention, the GaN high resistance layer 4 is an externally doped C-GaN layer, and the C doping concentration in the C-GaN layer is preferably greater than or equal to 5E18cm -3 and less than or equal to 1E19cm -3 , the thickness of the C-GaN layer is preferably greater than or equal to 500 nanometers and less than or equal to 1500 nanometers;

[0027] In some other embodiments, the GaN high resistance layer 4 is a Mg-doped P-GaN layer, and the hole concentration of the P-GaN layer is preferably greater than or equal to 5E16 cm -3 and less than or equal to 5E17cm -3 , the thickness of the P-GaN layer is preferably greater than or equal to 500 nanometers and less than or equal to 1000 nanometers.

[0028] Therefore, in order to solve the serious vertical leakage problem in homoepitaxial growth, a Mg-doped or C-doped GaN high-resistance layer 4 is used in combination with an Al y Ga 1-yThe N back barrier layer 5 can effectively reduce vertical leakage and improve vertical withstand voltage. The HEMT epitaxial structure of the GaN single crystal substrate in the embodiment of the present invention can obtain an epitaxial structure with high mobility and low square resistance. The HEMT epitaxial structure of the GaN single crystal substrate is particularly suitable for the manufacture of power devices with high current density or radio frequency devices with high operating frequency.

[0029] In the embodiment of the present invention, Al y Ga 1-y The thickness of the N back barrier layer 5 is preferably greater than or equal to 50 nanometers and less than or equal to 150 nanometers.

[0030] In the embodiment of the present invention, the thickness of the GaN channel layer 6 is preferably greater than or equal to 150 nanometers and less than or equal to 300 nanometers. z Ga 1-z The thickness of the N barrier layer 7 is preferably greater than or equal to 15 nanometers and less than or equal to 30 nanometers, and the thickness of the GaN cap layer 8 is preferably greater than or equal to 1 nanometer and less than or equal to 3 nanometers.

[0031] Embodiment 2

[0032] The embodiment of the present invention further provides a HEMT epitaxial growth method of a GaN single crystal substrate 1, which is used to prepare the HEMT epitaxial structure of the GaN single crystal substrate 1, and comprises the following steps:

[0033] S1. Provide a GaN single crystal substrate 1, and epitaxially grow a GaN buffer layer 2 on the GaN single crystal substrate 1; specifically, the GaN single crystal substrate 1 is a self-supporting structure, the thickness of the GaN single crystal substrate 1 is greater than or equal to 400 microns and less than or equal to 500 microns, for example, the thickness of the GaN single crystal substrate 1 can be 450 microns, the growth temperature of the GaN buffer layer 2 is greater than or equal to 900 degrees Celsius and less than or equal to 1000 degrees Celsius, the growth pressure of the GaN buffer layer 2 is greater than or equal to 200 mbar and less than or equal to 400 mbar, the growth rate of the GaN buffer layer 2 is greater than or equal to 1 um / h and less than or equal to 3 um / h, the thickness of the GaN buffer layer 2 is greater than or equal to 200 nanometers and less than or equal to 500 nanometers, and in addition, the insulation performance of the GaN single crystal substrate 1 can be selected according to the type of device actually required to be manufactured.

[0034] S2. epitaxially grow a low-temperature stress regulation layer 3 on the GaN buffer layer 2, wherein the low-temperature stress regulation layer 3 is an InN / GaN superlattice layer; specifically, the growth pressure of the low-temperature stress regulation layer 3 is greater than or equal to 100 mbar and less than or equal to 300 mbar, and the growth temperature of the low-temperature stress regulation layer 3 is greater than or equal to 750 degrees Celsius and less than or equal to 850 degrees Celsius. A lower temperature is conducive to the formation of InN. The InN / GaN superlattice layer is formed by alternately introducing trimethylgallium and trimethylindium while introducing ammonia gas into the GaN buffer layer 2, that is, during the growth of the InN / GaN superlattice layer, trimethylgallium and trimethylindium are introduced. Ammonia, and trimethylgallium and trimethylindium are alternately introduced, the number of cycles is greater than or equal to 15 and less than or equal to 30, the growth rate of InN is greater than or equal to 0.1um / h and less than or equal to 0.5um / h, the growth rate of GaN is greater than or equal to 0.4um / h and less than or equal to 1.5um / h, the thickness of each layer of InN in the InN / GaN superlattice layer is greater than 0 nanometers and less than or equal to 10 nanometers and the thickness of each layer of GaN is greater than or equal to 50 nanometers and less than or equal to 100 nanometers, the thickness of each period is controlled by time, and the period thickness can be obtained by XRD diffraction. Of course, in some other specific embodiments, it is not limited to using ammonia, trimethylgallium, and trimethylindium as nitrogen sources, gallium sources, and indium sources, and can be selected according to actual needs.

[0035] S3. Epitaxially grow a GaN high resistance layer 4 on the low temperature stress regulation layer 3; specifically, ammonia and trimethylgallium can be used as a nitrogen source and a gallium source to grow the GaN high resistance layer 4, the GaN high resistance layer 4 has a first growth setting pressure, the first growth setting pressure is greater than or equal to 50 mbar and less than or equal to 200 mbar, the GaN high resistance layer 4 has a first growth setting temperature, the first growth setting temperature is greater than or equal to 900 degrees Celsius and less than or equal to 1050 degrees Celsius, the growth pressure of the low temperature stress regulation layer 3 in step S2 is adjusted to the first growth setting pressure, and the growth temperature of the low temperature stress regulation layer 3 in step S2 is adjusted to the first growth setting temperature, and ammonia and trimethylgallium are introduced to grow the GaN high resistance layer 4 when the pressure and temperature are adjusted.

[0036] S4, growing Al on the GaN high resistance layer 4 y Ga 1-y N back barrier layer 5, wherein 0.05≤y≤0.15; specifically, ammonia, trimethylgallium, and trimethylaluminum are used as nitrogen source, gallium source, and aluminum source, respectively; Al y Ga 1-y The N back barrier layer 5 has a second growth setting pressure, which is greater than or equal to 50 mbar and less than or equal to 100 mbar. y Ga 1-yThe N back barrier layer 5 has a second growth setting temperature, which is greater than or equal to 1050 degrees Celsius and less than or equal to 1150 degrees Celsius. The first growth setting pressure of the GaN high resistance layer 4 in step S3 is adjusted to the second growth setting pressure, and the first growth setting temperature of the GaN high resistance layer 4 in step S3 is increased to the second growth setting temperature. When the temperature and pressure change, ammonia, trimethylgallium, trimethylaluminum, Al y Ga 1-y The growth rate of the N back barrier layer 5 is greater than or equal to 0.5 um / h and less than or equal to 2 um / h, and the Al y Ga 1-y The thickness of the N back barrier layer 5 is greater than or equal to 50 nanometers and less than or equal to 150 nanometers. The doping concentration of the Al component is controlled by controlling the flow rate of trimethylgallium and trimethylaluminum. The doping concentration of the Al component and the Al y Ga 1-y The thickness of the N back barrier layer 5 can be measured by an XRD method.

[0037] S5. In Al y Ga 1-y A GaN channel layer 6 is grown on the N back barrier layer 5; specifically, ammonia and trimethylgallium can be used as a nitrogen source and a gallium source, respectively, the growth temperature of the GaN channel layer 6 is greater than or equal to 1050 degrees Celsius and less than or equal to 1100 degrees Celsius, the growth pressure of the GaN channel layer 6 is greater than or equal to 200 mbar and less than or equal to 400 mbar, the growth rate of the GaN channel layer 6 is greater than or equal to 1 um / h and less than or equal to 3 um / h, and the thickness of the GaN channel layer 6 can be greater than or equal to 150 nanometers and less than or equal to 300 nanometers.

[0038] S6, growing Al on the GaN channel layer 6 z Ga 1-z N barrier layer 7, wherein 0.2≤z≤0.3; specifically, Al z Ga 1-z The growth temperature of the N barrier layer 7 is greater than or equal to 1050 degrees Celsius and less than or equal to 1150 degrees Celsius. z Ga 1-z The growth pressure of the N barrier layer 7 is greater than or equal to 50 mbar and less than or equal to 100 mbar. z Ga 1-z The growth rate of the N barrier layer 7 is greater than or equal to 0.2 um / h and less than or equal to 1 um / h. z Ga 1-z The thickness of the N barrier layer 7 may be greater than or equal to 15 nanometers and less than or equal to 30 nanometers.

[0039] S7, in Alz Ga 1-z A GaN cap layer 8 is grown on the N barrier layer 7. Specifically, the growth temperature and growth pressure of the GaN cap layer 8 are the same as those in step S6. z Ga 1-z The process conditions such as the growth temperature and growth pressure of the N barrier layer 7 are the same, so the GaN cap layer 8 can continue to grow by simply stopping the introduction of trimethylaluminum. The thickness of the GaN cap layer 8 is greater than or equal to 1 nanometer and less than or equal to 3 nanometers.

[0040] It should be noted that, in some other embodiments, the low temperature stress regulating layer 3 in step S2 may also be In x Ga 1-x N solid solution thin film layer, wherein 0≤x≤0.1, specifically, In x Ga 1-x The N solid solution thin film layer is formed by simultaneously passing ammonia, trimethylgallium and trimethylindium on the GaN buffer layer 2. x Ga 1-x The specific growth pressure and growth temperature of the N solid solution thin film layer are in the same range as the growth pressure and growth temperature of the InN / GaN superlattice layer, and can be set according to actual needs.

[0041] In the embodiment of the present invention, a low temperature stress regulating layer is grown on the GaN buffer layer to regulate the epitaxial growth process, especially the Al z Ga 1-z The warpage of the N barrier layer 7 during growth is used to obtain a HEMT epitaxial structure with better thickness and composition uniformity, especially a large-sized HEMT epitaxial structure to achieve good consistency of the HEMT device.

[0042] In the embodiment of the present invention, when the GaN high resistance layer 4 is an externally doped C-GaN layer, step S3 includes: growing the GaN high resistance layer 4 by introducing ammonia, trimethylgallium and hexene on the low temperature stress regulation layer 3. Specifically, the growth pressure of the low temperature stress regulation layer 3 in step S2 is adjusted to a first growth setting pressure, and the growth temperature of the low temperature stress regulation layer 3 in step S2 is adjusted to a first growth setting temperature, and ammonia, trimethylgallium and hexene are introduced during the pressure and temperature adjustment to grow the GaN high resistance layer 4. The C doping concentration in the C-GaN layer is preferably greater than or equal to 5E18cm -3 and less than or equal to 1E19cm -3 The thickness of the C-GaN layer is preferably greater than or equal to 500 nanometers and less than or equal to 1500 nanometers. The C-doped GaN high-resistance layer can compensate for the excess electrons in GaN, thereby increasing resistance and preventing current from passing through, while the Al y Ga 1-yThe N back barrier layer 5 utilizes the wider bandgap of AlN to forcibly increase the energy of the conduction band at this position, forming a potential barrier and reducing the current in the vertical direction.

[0043] In the embodiment of the present invention, when the GaN high resistance layer 4 is a Mg-doped P-GaN layer, step S3 includes: growing the GaN high resistance layer 4 by introducing ammonia, trimethylgallium and bis(cyclopentadienyl)magnesium on the low temperature stress regulation layer 3. Specifically, the growth pressure of the low temperature stress regulation layer 3 in step S2 is adjusted to the first growth setting pressure, and the growth temperature of the low temperature stress regulation layer 3 in step S2 is adjusted to the first growth setting temperature, and ammonia, trimethylgallium and bis(cyclopentadienyl)magnesium are introduced when the pressure and temperature are adjusted to grow the P-GaN layer. At this time, after step S7, the grown HEMT epitaxial structure needs to be annealed in a rapid annealing furnace, the annealing temperature is greater than or equal to 850 degrees Celsius and less than or equal to 950 degrees Celsius, the annealing time is greater than or equal to 30 seconds and less than or equal to 60 seconds, and the concentration of holes in the P-GaN layer is preferably greater than or equal to 5E16cm -3 and less than or equal to 5E17cm -3 The thickness of the P-GaN layer is preferably greater than or equal to 500 nanometers and less than or equal to 1000 nanometers. The Mg-doped GaN high resistance layer can form a P-GaN layer. The P-GaN layer and the GaN channel layer 6 form a reverse PN junction to reduce leakage.

[0044] The embodiment of the present invention solves the serious vertical leakage problem in homoepitaxial growth by using a Mg-doped or C-doped GaN high-resistance layer 4 and combining it with Al y Ga 1-y The N back barrier layer 5 can effectively reduce vertical leakage and improve vertical withstand voltage. The HEMT epitaxial structure of the GaN single crystal substrate in the embodiment of the present invention can obtain an epitaxial structure with high mobility and low square resistance. The HEMT epitaxial structure of the GaN single crystal substrate is particularly suitable for the manufacture of power devices with high current density or radio frequency devices with high operating frequency.

[0045] When the HEMT epitaxial growth method of a GaN single crystal substrate according to an embodiment of the present invention is used to prepare a HEMT epitaxial structure of a GaN single crystal substrate for a high operating frequency gallium nitride HEMT radio frequency device, the specific process parameters are as follows:

[0046] In step S1, the GaN single crystal substrate 1 is specifically a GaN semi-insulating substrate grown by HVPE, the resistivity of the GaN single crystal substrate 1 is greater than 1E7Ωcm, the thickness of the GaN single crystal substrate 1 is 450 microns, the growth temperature of the GaN buffer layer 2 is 900 degrees Celsius, the growth pressure is 200mbar, the growth rate is 2um / h, and the thickness of the GaN buffer layer 2 is specifically 200 nanometers.

[0047] In step S2, the low-temperature stress regulation layer 3 is an InN / GaN superlattice layer with a cycle number of 20, the growth temperature is reduced to 820 degrees Celsius, the growth pressure is 200mBar, ammonia is continuously introduced, and trimethylgallium and trimethylindium are introduced alternately. The thickness of each InN layer is 5 nanometers, and the thickness of each GaN layer is 100 nanometers.

[0048] In step S3, the GaN high resistance layer 4 is an externally doped C-GaN layer, ammonia and trimethyl gallium are used as nitrogen source and gallium source, and hexene is used as doping source. The growth temperature is increased to 1000 degrees Celsius, and the growth pressure is changed to 75mbar. When the growth temperature and growth pressure change, ammonia, trimethyl gallium and hexene are introduced, and the growth rate is 2.5um / h. The thickness of the C-GaN layer is preferably greater than or equal to 750 nanometers and less than or equal to 1250 nanometers, and the C concentration in the C-GaN layer is greater than 5E18cm -3 , C doping concentration can be obtained by SIMS test.

[0049] In step S4, ammonia, trimethylgallium, and trimethylaluminum are used as nitrogen source, gallium source, and aluminum source to epitaxially grow Al y Ga 1-y N back barrier layer 5, based on step S3, the temperature is raised to 1080 degrees Celsius, the growth pressure is 75mBar, the growth rate is 1.2um / h, Al y Ga 1-y The value of y in the N back barrier layer 5 is 0.1, which is Al 0.1 Ga 0.9 N back barrier layer, Al y Ga 1-y The thickness of the N back barrier layer 5 is 150 nanometers. The doping concentration of the Al component is controlled by controlling the flow rate of trimethylgallium and trimethylaluminum. y Ga 1-y The thickness of the N back barrier layer 5 can be measured by an XRD method.

[0050] In step S5, ammonia and trimethylgallium are used as nitrogen source and gallium source respectively to grow GaN channel layer 6, the growth temperature of GaN channel layer 6 is 1080 degrees Celsius, the growth pressure is 200 mbar, the growth rate is 2.5 um / h, GaN channel layer 6 is unintentionally doped GaN channel layer 6, and the thickness of GaN channel layer 6 is 300 nanometers.

[0051] In step S6, ammonia, trimethylgallium, and trimethylaluminum are used as nitrogen source, gallium source, and aluminum source to grow Al z Ga 1-zN barrier layer 7, based on step S5, the temperature is raised to 1090 degrees Celsius, the growth pressure is 50mBar, the growth rate is 0.8um / h, Al z Ga 1-z The value of z in the N barrier layer 7 is 0.22, that is, Al 0.22 Ga 0.78 N barrier layer, Al z Ga 1-z The thickness of the N barrier layer 7 is 20 nanometers. The doping concentration of the Al component is controlled by controlling the flow rate of trimethylgallium and trimethylaluminum. z Ga 1-z The thickness of the N barrier layer 7 can be measured by the XRR method. z Ga 1-z The composition of the N barrier layer 7 can be obtained by XRD.

[0052] In step S7, based on step S6, the trimethylaluminum source is turned off, and the growth is continued for a period of time. The GaN cap layer 8 is an unintentionally doped GaN cap layer 8, and the thickness of the GaN cap layer 8 is 2 nanometers. The thickness of the GaN cap layer 8 can be measured by the XRR method.

[0053] In some other specific implementations of the present invention, when the HEMT epitaxial growth method of a GaN single crystal substrate is used to prepare a HEMT epitaxial structure of a GaN single crystal substrate 1 for a high power density gallium nitride HEMT power device, the specific process parameters are as follows:

[0054] In step S1, since the high power density gallium nitride HEMT power device does not have high requirements on the resistivity of the GaN single crystal substrate 1, the GaN single crystal substrate 1 can be a GaN non-intentionally doped substrate grown by HVPE. The GaN single crystal substrate 1 has lower cost and relatively low defect density. The thickness of the GaN single crystal substrate 1 is 450 microns, the growth temperature of the GaN buffer layer 2 is 900 degrees Celsius, the growth pressure is 200 mbar, the growth rate is 2 um / h, and the thickness of the GaN buffer layer 2 is specifically 200 nanometers.

[0055] In step S2, the low-temperature stress regulation layer 3 is an InN / GaN superlattice layer with a cycle number of 30. On the basis of step S1, the temperature is lowered to 800 degrees Celsius, the growth pressure is 200mBar, ammonia is continuously introduced, and trimethylgallium and trimethylindium are introduced alternately. The thickness of each InN layer is 10 nanometers, and the thickness of each GaN layer is 100 nanometers.

[0056] In step S3, the GaN high resistance layer 4 is a Mg-doped P-GaN layer, ammonia and trimethylgallium are used as nitrogen source and gallium source, and bis(cyclopentadienyl)magnesium is used as doping source. The growth temperature is increased to 900 degrees Celsius, and the growth pressure is reduced to 75 mbar. When the growth temperature and growth pressure change, ammonia, trimethylgallium and bis(cyclopentadienyl)magnesium are introduced. The growth rate is 1 um / h, the thickness of the P-GaN layer is 500 nanometers, and the hole concentration in the P-GaN layer is preferably greater than 1E17 cm -3 , the Mg doping concentration can be obtained by SIMS test, and the hole concentration can be obtained by Hall measurement.

[0057] In step S4, ammonia, trimethylgallium, and trimethylaluminum are used as nitrogen source, gallium source, and aluminum source to epitaxially grow Al y Ga 1-y N back barrier layer 5, based on step S3, the temperature is raised to 1060 degrees Celsius, the growth pressure is still 75mBar, the growth rate is 1.8um / h, Al y Ga 1-y The value of y in the N back barrier layer 5 is 0.05, which is Al 0.05 Ga 0.95 N back barrier layer, Al y Ga 1-y The thickness of the N back barrier layer 5 is 200 nanometers. The doping concentration of the Al component is controlled by controlling the flow rate of trimethylgallium and trimethylaluminum. y Ga 1-y The thickness of the N back barrier layer 5 can be measured by an XRD method.

[0058] In step S5, ammonia and trimethylgallium are used as nitrogen source and gallium source respectively to grow GaN channel layer 6, the growth temperature of GaN channel layer 6 is 1080 degrees Celsius, the growth pressure is 200 mbar, the growth rate is 2.5 um / h, GaN channel layer 6 is unintentionally doped GaN channel layer 6, and the thickness of GaN channel layer 6 is 250 nanometers.

[0059] In step S6, ammonia, trimethylgallium, and trimethylaluminum are used as nitrogen source, gallium source, and aluminum source to grow Al z Ga 1-z N barrier layer 7, based on step S5, the temperature is raised to 1100 degrees Celsius, the growth pressure is 50mBar, the growth rate is 0.8um / h, Al z Ga 1-z The value of z in the N barrier layer 7 is 0.25, that is, Al 0.25 Ga 0.75 N barrier layer, Al z Ga 1-zThe thickness of the N barrier layer 7 is 25 nanometers. The doping concentration of the Al component is controlled by controlling the flow rate of trimethylgallium and trimethylaluminum. z Ga 1-z The thickness of the N barrier layer 7 can be measured by the XRR method. z Ga 1-z The composition of the N barrier layer 7 can be obtained by XRD.

[0060] In step S7, based on step S6, the trimethylaluminum source is turned off, and the growth is continued for a period of time. The GaN cap layer 8 is an unintentionally doped GaN cap layer 8, and the thickness of the GaN cap layer 8 is 2 nanometers. The thickness of the GaN cap layer 8 can be measured by the XRR method.

[0061] After step S7, step S8 is also included: after the epitaxial growth is completed, the epitaxial wafer is taken out and placed in a rapid annealing furnace, and rapid annealing is performed at 850 degrees Celsius for 60 seconds. Specifically, Mg is activated by annealing to obtain a hole concentration and achieve a high resistance effect.

[0062] It should be noted that when the HEMT epitaxial growth method of a GaN single crystal substrate is used to prepare a HEMT epitaxial structure of a GaN single crystal substrate for a high operating frequency gallium nitride HEMT radio frequency device and when the HEMT epitaxial growth method of a GaN single crystal substrate is used to prepare a HEMT epitaxial structure of a GaN single crystal substrate 1 for a high power density gallium nitride HEMT power device, unless otherwise specified, each process parameter may fluctuate within the parameter range in steps S1 to S7.

[0063] The above disclosure is only a preferred embodiment of the present invention, and certainly cannot be used to limit the scope of rights of the present invention. Therefore, equivalent changes made according to the scope of the patent application of the present invention still fall within the scope covered by the present invention.

Claims

1. A HEMT epitaxial structure of a GaN single crystal substrate, characterized in that: The invention comprises a GaN single crystal substrate and a GaN buffer layer, a low temperature stress regulating layer, a GaN high resistance layer, an Al y Ga 1-y N back barrier layer, GaN channel layer, Al z Ga 1-z N barrier layer and GaN cap layer, the low temperature stress regulating layer is In x Ga 1-x N solid solution thin film layer and / or InN / GaN superlattice layer, wherein 0≤x≤0.1, 0.05≤y≤0.15, 0.2≤z≤0.

3.

2. The HEMT epitaxial structure of the GaN single crystal substrate according to claim 1, characterized in that: In x Ga 1-x The solvent in the N solid solution thin film layer is GaN crystal, and the solute is In atoms.

3. The HEMT epitaxial structure of the GaN single crystal substrate according to claim 1, characterized in that: The thickness of the GaN single crystal substrate is greater than or equal to 400 microns and less than or equal to 500 microns; and / or the resistivity of the GaN single crystal substrate is greater than 1E7 ohm-cm; And / or, the thickness of the GaN buffer layer is greater than or equal to 200 nanometers and less than or equal to 500 nanometers.

4. The HEMT epitaxial structure of the GaN single crystal substrate according to claim 1, characterized in that: In x Ga 1-x The thickness of the N solid solution thin film layer is greater than or equal to 1.5 micrometers and less than or equal to 3 micrometers.

5. The HEMT epitaxial structure of the GaN single crystal substrate according to claim 1, characterized in that: The thickness of each InN layer in the InN / GaN superlattice layer is greater than 0 nanometers and less than or equal to 10 nanometers, and the thickness of each GaN layer is greater than or equal to 50 nanometers and less than or equal to 100 nanometers. The number of cycles of the InN / GaN superlattice is greater than or equal to 15 and less than or equal to 30.

6. The HEMT epitaxial structure of the GaN single crystal substrate according to claim 1, characterized in that: The GaN high resistance layer is an externally doped C-GaN layer, and the C doping concentration in the C-GaN layer is greater than or equal to 5E18cm -3 and less than or equal to 1E19cm -3 , the thickness of the C-GaN layer is greater than or equal to 500 nanometers and less than or equal to 1500 nanometers; or, The GaN high resistance layer is a Mg-doped P-GaN layer, and the hole concentration of the P-GaN layer is greater than or equal to 5E16cm -3 and less than or equal to 5E17cm -3 , the thickness of the P-GaN layer is greater than or equal to 500 nanometers and less than or equal to 1000 nanometers.

7. The HEMT epitaxial structure of the GaN single crystal substrate according to claim 1, characterized in that: The Al y Ga 1-y The thickness of the N back barrier layer is greater than or equal to 50 nanometers and less than or equal to 150 nanometers; and / or the thickness of the GaN channel layer is greater than or equal to 150 nanometers and less than or equal to 300 nanometers; and / or the Al z Ga 1-z The thickness of the N barrier layer is greater than or equal to 15 nanometers and less than or equal to 30 nanometers; and / or the thickness of the GaN cap layer is greater than or equal to 1 nanometer and less than or equal to 3 nanometers.

8. A method for HEMT epitaxy on a GaN single crystal substrate, characterized in that: The following steps are involved: S1, providing a GaN single crystal substrate, and epitaxially growing a GaN buffer layer on the GaN single crystal substrate; S2, epitaxially growing a low-temperature stress regulating layer on the GaN buffer layer, wherein the low-temperature stress regulating layer is In x Ga 1-x N solid solution thin film layer and / or InN / GaN superlattice layer, wherein 0≤x≤0.1; S3, epitaxially growing a GaN high resistance layer on the low temperature stress regulating layer; S4, growing Al on the GaN high resistance layer y Ga 1-y N back barrier layer, where 0.05≤y≤0.15; S5, in the Al y Ga 1-y A GaN channel layer is grown on the N back barrier layer; S6, growing Al on the GaN channel layer z Ga 1-z N barrier layer, where 0.2≤z≤0.3; S7, in the Al z Ga 1-z A GaN cap layer is grown on the N barrier layer.

9. The HEMT epitaxial growth method of a GaN single crystal substrate according to claim 8, characterized in that: The growth pressure of the low temperature stress regulation layer is greater than or equal to 100 mbar and less than or equal to 300 mbar, and the growth temperature of the low temperature stress regulation layer is greater than or equal to 750 degrees Celsius and less than or equal to 850 degrees Celsius; the GaN high resistance layer has a first growth setting pressure, the first growth setting pressure is greater than or equal to 50 mbar and less than or equal to 200 mbar, and the GaN high resistance layer has a first growth setting temperature, the first growth setting temperature is greater than or equal to 900 degrees Celsius and less than or equal to 1050 degrees Celsius; the Al y Ga 1-y The N back barrier layer has a second growth setting pressure, which is greater than or equal to 50 mbar and less than or equal to 100 mbar. y Ga 1-y The N back barrier layer has a second growth setting temperature, which is greater than or equal to 1050 degrees Celsius and less than or equal to 1150 degrees Celsius.

10. The HEMT epitaxial growth method of a GaN single crystal substrate according to claim 8, characterized in that: In x Ga 1-x The N solid solution thin film layer is formed by simultaneously introducing ammonia, trimethylgallium and trimethylindium into the GaN buffer layer; the InN / GaN superlattice layer is formed by alternately introducing trimethylgallium and trimethylindium into the GaN buffer layer while introducing ammonia.

11. The HEMT epitaxial growth method of a GaN single crystal substrate according to claim 8, characterized in that: The GaN high resistance layer is an externally doped C-GaN layer, and step S3 includes: growing the GaN high resistance layer by introducing ammonia, trimethylgallium and hexene onto the low temperature stress regulating layer; or, The GaN high resistance layer is a Mg-doped P-GaN layer, and step S3 includes: growing the GaN high resistance layer by introducing ammonia, trimethylgallium and magnesium cyclopentadienyl on the low-temperature stress regulating layer.

Citation Information

Cited By

  • Preparation method of high-quality enhanced gallium nitride epitaxial wafer

    CN121381165A