Preparation method of silicon-carbon negative electrode material, silicon-carbon negative electrode material and secondary battery

Through sanding of silicon powder, carbon sources and dispersants and spray drying heat treatment of spherical additives, spherical silicon carbon negative electrode material is formed, which solves the problems of volume expansion and low conductivity of silicon negative electrode material, and achieves high mechanical strength and electricity Improvement of chemical properties.

CN118983420APending Publication Date: 2024-11-19GUANGDONG KAIJIN NEW ENERGY TECH CORP LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411076056.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The volume expansion of silicon negative electrode materials in lithium-ion batteries is severely caused by capacity attenuation and low conductivity, making it difficult to meet the demand for high magnification. The existing silicon carbon negative electrode materials have irregular morphology, uneven stress distribution and poor circulation performance.

Method used

Nanosilicon slurry is prepared by sand milling silicon powder, carbon source, dispersant and organic solvents. After adding spheroidizing additives, spray-drying is performed. The heat treatment is used to form a spherical precursor, and then the carbon filler and outer carbon are coated to form a triple coat. Structure, improves the stability and conductivity of the material.

Benefits of technology

The spherical structure of silicon-carbon negative electrode material is realized, with uniform stress distribution, improved mechanical strength and electrochemical performance, enhanced cycling stability, avoided side reactions, and improved capacity retention and conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983420A_ABST
    Figure CN118983420A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a silicon-carbon negative electrode material, the silicon-carbon negative electrode material and a secondary battery. The preparation method of the silicon-carbon negative electrode material comprises the following steps: sanding silicon powder, a carbon source, a dispersing agent and an organic solvent to prepare nano silicon slurry; a spheroidizing additive is added into the nanometer silicon slurry to be dispersed to obtain mixed slurry, the mixed slurry is subjected to spray drying to obtain a spherical precursor, the spheroidizing additive is organic salt or organic acid dissolved in an organic solvent, the boiling point of the spheroidizing additive is lower than 500 DEG C, the solubility of the spheroidizing additive in the organic solvent is larger than 20 g / L, and the mass ratio of the silicon powder to the spheroidizing additive is 1: 0.15-1.0; carrying out heat treatment on the spherical precursor at 500-700 DEG C to obtain a first intermediate, and coating the first intermediate with a carbon filling body to obtain a second intermediate; and coating the second intermediate with a carbon outer layer. The silicon-carbon negative electrode material is spherical, not only can effectively inhibit expansion of silicon, but also is uniform in stress distribution and not easy to crack when the silicon is expanded, and has better physical properties and electrochemical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery material preparation, and in particular to a silicon-carbon negative electrode material and a method for preparing the silicon-carbon negative electrode material, and a secondary battery. Background Art

[0002] Lithium-ion batteries have been successfully applied in portable electronic devices, new energy vehicles, energy storage and other fields. With the development of society, the market demand for high energy density and power density lithium-ion batteries is getting higher and higher, while the capacity of graphite is close to the theoretical capacity (372mAh / g). Its theoretical capacity is low and it is difficult to meet the market demand for high energy density lithium-ion batteries. Silicon has received extensive attention due to its high theoretical specific capacity (4200mAh / g), relatively low lithium insertion platform (0.4V), wide resources and environmental friendliness.

[0003] Silicon negative electrode materials have a high theoretical capacity (4200mAh / g) and are abundant in resources. They are ideal negative electrode materials and are currently receiving widespread attention and research in the industry. However, compared with graphite negative electrode materials, silicon negative electrode materials have obvious disadvantages. The volume expansion during the cycle process is extremely high. The volume expansion of Si during the lithium insertion process is greater than 300%, resulting in serious capacity attenuation. Secondly, the electrical conductivity of silicon negative electrode materials is low, making it difficult to meet the needs of fast charging such as high rate.

[0004] Although the industry has adopted carbon coating to produce silicon-carbon negative electrode materials to buffer the volume expansion of silicon and improve the conductivity of the material, the produced silicon-carbon negative electrode materials usually have irregular morphology, uneven stress distribution during lithium insertion expansion, easy rupture of particles, and poor cycle performance. Summary of the invention

[0005] In view of the above problems, the purpose of the present invention is to provide a method for preparing a silicon-carbon negative electrode material, a silicon-carbon negative electrode material, and a secondary battery. The silicon-carbon negative electrode material is spherical, which can not only effectively inhibit the expansion of silicon, but also has uniform stress distribution when silicon expands, is not easy to break, and has better physical and electrochemical properties.

[0006] The first aspect of the present invention provides a method for preparing a silicon-carbon negative electrode material, comprising the following steps.

[0007] (I) preparing nano-silicon slurry by sand grinding silicon powder, a carbon source, a dispersant and an organic solvent;

[0008] (II) adding a spheroidizing additive to the nano-silicon slurry and dispersing the mixture to obtain a mixed slurry, and spray drying the mixed slurry to obtain a spherical precursor, wherein the spheroidizing additive is an organic salt or an organic acid soluble in the organic solvent, and the boiling point of the spheroidizing additive is lower than 500° C. and the solubility in the organic solvent is greater than 20 g / L, and the mass ratio of the silicon powder to the spheroidizing additive is 1:0.15-1.0;

[0009] (III) heat treating the spherical precursor at 500° C. to 700° C. to obtain a first intermediate, and then coating the spherical precursor with a carbon filler to obtain a second intermediate;

[0010] (IV) coating the second intermediate with a carbon outer layer.

[0011] In the preparation method of the silicon-carbon negative electrode material of the present invention, silicon powder, carbon source, dispersant and organic solvent are sand-milled to obtain nano silicon with an oxide layer on the surface, and the nano silicon, carbon source and dispersant are uniformly dispersed in the organic solvent. After the spheroidizing additive is added under the action of the dispersant, it is uniformly dispersed in the mixed slurry. A certain amount of specific spheroidizing additive can change the state of the nano silicon slurry, so that the nano silica gel particles are micro-agglomerated to avoid the formation of a dense shell layer on the surface during subsequent spray drying, resulting in loose and easy collapse inside, so a spherical precursor can be obtained. The dispersant and spheroidizing additive can be removed by heat treatment, and the carbon source can be carbonized to form a carbon coating inner layer coated on the surface of the nano silicon. The water vapor generated by the thermal decomposition of the spheroidizing additive leads to an increase in the oxygen content on the surface of the nano silicon, and the formed surface oxide layer is beneficial to improving the cycle performance of the material. The first intermediate obtained after the heat treatment is then coated with a carbon filler to fill the gaps in the spherical precursor skeleton to improve the stability and conductivity of the material. Finally, coating with a carbon outer layer can reduce the specific surface area of ​​the material, improve electronic conductivity, hinder side reactions, and inhibit the volume expansion of silicon.

[0012] In some embodiments, the Dv50 of the silicon powder satisfies 1 μm≤Dv50≤10 μm.

[0013] In some embodiments, the silicon content of the silicon powder is ≥ 95 wt.%.

[0014] In some embodiments, the carbon source includes at least one of phenolic resin, citric acid, asphalt, sucrose, glucose, fructose, lignin, tannic acid, and dopamine.

[0015] In some embodiments, the dispersant includes at least one of n-dodecylamine, triethanolamine, isoamyl alcohol, oleic acid, and cycloalkylsulfonic acid.

[0016] In some embodiments, the organic solvent includes at least one of methanol, ethanol, propanol, isopropanol, acetone, toluene, and xylene.

[0017] In some embodiments, the mass ratio of silicon powder, carbon source, dispersant and solvent is 1:0.02-0.15:0.05-0.10:2-10.

[0018] In some embodiments, the sanding speed is 500 rpm to 1500 rpm.

[0019] In some embodiments, the nano-silicon slurry contains nano-silicon, the particle size of the nano-silicon satisfies 50nm≤Dv50≤150nm, Dv100≤400nm, and the oxygen content in the nano-silicon is ≤15wt.%.

[0020] In some embodiments, the organic salt includes at least one of ammonium malate, ammonium citrate, ammonium tartrate, and ammonium succinate.

[0021] In some embodiments, the organic acid includes at least one of propionic acid, acrylic acid, glyceric acid, n-butyric acid, citric acid, tartaric acid, salicylic acid, malic acid, succinic acid, and terephthalic acid.

[0022] In some embodiments, the viscosity of the mixed slurry is 1 mPas to 400 mPas.

[0023] In some embodiments, the mixed slurry has a solid content of 20% to 50%.

[0024] In some embodiments, the linear velocity of the atomizer used in the spray drying is 150 m / s to 250 m / s.

[0025] In some embodiments, the inlet air temperature of the spray drying is 120°C to 200°C.

[0026] In some embodiments, the outlet air temperature of the spray drying is 70°C to 120°C.

[0027] In some embodiments, the spray drying has a spray yield of ≥ 90%.

[0028] In some embodiments, the heat treatment is performed under an inert atmosphere comprising at least one of helium, neon, argon, krypton, and xenon.

[0029] In some embodiments, the heating rate of the heat treatment is 1° C. / min to 5° C. / min.

[0030] In some embodiments, the heat treatment time is 2 hours to 10 hours.

[0031] In some embodiments, the carbon filling body may be filled multiple times.

[0032] In some embodiments, the carbon sources of the carbon filler and the carbon outer layer are each independently a liquid carbon source, a solid carbon source, and a gaseous carbon source.

[0033] In some embodiments, the reaction temperature of coating the carbon filler is 500°C to 700°C.

[0034] In some embodiments, the reaction time of coating the carbon filler is 2 hours to 24 hours.

[0035] In some embodiments, the carbon coating amount of the coated carbon filler is 18 wt.% to 44 wt.% of the second intermediate.

[0036] In some embodiments, the reaction temperature of coating the carbon outer layer is 600°C to 700°C.

[0037] In some embodiments, the carbon coating amount of the carbon-coated outer layer accounts for 3 wt.% to 10 wt.% of the silicon-carbon negative electrode material.

[0038] In some embodiments, the sanding includes coarse grinding and fine grinding.

[0039] In some embodiments, the coarse grinding uses coarse grinding balls, the diameter of the coarse grinding balls is 0.1 mm to 1.0 mm, and the coarse grinding time is 1 h to 8 h.

[0040] In some embodiments, the fine grinding uses fine grinding balls, the diameter of the fine grinding balls is 0.03 mm to 0.20 mm, and the sanding time of the fine grinding is 2 h to 24 h.

[0041] The second aspect of the present invention provides a silicon-carbon negative electrode material. The silicon-carbon negative electrode material comprises a silicon-carbon matrix, a carbon filler and a carbon-coated outer layer, wherein the carbon filler is between the silicon-carbon matrix and the carbon-coated outer layer, the silicon-carbon matrix comprises nano-silicon, a silicon-oxygen layer and a carbon-coated inner layer from the inside to the outside, and the circularity of the silicon-carbon negative electrode material is ≥0.9.

[0042] The silicon-carbon negative electrode material of the present invention has at least the following technical effects.

[0043] (1) The circularity of the silicon-carbon negative electrode material is ≥0.9. It has a spherical structure, which can evenly distribute stress when silicon expands. The material is difficult to break, has high mechanical strength, and has better electrochemical performance such as cycling.

[0044] (2) The triple coating layers of carbon coating outer layer, carbon coating inner layer and carbon filling body can improve the stability of silicon-carbon negative electrode materials. Even if the material is broken, it can prevent side reactions from occurring, thereby improving cycle stability and avoiding cycle diving and other phenomena.

[0045] (3) The silicon oxide layer that wraps the nano-silicon can buffer the volume expansion of silicon and form a protective layer on the surface of the nano-silicon, further preventing the nano-silicon from directly contacting the electrolyte and causing side reactions. The Si-O bond is stronger than the Si-Si bond, which can make the structure of the silicon-carbon negative electrode material more stable.

[0046] In some embodiments, the repose angle of the silicon-carbon negative electrode material is <30°.

[0047] In some embodiments, the compaction density corresponding to the rebound rate inflection point of the silicon-carbon negative electrode material is ≥1.65 g / cm 3 .

[0048] In some embodiments, the pore volume of the silicon-carbon negative electrode material is less than 0.01 cm 3 / g.

[0049] In some embodiments, the ash content of the silicon-carbon negative electrode material is 107% to 141%.

[0050] In some embodiments, the specific surface area of ​​the silicon-carbon negative electrode material is 0.5 m 2 / g to 3.0m 2 / g.

[0051] In some embodiments, the tap density of the silicon-carbon negative electrode material is ≥1.00 g / cm 3 .

[0052] In some embodiments, the compaction density of the silicon-carbon negative electrode material is ≥1.10 g / cm 3 .

[0053] In some embodiments, the true density of the silicon-carbon negative electrode material is 2.00 g / cm 3 Up to 2.20g / cm 3 .

[0054] In some embodiments, the relative true density of the silicon-carbon negative electrode material is K, 0.98≤K≤1.00.

[0055] In some embodiments, the carbon content of the silicon-carbon negative electrode material is 23 wt.% to 49 wt.%.

[0056] In some embodiments, the silicon content of the silicon-carbon negative electrode material is 50 wt.% to 66 wt.%.

[0057] In some embodiments, the oxygen content of the silicon-carbon negative electrode material is 1 wt.% to 10 wt.%.

[0058] In some embodiments, the carbon content of the silicon-carbon negative electrode material is a, the silicon content of the silicon-carbon negative electrode material is b, the oxygen content of the silicon-carbon negative electrode material is c, and 1≤b / (a+c)<2.

[0059] In some embodiments, the first reversible specific capacity of the silicon-carbon negative electrode material is ≥1800 mAh / g.

[0060] In some embodiments, the first coulombic efficiency of the silicon-carbon negative electrode material is ≥88%.

[0061] In some embodiments, the expansion rate of the silicon-carbon negative electrode material after 100 cycles is ≤45%.

[0062] In some embodiments, the capacity retention rate of the silicon-carbon negative electrode material after 100 cycles is ≥95%.

[0063] In some embodiments, the particle size of the silicon-carbon negative electrode material satisfies 1 μm≤Dv50≤10 μm, Dv100≤30 μm, (Dv90-Dv10) / Dv50≤2.0, and D60 / D10≤3.

[0064] In some embodiments, the difference in area ratio of the nano-silicon on the same cut surface of the silicon-carbon negative electrode material is σ1, and σ1≤1%.

[0065] In some embodiments, the size of silicon grains in the silicon-carbon negative electrode material is 1 nm to 15 nm.

[0066] In some embodiments, the silicon-carbon negative electrode material is tested to obtain a differential capacitance curve, and the delithiation peak height between 0.30V and 0.36V is defined as H1, the delithiation peak between 0.43V and 0.47V is defined as H2, and H1 / H2>1.

[0067] In some embodiments, the silicon oxide layer comprises SiO x , 0<x≤2.

[0068] In some embodiments, the area of ​​the nano-silicon in the cross section of the silicon-carbon matrix accounts for 45% to 70%.

[0069] In some embodiments, the pore volume of the silicon carbon matrix is ​​0.2 cm 3 / g to 0.4cm 3 / g.

[0070] In some embodiments, the circularity of the silicon carbon matrix is ​​≥ 0.9.

[0071] In some embodiments, the particle size of the silicon carbon matrix satisfies 1 μm≤Dv50≤10 μm.

[0072] In some embodiments, the tap density of the silicon carbon matrix is ​​≥0.65 g / cm 3 .

[0073] In some embodiments, the carbon coating inner layer accounts for 3 wt.% to 15 wt.% of the silicon-carbon negative electrode material.

[0074] In some embodiments, the silicon-carbon matrix accounts for 54 wt.% to 80 wt.% of the silicon-carbon negative electrode material.

[0075] In some embodiments, the carbon filler accounts for 17 wt.% to 43 wt.% of the silicon-carbon negative electrode material.

[0076] In some embodiments, the carbon coating outer layer accounts for 3 wt.% to 10 wt.% of the silicon-carbon negative electrode material.

[0077] The third aspect of the present invention provides the use of the aforementioned silicon-carbon negative electrode material in negative electrode materials.

[0078] A fourth aspect of the present invention provides a secondary battery, comprising a positive electrode material and a negative electrode material, wherein the negative electrode material comprises the aforementioned silicon-carbon negative electrode material.

[0079] In some embodiments, the positive electrode material includes at least one of a lithium cobalt oxide positive electrode material, a lithium iron phosphate positive electrode material, a lithium nickel cobalt manganese oxide positive electrode material, and a lithium nickel cobalt aluminum oxide positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0080] Figure 1 It is a schematic structural diagram of the silicon-carbon negative electrode material of the present invention.

[0081] Figure 2 This is the SEM image of the first intermediate of Example 1.

[0082] Figure 3 This is the SEM image of the silicon-carbon negative electrode material of Example 1.

[0083] Figure 4 This is the CP diagram of the silicon-carbon negative electrode material of Example 1.

[0084] Figure 5 This is the SEM image of the first intermediate of Comparative Example 1.

[0085] Figure 6 This is the SEM image of the silicon-carbon negative electrode material of Comparative Example 1.

[0086] Figure 7 This is the CP diagram of the silicon-carbon negative electrode material of Comparative Example 1. DETAILED DESCRIPTION

[0087] The silicon-carbon negative electrode material of the present invention can be used alone or mixed with other negative electrode active materials (such as natural graphite, artificial graphite, soft carbon and / or hard carbon, etc.). The silicon-carbon negative electrode material can be applied to secondary batteries, which include positive electrode materials and negative electrode materials. The positive electrode material includes at least one of a lithium cobalt oxide positive electrode material, a lithium iron phosphate positive electrode material, a nickel cobalt manganese oxide positive electrode material, and a nickel cobalt aluminum oxide positive electrode material.

[0088] The structure of the silicon-carbon negative electrode material of the present invention can be Figure 1 An example is given below. Figure 1 As shown, the silicon-carbon negative electrode material 100 includes a silicon-carbon matrix 10, a carbon filler 30 and a carbon coating outer layer 50. The carbon filler 30 is between the silicon-carbon matrix 10 and the carbon coating outer layer 50. The silicon-carbon matrix 10 includes nano-silicon 11, a silicon oxide layer 13 and a carbon coating inner layer 15 from inside to outside.

[0089] The first reversible specific capacity of the silicon-carbon negative electrode material of the present invention is ≥1800mAh / g. As a technical solution, the capacity of the silicon-carbon negative electrode material is 2000mAh / g to 2500mAh / g. As an example, the capacity of the silicon-carbon negative electrode material can be, but is not limited to, 1800mAh / g, 1850mAh / g, 1900mAh / g, 1950mAh / g, 2000mAh / g, 2050mAh / g, 2100mAh / g, 2150mAh / g, 2200mAh / g, 2250mAh / g, 2300mAh / g, 2350mAh / g, 2400mAh / g, 2450mAh / g, 2500mAh / g. The first coulombic efficiency of the silicon-carbon negative electrode material is ≥88%. As a technical solution, the first coulombic efficiency of the silicon-carbon negative electrode material is ≥90%. As an example, the first coulombic efficiency of the silicon-carbon negative electrode material can be, but is not limited to, 88%, 89%, 90%, 91%, 92%, 93%. The expansion rate of the silicon-carbon negative electrode material after 100 cycles is ≤45%, and as an example, it can be, but is not limited to, 45%, 40%, 8%, 36%, 34%, 32%, 30%. The capacity retention rate of the silicon-carbon negative electrode material after 100 cycles is ≥95%, and as an example, it can be, but is not limited to, 95%, 96%, 97%, 98%, 99%.

[0090] The circularity of the silicon-carbon negative electrode material is ≥ 0.9. As an example, the circularity can be, but not limited to, 0.90, 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98. The repose angle of the silicon-carbon negative electrode material is < 30°. As an example, the repose angle can be, but not limited to, 29°, 28°, 27°, 26°, 25°, 24°, 23°, 22°, 21°. The pore volume of the silicon-carbon negative electrode material is less than 0.01 cm 3 / g, as an example, the pore volume can be, but is not limited to, 0.009 cm3 / g, 0.008cm 3 / g, 0.007cm 3 / g, 0.006cm 3 / g, 0.005cm 3 / g, 0.004cm 3 / g, 0.003cm 3 / g, 0.002cm 3 / g, 0.001cm 3 / g. The ash content of the silicon-carbon negative electrode material is 107% to 141%. As an example, the ash content can be, but is not limited to, 107%, 110%, 115%, 120%, 125%, 130%, 135%, 140%, 141%. The specific surface area of ​​the silicon-carbon negative electrode material is 0.5m 2 / g to 3.0m 2 / g, as an example, it can be but not limited to 0.5m 2 / g, 1.0m 2 / g, 1.5m 2 / g, 2.0m 2 / g, 2.5m 2 / g, 3.0m 2 / g. The particle size of the silicon-carbon negative electrode material satisfies 1μm≤Dv50≤10μm, Dv100≤30μm, (Dv90-Dv10) / Dv50≤2.0, and D60 / D10≤3. As a technical solution, the particle size of the silicon-carbon negative electrode material satisfies 1μm≤Dv50≤10μm, Dv100≤30μm, and (Dv90-Dv10) / Dv50≤2.0. The compaction density corresponding to the inflection point of the rebound rate of the silicon-carbon negative electrode material is ≥1.65g / cm 3 , can be but not limited to 1.65g / cm 3 , 1.66g / cm 3 , 1.67g / cm 3 、1.68g / cm 3 , 1.69g / cm 3 , 1.70g / cm 3 The rebound rate inflection point is the critical point of particle crushing. Its compaction density is high, indicating that the material structure is stable and not prone to rupture. The tap density of silicon-carbon negative electrode material is ≥1.00g / cm 3 As an example, the tap density of the silicon-carbon negative electrode material may be, but is not limited to, 1.00 g / cm 3 , 1.05g / cm 3 , 1.10g / cm 3 , 1.15g / cm 3 , 1.20g / cm 3 The true density of silicon-carbon negative electrode material is 2.00g / cm3 Up to 2.20g / cm 3 As an example, the true density of the silicon-carbon negative electrode material may be, but is not limited to, 2.00 g / cm 3 , 2.05g / cm 3 , 2.10g / cm 3 , 2.15g / cm 3 , 2.20g / cm 3 The compaction density of silicon-carbon negative electrode material is ≥1.10g / cm 3 As an example, the compaction density of the silicon-carbon negative electrode material may be, but is not limited to, 1.10 g / cm 3 , 1.20g / cm 3 , 1.40g / cm 3 , 1.40g / cm 3 , 1.50g / cm 3 The relative true density of silicon-carbon negative electrode material is K, 0.98≤K≤1.00. As an example, K can be, but is not limited to, 0.98, 0.99, 1.00. The higher the K value of silicon-carbon negative electrode material, the denser the silicon-carbon negative electrode material is, which reduces the consumption of electrolyte and improves the cycle stability of the material. The calculation formula of K is as follows.

[0091] K = true density / (1.82*carbon content + 2.30*(1-carbon content))

[0092] The carbon content of the silicon-carbon negative electrode material is 23wt.% to 49wt.%, and as an example, it can be, but not limited to, 23wt.%, 25wt.%, 27wt.%, 30wt.%, 33wt.%, 35wt.%, 37wt.%, 40wt.%, 43wt.%, 45wt.%, 47wt.%, 49wt.. The silicon content of the silicon-carbon negative electrode material is 50wt.% to 66wt.%, and as an example, it can be, but not limited to, 50wt.%, 52wt.%, 54wt.%, 56wt.%, 58wt.%, 60wt.%, 63wt.%, 65wt.%, 66wt.%. The oxygen content of the silicon-carbon negative electrode material is 1wt.% to 10wt.%. As an example, it can be but not limited to 1wt.%, 2wt.%, 3wt.%, 4wt.%, 5wt.%, 6wt.%, 7wt.%, 8wt.%, 9wt.%, 10wt.%. The carbon content of the silicon-carbon negative electrode material is a, the silicon content of the silicon-carbon negative electrode material is b, and the oxygen content of the silicon-carbon negative electrode material is c, 1≤b / (a+c)<2. As an example, b / (a+c) can be but not limited to 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9. The area ratio difference of the nano-silicon on the same cross section of the silicon-carbon negative electrode material is σ1, and σ1≤1% indicates that the nano-silicon is evenly distributed in the silicon-carbon negative electrode material. When testing, any 3μm*3μm area on the cross section can be selected for calculation. The silicon-oxygen layer of the silicon-carbon negative electrode material contains SiO x , 0<x≤2, which is formed by silicon powder during sand grinding. The size of silicon grains in the silicon-carbon negative electrode material is 1nm to 15nm. As an example, the size can be but not limited to 1nm, 3nm, 5nm, 7nm, 9nm, 11nm, 31nm, 15nm. The differential capacitance curve of the silicon-carbon negative electrode material is tested, and the delithiation peak height of 0.30V to 0.36V is defined as H1, and the delithiation peak of 0.43V to 0.47V is defined as H2, H1 / H2>1, indicating that the preparation method of the present invention is beneficial to inhibiting Li 3.75 Formation of Si.

[0093] The area of ​​nano-silicon in the cross section of the silicon-carbon matrix accounts for 45% to 70%. As an example, the area of ​​nano-silicon can be, but is not limited to, 45%, 50%, 55%, 60%, 65%, and 70%. The pore volume of the silicon-carbon matrix is ​​0.2 cm 3 / g to 0.4cm 3 / g, as an example, the pore volume can be but is not limited to 0.2cm 3 / g, 0.3cm 3 / g, 0.4cm 3 / . The circularity of the silicon carbon matrix is ​​≥0.9. As an example, the circularity can be, but not limited to, 0.90, 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98. The particle size of the silicon carbon matrix satisfies 1μm≤Dv50≤10μm. As an example, Dv50 can be, but not limited to, 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm. The tap density of the silicon carbon matrix is ​​≥0.65g / cm 3 As an example, the tap density of the silicon carbon matrix can be, but is not limited to, 0.65 / cm 3 、0.70g / cm 3 , 0.75g / cm 3 , 0.80g / cm 3 , 0.85g / cm 3 . The carbon-coated inner layer accounts for 3wt.% to 15wt.% of the silicon-carbon negative electrode material. As an example, it can be, but not limited to, 3wt.%, 4wt.%, 5wt.%, 6wt.%, 7wt.%, 8wt.%, 9wt.%, 10wt.%, 11wt.%, 12wt.%, 13wt.%, 14wt.%, 15wt.%. The silicon-carbon matrix accounts for 54wt.% to 80wt.% of the silicon-carbon negative electrode material. As an example, it can be, but not limited to, 54wt.%, 60wt.%, 65wt.%, 70wt.%, 75wt.%, 80wt.%. The carbon filler accounts for 17wt.% to 43wt.% of the silicon-carbon negative electrode material. As an example, it can be, but not limited to, 17wt.%, 20wt.%, 25wt.%, 30wt.%, 35wt.%, 40wt.%, 43wt.%. The carbon coating outer layer accounts for 3wt.% to 10wt.% of the silicon-carbon negative electrode material. As an example, it can be but not limited to 3wt.%, 4wt.%, 5wt.%, 6wt.%, 7wt.%, 8wt.%, 9wt.%, 10wt.%.

[0094] The method for preparing the silicon-carbon negative electrode material of the present invention may include the following steps.

[0095] (I) Silicon powder, a carbon source, a dispersant and an organic solvent are sand-ground to prepare nano-silicon slurry.

[0096] (II) adding a spheroidizing additive to the nano-silicon slurry and dispersing the mixture to obtain a mixed slurry, and spray drying the mixed slurry to obtain a spherical precursor.

[0097] (III) The spherical precursor is heat treated to obtain a first intermediate, which is then coated with a carbon filler to obtain a second intermediate.

[0098] (IV) coating the second intermediate with a carbon outer layer.

[0099] Wherein, the Dv50 of silicon powder in step (I) satisfies 1μm≤Dv50≤10μm, as an example, the Dv50 of silicon powder can be but not limited to 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm. The silicon content of silicon powder is ≥95wt.%, as an example, the silicon content of silicon powder can be but not limited to 95wt.%, 96wt.%, 97wt.%, 98wt.%, 99wt.%. The carbon source includes at least one of phenolic resin, citric acid, asphalt, sucrose, glucose, fructose, lignin, tannic acid and dopamine. The dispersant includes at least one of n-dodecylamine, triethanolamine, isoamyl alcohol, oleic acid and cycloalkylsulfonic acid. The organic solvent includes at least one of methanol, ethanol, propanol, isopropanol, acetone, toluene and xylene. The mass ratio of silicon powder, carbon source, dispersant and solvent is 1:0.02-0.15:0.05-0.10:2-10. As an example, the mass ratio of the four can be, but is not limited to, 1:0.02:0.05:2, 1:0.02:0.08:2, 1:0.02:0.10:2, 1:0.02:0.05:5, 1:0.02:0.08:8, 1:0.02:0.10:10, 1:0.08:0.05:2, 1:0.08:0.08:2, 1:0.08:0.10:2, 1:0.08:0.05: 5. 1:0.08:0.08:8, 1:0.08:0.10:10, 1:0.10:0.05:2, 1:0.10:0.08:2, 1:0.10:0.10:2, 1:0.10:0.05:5, 1:0.10:0.08:8, 1:0.10:0.10:10, 1:0.15:0.05:2, 1:0.15:0.08:2, 1:0.15:0.10:2, 1:0.15:0.05:5, 1:0.15:0.08:8, 1:0.15:0.10:10.

[0100] The speed of sanding is 500rpm to 1500rpm, and as an example, it can be but not limited to 500rpm, 600rpm, 700rpm, 800rpm, 900rpm, 1000rpm, 1100rpm, 1200rpm, 1300rpm, 1400rpm, 1500rpm. Sanding includes coarse grinding and fine grinding, and coarse grinding and fine grinding can be carried out simultaneously. Coarse grinding uses coarse grinding balls, and the diameter of the coarse grinding balls is 0.1mm to 1mm, and as an example, it can be but not limited to 0.1mm, 0.2mm, 0.3mm, 0.4mm, 0.5mm, 0.6mm, 0.7mm, 0.8mm, 0.9mm, 1.0mm. The sanding time of coarse grinding is 1h to 8h, and as an example, it can be but not limited to 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h. Fine grinding uses fine grinding balls, and the diameter of the fine grinding balls is 0.03mm to 0.20mm. As an example, it can be but not limited to 0.03mm, 0.05mm, 0.10mm, 0.15mm, 0.20mm. The sanding time of fine grinding is 2h to 24h. As an example, it can be but not limited to 2h, 4h, 6h, 8h, 10h, 12h, 14h, 16h, 18h, 20h, 22h, 24h.

[0101] The nano-silicon slurry contains nano-silicon, and the particle size of the nano-silicon satisfies 50nm≤Dv50≤150nm, Dv100≤400nm, and the oxygen content in the nano-silicon is ≤15wt.%. As an example, Dv50 can be, but is not limited to, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 110nm, 120nm, 130nm, 140nm, 150nm. Dv100 can be, but is not limited to, 100nm, 120nm, 140nm, 160nm, 180nm, 200nm, 220nm, 240nm, 260nm, 280nm, 300nm, 320nm, 340nm, 360nm, 380nm, 400nm. The oxygen content in nano-silicon can be, but is not limited to, 1wt.%, 2wt.%, 3wt.%, 4wt.%, 5wt.%, 6wt.%, 7wt.%, 8wt.%, 9wt.%, 10wt.%, 11wt.%, 12wt.%, 13wt.%, 14wt.%, and 15wt.%.

[0102] In step (II), the spheroidizing additive is an organic salt or organic acid soluble in an organic solvent. The boiling point of the spheroidizing additive is lower than 500°C, and the solubility of the spheroidizing additive in the organic solvent is greater than 20g / L, that is, the solubility of such additive in the organic solvent is better. The organic salt includes at least one of ammonium malate (boiling point is 273.1°C), ammonium citrate (boiling point is 309.6°C), ammonium tartrate (boiling point is 399.3°C) and ammonium succinate (boiling point is 236.1°C). The organic acid includes at least one of propionic acid (boiling point of 141.1°C), acrylic acid (boiling point of 140.9°C), glyceric acid (boiling point of 412.0±30.0°C), butyric acid (boiling point of 162.0°C), citric acid (boiling point of 175.0°C), tartaric acid (boiling point of 399.3±42.0°C), salicylic acid (boiling point of 211.0°C), malic acid (boiling point of 306.4°C), succinic acid (boiling point of 235.0°C) and terephthalic acid (boiling point of 214.3°C). Such organic salts or organic acids can reduce the repulsive effect of nanosilicon silica particles in nanosilicon slurry by changing the pH value and increasing the ionization strength, so that the nanosilicon particles are micro-aggregated, and a dense shell is avoided during spraying, thereby obtaining a spherical precursor. Therefore, such additives can not only adjust the state of nanosilicon slurry and micro-aggregate nanosilicon particles, but also have a low boiling point and can be removed by heat treatment. The mass ratio of silicon powder to spheroidizing additive is 1:0.15-1.0. As an example, the mass ratio can be but not limited to 1:0.15, 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1.0. The amount of spheroidizing additive cannot be too low, otherwise the ionic strength is insufficient, and the morphology of the slurry after spraying can only be slightly improved, and a completely spherical morphology cannot be obtained.

[0103] The viscosity of the mixed slurry is 1mPas to 400mPas. As an example, the viscosity can be but not limited to 1mPas, 50mPas, 100mPas, 150mPas, 200mPas, 250mPas, 300mPas, 350mPas, 400mPas. The viscosity should not be too large, otherwise it will affect the self-assembly of the material, easily form a hollow or internal concave structure, and easily cause the spray pipe to be blocked, and spray drying cannot be performed normally. The solid content of the mixed slurry is 20% to 50%. As an example, the solid content can be but not limited to 20%, 25%, 30%, 35%, 40%, 45%, 50%. The solid content should not be too high, otherwise the viscosity is too high and the pipeline is easily blocked, and normal spraying cannot be performed. If the solid content is too small, it is easy to form a shell layer on the surface of the particles during spray drying, resulting in internal looseness and irregular structure after drying. The linear speed of the atomizer used in spray drying is 150m / s to 250m / s. As an example, the linear speed can be, but not limited to, 150m / s, 160m / s, 170m / s, 180m / s, 190m / s, 200m / s, 210m / s, 220m / s, 230m / s, 240m / s, 250m / s. The inlet air temperature of spray drying is 120°C to 200°C. As an example, the inlet air temperature can be, but not limited to, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C. The outlet air temperature of spray drying is 70°C to 120°C. As an example, the outlet air temperature can be, but not limited to, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C. The spray yield of spray drying is ≥90%. As an example, the spray yield can be, but is not limited to, 90%, 91%, 92%, 93%, 94%, or 95%.

[0104] The heat treatment temperature of step (III) is 500°C to 700°C. As an example, the heat treatment temperature may be, but is not limited to, 500°C, 520°C, 540°C, 560°C, 580°C, 600°C, 620°C, 640°C, 660°C, 680°C, and 700°C. A lower heat treatment temperature is beneficial to suppress the Li 3.75 The formation of Si, the cycle performance of the product is higher. The heating rate of the heat treatment is 1°C / min to 5°C / min. As an example, the heating rate can be but not limited to 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min. The time of the heat treatment is 2h to 10h, and can be but not limited to 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h. The heat treatment is carried out under an inert atmosphere, and the inert atmosphere includes at least one of helium, neon, argon, krypton and xenon. The first intermediate obtained is the silicon-carbon matrix in the silicon-carbon negative electrode material.

[0105] The carbon source of the carbon filler is a liquid carbon source, a solid carbon source and a gaseous carbon source. In other words, the carbon filler can be formed by liquid coating, solid coating and gas coating, and the liquid coating, solid coating and gas coating can be carried out in a conventional manner. The liquid coating and solid coating can be carried out in a vacuum furnace to increase the density of the material. The liquid carbon source includes resins and / or polyvinyl pyrrolidone. The solid carbon source includes at least one of asphalt, sucrose, glucose, polyaniline, polyvinyl alcohol and polypyrrole. The gaseous carbon source includes at least one of methane, ethane, acetylene, propane and ethylene. The carbon filler can be formed by multiple fillings. The reaction temperature of the coated carbon filler is 500°C to 700°C, and as an example, it can be but not limited to 500°C, 550°C, 600°C, 650°C, 700°C. The reaction time of the coated carbon filler is 2h to 24h. As an example, the reaction time can be, but not limited to, 2h, 6h, 10h, 14h, 18h, 20h, 22h, 24h. The carbon coating amount of the coated carbon filler accounts for 18wt.% to 44wt.% of the second intermediate. As an example, it can be, but not limited to, 18wt.%, 20wt.%, 25wt.%, 30wt.%, 35wt.%, 40wt.%, 44wt.%.

[0106] The carbon source of the carbon outer layer of step (IV) is a liquid carbon source, a solid carbon source and a gaseous carbon source. In other words, the carbon outer layer can be formed by liquid coating, solid coating and gas coating, and the liquid coating, solid coating and gas coating can be carried out in a conventional manner. The liquid carbon source includes resins and / or polyvinyl pyrrolidone. The solid carbon source includes at least one of asphalt, sucrose, glucose, polyaniline, polyvinyl alcohol and polypyrrole. The gaseous carbon source includes at least one of methane, ethane, acetylene, propane and ethylene. The reaction temperature of the coated carbon outer layer is 600°C to 700°C, and as an example, it can be but not limited to 600°C, 610°C, 620°C, 630°C, 640°C, 650°C, 660°C, 670°C, 680°C, 690°C, 700°C. The carbon coating amount of the carbon outer layer accounts for 3wt.% to 10wt.% of the silicon-carbon negative electrode material. As an example, it can be but not limited to 3wt.%, 4wt.%, 5wt.%, 6wt.%, 7wt.%, 8wt.%, 9wt.%, and 10wt.%.

[0107] In order to better illustrate the purpose, technical scheme and beneficial effects of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be noted that the following implementation method is a further explanation of the present invention and should not be used as a limitation of the present invention. The embodiments of the present invention include a description of the technical scheme of the silicon-carbon negative electrode material and a description of the technical scheme of the preparation method of the silicon-carbon negative electrode material.

[0108] Example 1

[0109] This embodiment is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0110] (I) 10 kg of silicon powder (Dv50 is 5.5 μm, silicon content is 97 wt.%), 0.5 kg of asphalt, 0.5 kg of triethanolamine and 30 kg of ethanol are sand-milled together, firstly coarsely ground with a zirconia ball with a diameter of 0.4 mm for 4 h at a speed of 1000 rpm, and then finely ground with a zirconia ball with a diameter of 0.10 mm for 8 h at a speed of 1500 rpm to obtain a nano-silicon slurry.

[0111] (II) 2 kg of anhydrous malic acid (boiling point of 306.4°C, solubility in ethanol>20 g / L) was added to the nano-silicon slurry and dispersed at 1000 rpm for 1 hour to obtain a mixed slurry with a viscosity of 74 mPas and a solid content of 29%. The mixed slurry was spray dried with an inlet air temperature of 160°C, an outlet air temperature of 90°C, an atomizer linear speed of 180 m / s, a feed rate of 10 kg / h, a spray yield of 91%, and a spherical precursor after cooling.

[0112] (III) The spherical precursor was placed in a box furnace, and the temperature was first raised to 650°C at a heating rate of 1°C / min under a nitrogen atmosphere for 4 hours to obtain a first intermediate. The first intermediate was mixed with asphalt at a ratio of 1:0.6 (the carbon coating increment was about 26.5wt%), and then placed in a vacuum furnace for calcination with a vacuum degree of ≤10Pa, and the temperature was raised to 650°C at a heating rate of 1°C / min for 5 hours to obtain a second intermediate.

[0113] (IV) The second intermediate is loaded into a rotary kiln, heated to 700° C. at a heating rate of 5° C. / min, and coated with acetylene gas, wherein the carbon coating amount accounts for 5 wt.% of the silicon-carbon negative electrode material.

[0114] The first intermediate prepared in Example 1 was subjected to SEM detection, and the results are as follows: Figure 2 The silicon-carbon negative electrode material prepared in Example 1 was subjected to SEM detection, and the results are as follows: Figure 3 As shown by Figure 3 It can be seen that the morphology of the prepared silicon-carbon negative electrode material is spherical and has a high degree of circularity. The silicon-carbon negative electrode material prepared in Example 1 was subjected to CP section testing, and the results are as follows: Figure 4 As shown by Figure 4 It can be seen that the particles of the prepared silicon-carbon negative electrode material are spherical.

[0115] Example 2

[0116] This embodiment is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0117] (I) Same as step (I) of Example 1.

[0118] (II) 4 kg of anhydrous malic acid (boiling point of 306.4°C, solubility in ethanol>20 g / L) was added to the nano-silicon slurry and dispersed at 1000 rpm for 1 hour to obtain a mixed slurry with a viscosity of 74 mPas and a solid content of 32%. The mixed slurry was spray dried with an inlet air temperature of 160°C, an outlet air temperature of 90°C, an atomizer linear speed of 180 m / s, a feed rate of 10 kg / h, a spray yield of 91%, and a spherical precursor after cooling.

[0119] (III) Same as step (III) in Example 1.

[0120] (IV) Same as step (IV) of Example 1.

[0121] Example 3

[0122] This embodiment is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0123] (I) Same as step (I) of Example 1.

[0124] (II) 2 kg of anhydrous succinic acid (boiling point 235.0°C, solubility in ethanol>20 g / L) was added to the nano-silicon slurry and dispersed at 1000 rpm for 1 hour to obtain a mixed slurry with a viscosity of 24.5 mPas and a solid content of 29%. The mixed slurry was spray dried with an inlet air temperature of 160°C, an outlet air temperature of 80°C, an atomizer linear speed of 180 m / s, a feed rate of 10 kg / h, a spray yield of 91%, and a spherical precursor after cooling.

[0125] (III) Same as step (III) in Example 1.

[0126] (IV) Same as step (IV) of Example 1.

[0127] Example 4

[0128] This embodiment is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0129] (I) Same as step (I) of Example 1.

[0130] (II) Add 2kg of ammonium malate (boiling point 273.1°C, solubility in ethanol>20g / L) to the nano-silicon slurry and disperse at 1000rpm for 1h to obtain a mixed slurry with a viscosity of 24.5mPas and a solid content of 29%. The mixed slurry was spray dried with an inlet air temperature of 160°C, an outlet air temperature of 80°C, an atomizer linear speed of 180m / s, a feed rate of 10kg / h, a spray yield of 91%, and a spherical precursor after cooling.

[0131] (III) Same as step (III) in Example 1.

[0132] (IV) Same as step (IV) of Example 1.

[0133] Example 5

[0134] This embodiment is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0135] (I) Same as step (I) of Example 1.

[0136] (II) 2 kg of ammonium succinate (boiling point 236.1°C, solubility in ethanol>20 g / L) was added to the nano-silicon slurry and dispersed at 1000 rpm for 1 hour to obtain a mixed slurry with a viscosity of 24.5 mPas and a solid content of 29%. The mixed slurry was spray dried with an inlet air temperature of 160°C, an outlet air temperature of 80°C, an atomizer linear speed of 180 m / s, a feed rate of 10 kg / h, a spray yield of 91%, and a spherical precursor after cooling.

[0137] (III) Same as step (III) in Example 1.

[0138] (IV) Same as step (IV) of Example 1.

[0139] Example 6

[0140] This embodiment is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0141] (I) Same as step (I) of Example 1.

[0142] (II) Add 2kg of anhydrous malic acid (boiling point of 306.4°C, solubility in ethanol>20g / L) and 1kg of anhydrous tartaric acid (boiling point of 399.3±42.0°C, solubility in ethanol>20g / L) to the nano-silicon slurry and disperse at 1000rpm for 1h to obtain a mixed slurry with a viscosity of 24.5mPas and a solid content of 29%. The mixed slurry was spray-dried with an inlet air temperature of 160°C, an outlet air temperature of 80°C, a linear speed of 180m / s, a feed rate of 10kg / h, a spray yield of 91%, and a spherical precursor after cooling.

[0143] (III) Same as step (III) in Example 1.

[0144] (IV) Same as step (IV) of Example 1.

[0145] Example 7

[0146] This embodiment is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0147] (I) Same as step (I) of Example 1.

[0148] (II) 2 kg of anhydrous malic acid (boiling point of 306.4°C, solubility in ethanol>20 g / L) was added to the nano-silicon slurry and dispersed at 1000 rpm for 1 hour to obtain a mixed slurry, the viscosity of the mixed slurry was 74 mPas, and the solid content was 29%. The mixed slurry was spray-dried, the inlet air temperature was 140°C, the outlet air temperature was 80°C, the linear speed of the atomizer was 200 m / s, the feed amount was 9 kg / h, the spray yield was 90%, and a spherical precursor was obtained after cooling.

[0149] (III) Same as step (III) in Example 1.

[0150] (IV) Same as step (IV) of Example 1.

[0151] Example 8

[0152] This embodiment is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0153] (I) 10 kg of silicon powder (Dv50 is 5.5 μm, silicon content is 97 wt.%), 0.5 kg of asphalt, 0.5 kg of triethanolamine and 20 kg of ethanol are sand-milled together, firstly coarsely ground with a zirconia ball with a diameter of 0.4 mm for 4 h at a speed of 1000 rpm, and then finely ground with a zirconia ball with a diameter of 0.10 mm for 8 h at a speed of 1500 rpm to obtain a nano-silicon slurry.

[0154] (II) Same as step (II) of Example 1.

[0155] (III) Same as step (III) in Example 1.

[0156] (IV) The second intermediate is placed in a rotary kiln, heated to 650° C. at a heating rate of 5° C. / min, and coated with acetylene gas. The carbon coating amount accounts for 8 wt.% of the silicon-carbon negative electrode material.

[0157] Example 9

[0158] This embodiment is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0159] (I) 10 kg of silicon powder (Dv50 is 5.5 μm, silicon content is 97 wt.%), 0.5 kg of asphalt, 0.5 kg of triethanolamine and 30 kg of ethanol are sand-milled together, firstly coarsely ground with a zirconia ball with a diameter of 0.4 mm for 4 h at a speed of 1000 rpm, and then finely ground with a zirconia ball with a diameter of 0.10 mm for 8 h at a speed of 1500 rpm to obtain a nano-silicon slurry.

[0160] (II) 2 kg of anhydrous malic acid (boiling point of 306.4°C, solubility in ethanol>20 g / L) was added to the nano-silicon slurry and dispersed at 1000 rpm for 1 hour to obtain a mixed slurry with a viscosity of 74 mPas and a solid content of 29%. The mixed slurry was spray dried with an inlet air temperature of 160°C, an outlet air temperature of 90°C, an atomizer linear speed of 180 m / s, a feed rate of 10 kg / h, a spray yield of 91%, and a spherical precursor after cooling.

[0161] (III) The spherical precursor was placed in a box furnace, and the temperature was first raised to 650°C at a heating rate of 1°C / min under a nitrogen atmosphere for 4 hours to obtain a first intermediate. The first intermediate was mixed with asphalt at a ratio of 1:0.7 (the carbon coating increment was about 29.0wt%), and then placed in a vacuum furnace for calcination with a vacuum degree of ≤10Pa, and the temperature was raised to 650°C at a heating rate of 1°C / min for 5 hours to obtain a second intermediate.

[0162] (IV) The second intermediate is loaded into a rotary kiln, heated to 700° C. at a heating rate of 5° C. / min, and coated with acetylene gas, wherein the carbon coating amount accounts for 5 wt.% of the silicon-carbon negative electrode material.

[0163] Example 10

[0164] This embodiment is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0165] (I) 10 kg of silicon powder (Dv50 is 8.0 μm, silicon content is 98 wt.%), 1.2 kg of phenolic resin, 1.0 kg of n-dodecylamine and 40 kg of acetone are sand-milled together, firstly coarsely ground with a zirconia ball with a diameter of 0.4 mm for 4 h at a speed of 1000 rpm, and then finely ground with a zirconia ball with a diameter of 0.10 mm for 8 h at a speed of 1500 rpm to obtain a nano-silicon slurry.

[0166] (II) Same as step (II) of Example 1.

[0167] (III) The spherical precursor was placed in a rotary kiln, and the temperature was first raised to 600°C at a heating rate of 8°C / min under a nitrogen atmosphere and kept at this temperature for 5 hours to obtain the first intermediate. The reactants were mixed with asphalt in a ratio of 2:1 (the carbon coating increment was about 26wt%), and then placed in a vacuum furnace for calcination with a vacuum degree of ≤10Pa, and the temperature was raised to 650°C at a heating rate of 1°C / min and kept at this temperature for 5 hours to obtain the second intermediate.

[0168] (IV) Same as step (IV) of Example 1.

[0169] Embodiment 11

[0170] This embodiment is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0171] (I) 10 kg of silicon powder (Dv50 is 5.5 μm, silicon content is 97 wt.%), 0.5 kg of asphalt, 0.5 kg of triethanolamine and 30 kg of ethanol are sand-milled together, firstly coarsely ground for 3 h using a zirconia ball with a diameter of 0.6 mm and a sand mill speed of 1200 rpm, and then finely ground for 16 h using a zirconia ball with a diameter of 0.05 mm and a sand mill speed of 1400 rpm to obtain a nano-silicon slurry.

[0172] (II) 2 kg of anhydrous malic acid (boiling point of 306.4°C, solubility in ethanol>20 g / L) was added to the nano-silicon slurry and dispersed at 1500 rpm for 1 hour to obtain a mixed slurry with a viscosity of 45.1 mPas and a solid content of 29%. The mixed slurry was spray dried with an inlet air temperature of 185°C, an outlet air temperature of 95°C, an atomizer linear speed of 200 m / s, a feed rate of 12 kg / h, a spray yield of 92%, and a spherical precursor after cooling.

[0173] (III) The spherical precursor was placed in a rotary furnace, and the temperature was first increased to 650°C at a heating rate of 3°C / min under an argon atmosphere for 4 hours to obtain a first intermediate. The first intermediate was mixed with asphalt at a ratio of 1:0.6 (the carbon coating increment was about 26.5wt%), and then placed in a vacuum furnace for calcination with a vacuum degree of ≤10Pa, and the temperature was increased to 680°C at a heating rate of 3°C / min for 4 hours to obtain a second intermediate.

[0174] (IV) Same as step (IV) of Example 1.

[0175] Comparative Example 1

[0176] This comparative example is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0177] (I) Same as step (I) of Example 1.

[0178] (II) The mixed slurry was spray-dried, with an inlet air temperature of 160° C., an outlet air temperature of 90° C., an atomizer linear speed of 180 m / s, a feed rate of 10 kg / h, a spray yield of 88%, and a precursor obtained after cooling.

[0179] (III) Same as step (III) in Example 1.

[0180] (IV) Same as step (IV) of Example 1.

[0181] The first intermediate obtained in Comparative Example 1 was subjected to SEM detection, and the results are as follows: Figure 5 The silicon-carbon negative electrode material prepared in Comparative Example 1 was subjected to SEM detection, and the results are as follows: Figure 6 As shown in the figure, the morphology of the prepared silicon-carbon negative electrode material is irregular and has a low circularity. The silicon-carbon negative electrode material prepared in Comparative Example 1 was subjected to CP section testing, and the results are as follows: Figure 7 As shown in the figure, it can be seen that the particles of the prepared silicon-carbon negative electrode material are irregular.

[0182] Comparative Example 2

[0183] This comparative example is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0184] (I) Same as step (I) of Example 1.

[0185] (II) 0.5 kg of anhydrous malic acid (boiling point of 306.4°C, solubility in ethanol>20 g / L) was added to the nano-silicon slurry and dispersed at 1000 rpm for 1 hour to obtain a mixed slurry, the viscosity of the mixed slurry was 74 mPas, and the solid content was 27%. The mixed slurry was spray-dried, the inlet air temperature was 160°C, the outlet air temperature was 90°C, the linear speed of the atomizer was 180 m / s, the feed amount was 10 kg / h, the spray yield was 89%, and the precursor was obtained after cooling.

[0186] (III) Same as step (III) in Example 1.

[0187] (IV) Same as step (IV) of Example 1.

[0188] Comparative Example 3

[0189] This comparative example is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0190] (I) Same as step (I) of Example 1.

[0191] (II) Add 0.5 kg of anhydrous malic acid (boiling point of 306.4°C, solubility in ethanol>20 g / L) and 50 kg of anhydrous ethanol to the nano-silicon slurry and disperse at 1000 rpm for 1 hour to obtain a mixed slurry, the viscosity of the mixed slurry is 32 mPas, and the solid content is 12%. The mixed slurry is spray-dried, the air inlet temperature is 160°C, the air outlet temperature is 90°C, the linear speed of the atomizer is 180 m / s, the feed amount is 10 kg / h, the spray yield is 88%, and the precursor is obtained after cooling.

[0192] (III) Same as step (III) in Example 1.

[0193] (IV) Same as step (IV) of Example 1.

[0194] Comparative Example 4

[0195] This comparative example is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0196] (I) Same as step (I) of Example 1.

[0197] (II) Add 2kg of anhydrous sodium chloride (boiling point 1465.0°C, solubility in ethanol <20g / L) to the nano-silicon slurry and disperse at 1000rpm for 1h to obtain a mixed slurry with a viscosity of 74mPas and a solid content of 29%. The mixed slurry was spray dried with an inlet air temperature of 160°C, an outlet air temperature of 90°C, an atomizer linear speed of 180m / s, a feed rate of 10kg / h, a spray yield of 87%, and a precursor after cooling.

[0198] (III) Same as step (III) in Example 1.

[0199] (IV) Same as step (IV) of Example 1.

[0200] The first intermediates prepared in Examples 1 to 11 and Comparative Examples 1 to 4 were subjected to relevant tests, and the results are shown in Table 1. The silicon-carbon negative electrode materials prepared in Examples 1 to 11 and Comparative Examples 1 to 4 were subjected to various performance tests, and the test conditions were as follows, and the test results are shown in Tables 2 and 4.

[0201] (1) Angle of repose test

[0202] A funnel with a neck length of 4 cm and an inner diameter of 0.6 cm was used to hold the spherical silicon-carbon negative electrode material. The funnel was fixed on an iron frame. The diameter of the test chassis was 10 cm, and the edge was slightly raised. The distance between the bottom of the funnel and the test chassis was 10 cm. The silicon-carbon negative electrode material was dripped onto the test chassis through the funnel to form a conical structure. The cone height was measured with a ruler. The angle of repose was calculated using the formula: tan(a) = cone height / chassis radius

[0203] (2) Circularity test

[0204] ImageJ was used to calculate circularity. First, File>Open to open the FESEM image to be analyzed, (Image>type>8bit) convert the image to 8bit, Adjust>Threshold, adjust the color range, identify the particle morphology, click Apply, Process>Binary>Fill Holes to fill the spheres (there are blanks in the middle of some spheres), Process>Binary>watershed to split the overlapping spheres, then Analyze>Set Measurements, check Shape descriptors, Redirect to select the image name to be processed, click OK, and finally Analyze>Analyze Particles, Size range 100-Infinity, circularity range 0-1.0, show select Masks, check Display results, Exclude on edges, Summarize and Overlay, and click OK. Circ. in the Summary file corresponds to the average circularity (Count≥100 is required).

[0205] (3) Rebound rate inflection point test

[0206] The prepared silicon-carbon negative electrode material was used as the active material, mixed with the aqueous dispersion of acrylonitrile multipolymer (LA132, solid content 15%) and the conductive agent (Super P) in a mass ratio of 92:6:2, and an appropriate amount of water was added as a solvent to adjust the solid content of the slurry to 55%, which was coated on copper foil and vacuum dried to obtain a silicon negative electrode sheet. The density of the silicon-carbon negative electrode material was calculated according to the compaction density of 13.0 g / cm 3 Up to 1.80g / cm 3 Roll compaction (each tap density increases by 0.5 g / cm 3 ), test the roller thickness, calculate the rebound rate, make a compaction density-rebound rate curve, and obtain the rebound rate inflection point (i.e. the critical point of particle crushing).

[0207] (4) Calculation of silicon area ratio

[0208] ImageJ was used to calculate the silicon area percentage. First, File>Open to open the FESEM image to be analyzed, select the rectangle, select an area in FSEM (the selected area is larger than 3.0μm*3.0μm), (Image>Duplicate...>OK) copy the selected area to form a new image, (Image>type>8bit) convert the image to 8bit, Adjust>Threshold, adjust the color range, identify the morphology of silicon particles, click apply, and then Analyze>Measurements to obtain the area of ​​silicon particles Area, silicon particle area percentage = Area / area of ​​selected area (length*width).

[0209] (5) Aperture test

[0210] The pore size analysis was performed using an ASAP2460 multi-station fully automatic specific surface area and pore size analyzer. The test mode was Micropore Analysis, the degassing temperature was 300°C, the degassing time was 6h, the pressure value was 69 points, and the low-pressure air intake was 10CC.

[0211] (6) Density test

[0212] The true density was measured using a 1200e true density tester, with a gas pressure of 0.14Mpa to 0.15Mpa, a weighing volume of 80% of the sample cell, and 5 test data with RSD ≤ 0.02%.

[0213] The tap density was measured using a BT-312 tap density tester, with the sample height in the measuring cylinder ranging from 21 mL to 25 mL, a vibration frequency of 250 times / min, and 5000 vibrations.

[0214] The compaction density refers to the standard GB / T24533-2019, using the UTM7305 battery powder compaction density meter, sample mass 1g, pressure 10KN, displacement 10mm / min.

[0215] (7) Use a specific surface area analyzer to measure the specific surface area.

[0216] (8) Use a carbon-sulfur analyzer to test the carbon content of the silicon-carbon negative electrode material.

[0217] (9) Oxygen and carbon content was tested by oxygen-nitrogen and carbon-sulfur testers, and silicon and metal content was tested by XRF.

[0218] (10) Electrochemical test

[0219] The prepared silicon-carbon negative electrode material was used as the active material, mixed with the aqueous dispersion of the binder acrylonitrile multipolymer (LA132, solid content 15%) and the conductive agent (Super P) in a mass ratio of 92:6:2, and an appropriate amount of water was added as a solvent to adjust the solid content of the slurry to 55%, which was coated on a copper foil, and vacuum dried and rolled to prepare a negative electrode sheet. A metal lithium sheet was used as the counter electrode, 1 mol / L LiPF6 and a three-component mixed solvent of EC:DMC:EMC=1:1:1 (v / v / v) were used to form an electrolyte, and a polypropylene microporous membrane was used as a diaphragm to assemble a CR2032 button cell in a glove box filled with inert gas. The charge and discharge test of the button cell was carried out on a LANHE battery test system.

[0220] The first charge and discharge performance test: At room temperature, discharge at a constant current of 0.1C to a voltage of 0.01V, then discharge at a constant current of 0.02C to a voltage of 0.005V, and charge at a constant current of 0.1C to a voltage of 1.5V to obtain the first reversible specific capacity and the first coulombic efficiency.

[0221] Cycle performance test: Under room temperature conditions, 1C constant current charge and discharge to 0.01V, then 0.05C constant current discharge to 0.005V, and finally 1C constant current charge to 1.5V to obtain the lithium desorption specific capacity. This cycle is repeated 100 times, and the capacity retention rate and expansion rate after 100 cycles are calculated.

[0222] Table 1 Performance tests of the first intermediates obtained in Examples 1 to 11 and Comparative Examples 1 to 4

[0223]

[0224] From the results in Table 1, it can be seen that the first intermediate obtained by spheroidizing the nanosilicon slurry with a specific organic salt or organic acid and spray drying and heat treating is spherical. Not only does the area of ​​the nanosilicon in the cross section of the first intermediate account for a high proportion, but the particle size and pore volume are small and the tap density is high, indicating that the structure of the first intermediate is relatively dense and the silicon packing density is relatively high.

[0225] Table 2 Performance tests of silicon-carbon composite materials obtained in Examples 1 to 11 and Comparative Examples 1 to 4 (I)

[0226]

[0227]

[0228] Table 3 Performance tests of silicon-carbon composite materials of Examples 1 to 11 and Comparative Examples 1 to 4 (II)

[0229]

[0230] Table 4 Various performance tests of silicon-carbon composite materials of Examples 1 to 11 and Comparative Examples 1 to 4 (III)

[0231]

[0232] From the results in Tables 2 to 4, it can be seen that the silicon-carbon composite materials prepared in Examples 1 to 11 have a higher circularity, higher density values, and smaller pore volume and particle size, indicating that the material is dense and has a stable structure that is not easy to break, and its corresponding electrochemical performance is also better.

[0233] In Comparative Example 1, no spheroidizing additive was added, and a spherical silicon-carbon precursor could not be obtained, so the performance of the obtained silicon-carbon composite material was poor. In Comparative Example 2, the content of the spheroidizing additive added was too little, and the ionic strength was insufficient, so the spray morphology could only be slightly improved, and it was difficult to obtain a spherical silicon-carbon composite material. In Comparative Example 3, not only the amount of spheroidizing additive was small, but also the nano-silicon slurry was diluted, and the viscosity was reduced to fail to obtain a spherical precursor. In Comparative Example 4, sodium chloride was added, and sodium chloride was difficult to dissolve in anhydrous organic solvents, and the solubility did not meet the requirement of >20g / L, so it was difficult to change the state of the nano-silicon slurry, and it was difficult to obtain a spherical precursor by spraying.

[0234] From the comparison of the results of Examples 1 to 3 and Examples 4 and 5 in Tables 2 to 4, it can be seen that compared with organic salts, when the spheroidizing additive is an organic acid, the performance of the obtained silicon-carbon negative electrode material is better. This is because the organic acid adjusts the state of the slurry by adjusting the pH value and increasing the ionic strength, reduces the repulsive force between particles, and improves the sphericity and density after spraying. The organic ammonium salt can only adjust the slurry state by increasing the ionic strength, and the effect is not as good as that of the organic acid. Therefore, with the same addition amount, the sphericity and density obtained by spraying the organic ammonium salt are slightly worse.

[0235] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention is described in detail with reference to the preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing a silicon-carbon negative electrode material, characterized in that: Includes steps: (I) grinding silicon powder, a carbon source, a dispersant and an organic solvent to prepare a nano-silicon slurry; (II) adding a spheroidizing additive to the nano-silicon slurry and dispersing the mixture to obtain a mixed slurry, and spray drying the mixed slurry to obtain a spherical precursor, wherein the spheroidizing additive is an organic salt or an organic acid soluble in the organic solvent, and the boiling point of the spheroidizing additive is lower than 500° C. and the solubility in the organic solvent is greater than 20 g / L, and the mass ratio of the silicon powder to the spheroidizing additive is 1:0.15-1.0; (III) heat treating the spherical precursor at 500° C. to 700° C. to obtain a first intermediate, and then coating the spherical precursor with a carbon filler to obtain a second intermediate; (IV) coating the second intermediate with a carbon outer layer.

2. The method for preparing the silicon-carbon negative electrode material according to claim 1, characterized in that: Includes at least one of the following features (1) to (26): (1) The Dv50 of the silicon powder satisfies 1 μm ≤ Dv50 ≤ 10 μm; (ii) the silicon content of the silicon powder is ≥ 95wt.%; (iii) the carbon source comprises at least one of phenolic resin, citric acid, asphalt, sucrose, glucose, fructose, lignin, tannic acid and dopamine; (iv) the dispersant comprises at least one of n-dodecylamine, triethanolamine, isoamyl alcohol, oleic acid and cycloalkylsulfonic acid; (v) the organic solvent comprises at least one of methanol, ethanol, propanol, isopropanol, acetone, toluene and xylene; (vi) The mass ratio of silicon powder, carbon source, dispersant and solvent is 1:0.02-0.15:0.05-0.10:2-10; (VII) The sanding speed is 500 rpm to 1500 rpm; (VIII) The nano-silicon slurry contains nano-silicon, the particle size of the nano-silicon satisfies 50nm≤Dv50≤150nm, Dv100≤400nm, and the oxygen content of the nano-silicon is ≤15wt.%; (ix) the organic salt includes at least one of ammonium malate, ammonium citrate, ammonium tartrate and ammonium succinate; (j) the organic acid comprises at least one of propionic acid, acrylic acid, glyceric acid, butyric acid, citric acid, tartaric acid, salicylic acid, malic acid, succinic acid and terephthalic acid; (XI) The viscosity of the mixed slurry is 1 mPas to 400 mPas; (XII) The solid content of the mixed slurry is 20% to 50%; (XIII) The linear speed of the atomizer used in the spray drying is 150m / s to 250m / s; (14) The air inlet temperature of the spray drying is 120°C to 200°C; (15) The outlet air temperature of the spray drying is 70°C to 120°C; (XVI) The spray drying spray yield is ≥90%; (17) the heat treatment is carried out under an inert atmosphere, wherein the inert atmosphere comprises at least one of helium, neon, argon, krypton and xenon; (XVIII) The heating rate of the heat treatment is 1°C / min to 5°C / min; (19) The heat treatment time is 2h to 10h; (XX) The carbon filling body may be formed by multiple carbon coatings; (XXI) The carbon sources of the carbon filler and the carbon outer layer are independently a liquid carbon source, a solid carbon source and a gaseous carbon source; (XXII) The reaction temperature of the coated carbon filler is 500°C to 700°C; (XXIII) The reaction time of the coated carbon filler is 2h to 24h; (XXIV) The carbon coating amount of the coated carbon filler is 18wt.% to 44wt.% of the second intermediate; (XXV) The reaction temperature of coating the carbon outer layer is 600°C to 700°C; (Twenty-six) The carbon coating amount of the carbon-coated outer layer accounts for 3wt.% to 10wt.% of the silicon-carbon negative electrode material.

3. The method for preparing the silicon-carbon negative electrode material according to claim 1, characterized in that: The sand grinding includes coarse grinding and fine grinding.

4. The method for preparing the silicon-carbon negative electrode material according to claim 3, characterized in that: The coarse grinding uses coarse grinding balls, the diameter of the coarse grinding balls is 0.1 mm to 1.0 mm, and the coarse grinding time is 1 hour to 8 hours.

5. The method for preparing the silicon-carbon negative electrode material according to claim 3, characterized in that: The fine grinding adopts fine grinding balls, the diameter of the fine grinding balls is 0.03mm to 0.2mm, and the sanding time of the fine grinding is 2h to 24h.

6. The silicon-carbon negative electrode material according to any one of claims 1 to 5, characterized in that: It includes a silicon-carbon matrix, a carbon filler and a carbon-coated outer layer, wherein the carbon filler is between the silicon-carbon matrix and the carbon-coated outer layer, the silicon-carbon matrix includes nano-silicon, a silicon oxide layer and a carbon-coated inner layer from inside to outside, and the circularity of the silicon-carbon negative electrode material is ≥0.

9.

7. The silicon-carbon negative electrode material according to claim 6, characterized in that: The invention comprises at least one of the following features (1) to (31): (1) The repose angle of the silicon-carbon negative electrode material is less than 30°; (2) The compaction density corresponding to the rebound rate inflection point of the silicon-carbon negative electrode material is ≥1.65g / cm 3 ; (3) The pore volume of the silicon-carbon negative electrode material is less than 0.01 cm 3 / g; (4) The ash content of the silicon-carbon negative electrode material is 107% to 141%; (5) The specific surface area of ​​the silicon-carbon negative electrode material is 0.5 m 2 / g to 3.0m 2 / g; (6) The tap density of the silicon-carbon negative electrode material is ≥1.00 g / cm 3 ; (7) The compaction density of the silicon-carbon negative electrode material is ≥1.10 g / cm 3 ; (8) The true density of the silicon-carbon negative electrode material is 2.00 g / cm 3 Up to 2.20g / cm 3 ; (9) The relative true density of the silicon-carbon negative electrode material is K, 0.98≤K≤1.00; (10) The carbon content of the silicon-carbon negative electrode material is 23wt.% to 49wt.%; (11) The silicon content of the silicon-carbon negative electrode material is 50wt.% to 66wt.%; (12) The oxygen content of the silicon-carbon negative electrode material is 1 wt.% to 10 wt.%; (13) The carbon content of the silicon-carbon negative electrode material is a, the silicon content of the silicon-carbon negative electrode material is b, and the oxygen content of the silicon-carbon negative electrode material is c, 1≤b / (a+c)<2; (14) The first reversible specific capacity of the silicon-carbon negative electrode material is ≥ 1800 mAh / g; (15) The first coulombic efficiency of the silicon-carbon negative electrode material is ≥88%; (16) The expansion rate of the silicon-carbon negative electrode material after 100 cycles is ≤45%; (17) The capacity retention rate of the silicon-carbon negative electrode material after 100 cycles is ≥ 95%; (18) The particle size of the silicon-carbon negative electrode material satisfies 1 μm ≤ Dv50 ≤ 10 μm, Dv100 ≤ 30 μm, (Dv90-Dv10) / Dv50 ≤ 2.0, D60 / D10 ≤ 3; (19) The area ratio difference of the nano-silicon on the same section of the silicon-carbon negative electrode material is σ1, σ1≤1%; (20) The size of the silicon grains in the silicon-carbon negative electrode material is 1 nm to 15 nm; (21) Testing the silicon-carbon negative electrode material to obtain a differential capacitance curve, defining the delithiation peak height of 0.30 V to 0.36 V as H1, the delithiation peak height of 0.43 V to 0.47 V as H2, and H1 / H2>1; (22) The silicon oxide layer comprises SiO x , 0<x≤2; (23) The area of ​​the nano-silicon in the cross section of the silicon-carbon matrix accounts for 45% to 70%; (24) The pore volume of the silicon carbon matrix is ​​0.2 cm 3 / g to 0.4cm 3 / g; (25) The circularity of the silicon carbon substrate is ≥ 0.9; (26) The particle size of the silicon carbon matrix satisfies 1 μm ≤ Dv50 ≤ 10 μm; (27) The tap density of the silicon carbon matrix is ​​≥ 0.65 g / cm 3 ; (28) The carbon coating inner layer accounts for 3wt.% to 15wt.% of the silicon-carbon negative electrode material; (29) The silicon-carbon matrix accounts for 54 wt.% to 80 wt.% of the silicon-carbon negative electrode material; (30) The carbon filler accounts for 17wt.% to 43wt.% of the silicon-carbon negative electrode material; (31) The carbon coating outer layer accounts for 3wt.% to 10wt.% of the silicon-carbon negative electrode material.

8. Use of the silicon-carbon negative electrode material prepared by the method for preparing the silicon-carbon negative electrode material according to claim 1 or 2, or the silicon-carbon negative electrode material according to any one of claims 3 to 7 in negative electrode materials.

9. A secondary battery comprising a positive electrode material and a negative electrode material, characterized in that: The negative electrode material includes the silicon-carbon negative electrode material prepared by the method for preparing the silicon-carbon negative electrode material according to claim 1 or 2, or the silicon-carbon negative electrode material according to any one of claims 3 to 7.

10. The secondary battery according to claim 9, characterized in that: The positive electrode material includes at least one of a lithium cobalt oxide positive electrode material, a lithium iron phosphate positive electrode material, a nickel cobalt manganese oxide positive electrode material and a nickel cobalt aluminum oxide positive electrode material.

Citation Information

Cited By

  • Secondary battery and electrical device

    WO2026118574A1