Polydopamine modified nano chalcopyrite material as well as preparation method and application thereof

By dispersing dopamine hydrochloride with hydrophilic nanochalcopyrite to form polydopamine-modified nanochalcopyrite materials, the problem of insufficient CuFeS2 bactericidal ability in the water environment is solved, and efficient bacterial inactivation in the water environment is achieved, which significantly improves the Sterilization effect.

CN118988349APending Publication Date: 2024-11-22GUANGDONG UNIV OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410421329.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-04-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

When using CuFeS2 in a water environment, part of the heat generated by light and heat will be absorbed by water, which will not effectively inactivate bacteria in the water environment, resulting in weak bactericidal ability.

Method used

By dispersing dopamine hydrochloride and hydrophilic nanochalcopyrite into the alkaline solution, polydopamine-modified nanochalcopyrite materials are formed, and the nanochalcopyrite is wrapped with the adhesion of dopamine to form a material with strong adsorption and promote bacterial It is adsorbed to the surface of the material, so that the heat generated by the light and heat acts directly on the bacteria, and avoids the heat being absorbed by the water medium.

Benefits of technology

It effectively improves the bactericidal ability in the water environment, can quickly inactivate bacteria under the visible water phase system, and significantly improves the killing effect of drug-resistant bacteria.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988349A_ABST
    Figure CN118988349A_ABST
Patent Text Reader

Abstract

The invention discloses a polydopamine modified nano chalcopyrite material and a preparation method and application thereof, and relates to the technical field of water environment sterilization, and the preparation method of the polydopamine modified nano chalcopyrite material comprises the following steps that S1, dopamine hydrochloride and hydrophilic nano chalcopyrite are dispersed into an alkaline solution, and the alkaline solution is stirred to be uniform; mixing and stirring to form a first mixture; and S2, centrifuging, cleaning and drying the first mixture to obtain the polydopamine modified nano chalcopyrite material. The invention provides a polydopamine modified nano chalcopyrite material as well as a preparation method and application thereof, which are used for solving the technical problem that when CuFeS2 is used in a water environment, a part of heat generated by light and heat can be absorbed by water, bacteria in the water environment cannot be effectively inactivated, and the bactericidal ability is relatively weak.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of water environment sterilization, and in particular to a polydopamine modified nano chalcopyrite material and a preparation method and application thereof. Background Art

[0002] The growth of pathogenic microorganisms (including bacteria, parasites, viruses and fungi) in the environment has led to the intensification of environmental microbial pollution. According to estimates by the World Health Organization, hundreds of millions of cases of foodborne diseases worldwide each year are related to the intake of food and drinking water contaminated by pathogenic microorganisms.

[0003] In order to reduce microbial contamination, chalcopyrite is generally used for disinfection and sterilization in the prior art. The chemical formula of chalcopyrite is CuFeS2, which has an optical band gap of 0.5 eV and a tetragonal crystal structure. + and Fe 3+ Coordinated with sulfur in a tetrahedral configuration. CuFeS2 nanoparticles can exhibit localized surface plasmon resonance similar to gold under 2.4eV excitation. CuFeS2 has a wide spectral range and a high molar attenuation coefficient, can absorb more light energy and convert it into heat energy, and has good photothermal catalytic sterilization ability.

[0004] However, when CuFeS2 is used in an aqueous environment, part of the heat generated by photothermal treatment will be absorbed by the water, which cannot effectively inactivate the bacteria in the aqueous environment, resulting in a weaker bactericidal ability. Summary of the invention

[0005] The present invention provides a polydopamine-modified nano chalcopyrite material and a preparation method and application thereof, which are used to solve the technical problem that when CuFeS2 is used in an aqueous environment, part of the heat generated by photothermal heat will be absorbed by water, and the bacteria in the aqueous environment cannot be effectively inactivated, resulting in weak bactericidal ability.

[0006] The present invention provides a method for preparing a polydopamine modified nano chalcopyrite material, comprising the following steps:

[0007] S1, dispersing dopamine hydrochloride and hydrophilic nano chalcopyrite into an alkaline solution, mixing and stirring to form a first mixture;

[0008] S2. Centrifuging, washing and drying the first mixture to obtain a polydopamine-modified nano-chalcopyrite material.

[0009] Preferably, the hydrophilic nano-chalcopyrite is prepared from the hydrophobic nano-chalcopyrite by an aqueous phase conversion method, and the hydrophobic nano-chalcopyrite is prepared by a hot injection method.

[0010] Preferably, the hydrophobic nano chalcopyrite is prepared by a hot injection method, which specifically comprises the following steps:

[0011] S11, mixing and stirring the cuprous compound, the ferric compound and oleylamine to obtain a second mixture;

[0012] S12, heating the second mixture under vacuum until the temperature reaches a first preset threshold range, and continuing stirring until the time reaches a second preset threshold range;

[0013] S13, heating the second mixture under a nitrogen atmosphere until the temperature reaches a third preset threshold range, and continuing stirring until the time reaches a fourth preset threshold range;

[0014] S14, stirring the second mixture at a constant temperature, injecting a 1-octadecene solution of elemental sulfur to mix, and centrifuging to obtain a third mixture;

[0015] S15, after cooling to room temperature under room temperature environment, washing the third mixture, and drying to obtain hydrophobic nano chalcopyrite.

[0016] Preferably, the cuprous compound is one or more of CuI and cuprous acetate;

[0017] The trivalent iron compound is one or more of FeCl3 and Fe(acac)3.

[0018] Preferably, the hydrophilic nano-chalcopyrite is prepared from the hydrophobic nano-chalcopyrite by an aqueous phase conversion method, which specifically comprises the following steps:

[0019] S16, dispersing the hydrophobic nano-chalcopyrite in a dispersant, adding a ligand exchange solution, stirring, centrifuging, washing and drying to obtain the hydrophilic nano-chalcopyrite;

[0020] The preparation method of the ligand exchange solution comprises the following steps:

[0021] Na2S·9H2O is dissolved in water to obtain a Na2S·9H2O aqueous solution, and dimethylformamide is added to the Na2S·9H2O aqueous solution to form the ligand exchange solution.

[0022] Preferably, in S1, the molar ratio of the dopamine hydrochloride to the hydrophilic nano-chalcopyrite is 1 to 2:1;

[0023] The stirring time is 6 to 12 hours, and the stirring temperature is 30 to 50° C.;

[0024] In S2, the centrifugal speed is 5000-8000 rpm, and the centrifugal time is 2-5 min; the drying temperature is 60-80° C., and the drying time is 12-24 h.

[0025] Preferably, in S11, the molar ratio of CuI, FeCl3 and oleylamine is 1:1:90-120;

[0026] In S12, the first preset threshold range is 100-120° C., and the second preset threshold range is 1.5-2h;

[0027] In the S13, the third preset threshold range is 150-180°C, and the fourth preset threshold range is 20-40min;

[0028] In the S14, the method for preparing the elemental sulfur 1-octadecene solution comprises the following steps:

[0029] dissolving elemental sulfur in a 1-octadecene solution at a temperature of 50 to 60° C. to obtain the 1-octadecene solution of elemental sulfur;

[0030] The concentration of the 1-octadecene solution of elemental sulfur is 0.5-0.7 mmol / m, the molar ratio of the elemental sulfur to CuI and FeCl3 is 2:1:1; the elemental sulfur is one or more of sulfur powder, dodecanethiol and hexamethyldisilathione;

[0031] The stirring speed is 150-160 rpm, and the stirring time is 10-20 min;

[0032] In the S15, the washing is performed by washing with a mixture of ethanol and toluene; the volume ratio of the ethanol to the toluene is 1 to 2:1;

[0033] The drying temperature is 50-60° C., and the drying time is 6-12 hours.

[0034] Preferably, in S16, the dispersant is one or more of cyclohexane and hexane; the concentration of the dispersant is 0.02 to 0.05 g / mL;

[0035] The centrifugal speed is 5000-8000 rpm, and the centrifugal time is 2-5 min;

[0036] The cleaning is carried out by using ethanol;

[0037] The drying temperature is 50-60°C and the drying time is 6-12h;

[0038] The concentration of the Na2S·9H2O aqueous solution is 0.02-0.05 g / mL;

[0039] The volume ratio of the Na2S·9H2O aqueous solution to the dimethylformamide is 1:3-5;

[0040] The mass ratio of the hydrophobic nano chalcopyrite to the Na2S·9H2O aqueous solution is 1.5-2:1.

[0041] The polydopamine modified nano chalcopyrite material provided by the present invention is prepared based on the above-mentioned preparation method.

[0042] The invention provides an application of a polydopamine-modified nano-chalcopyrite material for killing bacteria in a visible light aqueous phase system.

[0043] Preferably, the alkaline solution is a tris(hydroxymethyl)aminomethane hydrochloride solution with a pH value of 8 to 8.5.

[0044] The present invention provides a method for preparing a polydopamine-modified nano-chalcopyrite material, which has the following advantages:

[0045] The method comprises the following steps: S1, dispersing dopamine hydrochloride and hydrophilic nano chalcopyrite in an alkaline solution, mixing and stirring to form a first mixture; S2, centrifuging, washing and drying the first mixture to obtain a polydopamine modified nano chalcopyrite material.

[0046] Dopamine hydrochloride and hydrophilic nano-chalcopyrite are dispersed in an alkaline solution. In an alkaline environment, dopamine (DA) can undergo oxidative self-polymerization to form polydopamine (PDA). Polydopamine uses its own adhesion to wrap the hydrophilic nano-chalcopyrite to form a polydopamine-modified nano-chalcopyrite material.

[0047] The PDA structure contains active double bonds that can react chemically with multiple groups, such as amino (-NH2), thiol (-SH), etc. Therefore, molecules containing thiol groups can be connected to the PDA shell to further functionalize the nanomaterial. The PDA structural fragment is a conjugated system with rich π electron clouds that can adsorb small molecules.

[0048] Due to the modification of CuFeS2 by polydopamine, the surface adsorption of the combined polydopamine-modified nano-chalcopyrite material is stronger, which can promote the adsorption of bacteria to the surface of the material, allowing the heat generated by photothermal energy to directly act on the bacteria, avoiding the heat from being absorbed by the water medium in the water environment, and effectively inactivating the bacteria in the water environment, thereby improving the bactericidal ability. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0050] Figure 1 This is an electron microscope image of the polydopamine-modified nano-chalcopyrite material described in an embodiment of the present invention at a resolution of 5 nm;

[0051] Figure 2 This is an electron microscope image of the nano-chalcopyrite material described in an embodiment of the present invention at a resolution of 5 nm;

[0052] Figure 3 This is a photothermal effect diagram of the polydopamine modified nano-chalcopyrite material described in an embodiment of the present invention within 90 seconds;

[0053] Figure 4 This is a diagram showing the killing effect of the polydopamine-modified nano-chalcopyrite material described in an embodiment of the present invention on cefotaxime-resistant Escherichia coli within 90 seconds;

[0054] Figure 5 This is a diagram showing the killing effect of the polydopamine-modified nano-chalcopyrite material and the nano-chalcopyrite material in killing Staphylococcus aureus within 4 minutes according to the embodiments of the present invention;

[0055] Figure 6 This is a diagram showing the killing effect of the polydopamine-modified nano-chalcopyrite material described in an embodiment of the present invention on polymyxin B-resistant Escherichia coli within 10 minutes. DETAILED DESCRIPTION

[0056] In order to make the purpose, features and advantages of the present invention more obvious and easy to understand, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the embodiments described below are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0057] It should be noted that, in the embodiments, those without specifying specific conditions are carried out according to normal conditions or conditions recommended by the manufacturer. Those without specifying the manufacturer of reagents or instruments used are conventional products that can be purchased commercially. In addition, the meaning of "and / or" appearing in the full text includes three parallel schemes, and "A and / or B" is taken as an example, including schemes A, B, or A and B that meet the same time. In addition, the technical schemes between the various embodiments can be combined with each other, but must be based on the ability of ordinary technicians in the field to achieve. When the combination of the technical schemes is contradictory or cannot be achieved, it should be considered that the combination of such technical schemes does not exist, and is not within the scope of protection required by the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work, all belong to the scope of protection of the present invention.

[0058] The present invention provides a polydopamine-modified nano chalcopyrite material and a preparation method and application thereof, which are used to solve the technical problem that when CuFeS2 is used in an aqueous environment, part of the heat generated by photothermal heat will be absorbed by water, and the bacteria in the aqueous environment cannot be effectively inactivated, resulting in weak bactericidal ability.

[0059] See also Figure 1 An embodiment of the present invention provides a method for preparing a polydopamine-modified nano-chalcopyrite material, comprising the following steps:

[0060] S1, dispersing dopamine hydrochloride and hydrophilic nano chalcopyrite into an alkaline solution, mixing and stirring to form a first mixture;

[0061] S2. Centrifuge, wash and dry the first mixture to obtain a polydopamine-modified nano-chalcopyrite material.

[0062] It should be noted that when dopamine hydrochloride and hydrophilic nano-chalcopyrite are dispersed in an alkaline solution, dopamine (DA) can undergo oxidative self-polymerization to form polydopamine (PDA) in an alkaline environment, and polydopamine uses its own adhesion to wrap the hydrophilic nano-chalcopyrite to form a polydopamine-modified nano-chalcopyrite material.

[0063] The PDA structure contains active double bonds that can react chemically with multiple groups, such as amino (-NH2), thiol (-SH), etc. Therefore, molecules containing thiol groups can be connected to the PDA shell to further functionalize the nanomaterial. The PDA structural fragment is a conjugated system with rich π electron clouds that can adsorb small molecules.

[0064] Due to the modification of CuFeS2 by polydopamine, the surface adsorption of the combined polydopamine-modified nano-chalcopyrite material is stronger, which can promote the adsorption of bacteria to the surface of the material, allowing the heat generated by photothermal energy to directly act on the bacteria, avoiding the heat from being absorbed by the water medium in the water environment, and effectively inactivating the bacteria in the water environment, thereby improving the bactericidal ability.

[0065] The alkaline solution is a tris(hydroxymethyl)aminomethane hydrochloride solution with a pH value of 8 to 8.5.

[0066] In a more specific embodiment, the hydrophilic nano-chalcopyrite is prepared from the hydrophobic nano-chalcopyrite by an aqueous phase conversion method, and the hydrophobic nano-chalcopyrite is prepared by a hot injection method.

[0067] It should be noted that the hot injection method mainly heats the sample to a high temperature state, and then cools the sample at an extremely fast cooling rate to change the structure of the sample.

[0068] The hot injection method is to synthesize and prepare nano chalcopyrite in an organic solvent, so the prepared nano chalcopyrite is hydrophobic. The hydrophobic nano chalcopyrite prepared by this preparation method has high purity.

[0069] The hydrophobic nano-chalcopyrite is transformed into hydrophilic nano-chalcopyrite through the aqueous phase conversion method, so that it can be better dispersed in the alkaline solution. Dopamine can only be polymerized into polydopamine when it is dispersed in the alkaline solution. Therefore, hydrophilic nano-chalcopyrite and polydopamine can be combined in the same system to form polydopamine-modified nano-chalcopyrite materials.

[0070] In a more specific embodiment, the hydrophobic nano-chalcopyrite is prepared by a hot injection method, which specifically comprises the following steps:

[0071] S11, mixing and stirring the cuprous compound, the ferric compound and oleylamine to obtain a second mixture;

[0072] S12, heating the second mixture under vacuum until the temperature reaches a first preset threshold range, and continuing stirring until the time reaches a second preset threshold range;

[0073] S13, heating the second mixture under a nitrogen atmosphere until the temperature reaches a third preset threshold range, and continuing stirring until the time reaches a fourth preset threshold range;

[0074] S14, stirring the second mixture at a constant temperature, injecting a 1-octadecene solution of elemental sulfur to mix, and centrifuging to obtain a third mixture;

[0075] S15, after cooling to room temperature under room temperature environment, washing the third mixture, and drying to obtain hydrophobic nano chalcopyrite.

[0076] It should be noted that in S11, the cuprous compound, the ferric compound and oleylamine are mixed and stirred in a round-bottom flask;

[0077] Adding oleylamine to the cuprous compound and the ferric iron compound to obtain a second mixture, wherein the oleylamine is used to control the size and shape of the nanoparticles and prevent their aggregation, and finally obtaining hydrophobic nano-chalcopyrite modified with oleylamine ligands;

[0078] In S12, heating under vacuum refers to heating under vacuum, which can remove water and oxygen in the reaction device and the solvent while heating;

[0079] In S13, the temperature is increased and heated in a nitrogen atmosphere to dissolve the metal precursor and provide an oxygen-free environment.

[0080] In a more specific embodiment, the cuprous compound is one or more of CuI and cuprous acetate;

[0081] The trivalent iron compound is one or more of FeCl3 and Fe(acac)3.

[0082] It should be noted that, preferably, the cuprous compound is CuI and the ferric iron compound is FeCl3.

[0083] In a more specific embodiment, the hydrophilic nano-chalcopyrite is prepared from the hydrophobic nano-chalcopyrite by an aqueous phase conversion method, which specifically includes the following steps:

[0084] S16, dispersing the hydrophobic nano-chalcopyrite in a dispersant, adding a ligand exchange solution, stirring, centrifuging, washing and drying to obtain the hydrophilic nano-chalcopyrite;

[0085] The method for preparing the ligand exchange solution comprises the following steps:

[0086] Na2S·9H2O is dissolved in water to obtain a Na2S·9H2O aqueous solution, and dimethylformamide is added to the Na2S·9H2O aqueous solution to form a ligand exchange solution.

[0087] It should be noted that the hydrophobic nano-chalcopyrite is dispersed in a dispersant to facilitate ligand exchange;

[0088] Na2S·9H2O is dissolved in ultrapure water to obtain a Na2S·9H2O aqueous solution. Dimethylformamide is added to the Na2S·9H2O aqueous solution to form a ligand exchange solution, which is a sulfide ligand exchange solution that can convert hydrophobic nano-chalcopyrite into a sulfide ligand exchange solution. 2- Ligand-bound hydrophilic nanocrystal.

[0089] In a more specific embodiment, in S1, the molar ratio of dopamine hydrochloride to hydrophilic nano-chalcopyrite is 1-2:1;

[0090] The stirring time is 6 to 12 hours, and the stirring temperature is 30 to 50°C;

[0091] In S2, the centrifugal speed is 5000-8000 rpm, and the centrifugal time is 2-5 min; the drying temperature is 60-80° C., and the drying time is 12-24 h.

[0092] In a more specific embodiment, in S11, the molar ratio of CuI, FeCl3 and oleylamine is 1:1:90-120;

[0093] In S12, the first preset threshold range is 100-120°C, and the second preset threshold range is 1.5-2h;

[0094] In S13, the third preset threshold range is 150-180°C, and the fourth preset threshold range is 20-40min;

[0095] In S14, the method for preparing the 1-octadecene solution of elemental sulfur comprises the following steps:

[0096] dissolving elemental sulfur in a 1-octadecene solution at a temperature of 50 to 60° C. to obtain a 1-octadecene solution of elemental sulfur;

[0097] The concentration of the 1-octadecene solution of elemental sulfur is 0.5-0.7 mmol / m, and the molar ratio of elemental sulfur to CuI and FeCl3 is 2:1:1; the elemental sulfur is one or more of sulfur powder, dodecanethiol and hexamethyldisilathione;

[0098] The stirring speed is 150-160 rpm, and the stirring time is 10-20 min;

[0099] In S15, washing is performed by using a mixture of ethanol and toluene; the volume ratio of ethanol to toluene is 1 to 2:1;

[0100] The drying temperature is 50-60°C and the drying time is 6-12 hours.

[0101] In a more specific embodiment, in S16, the dispersant is one or more of cyclohexane and hexane; the concentration of the dispersant is 0.02 to 0.05 g / mL;

[0102] The centrifugal speed is 5000-8000 rpm, and the centrifugal time is 2-5 minutes;

[0103] Cleaning is done by using ethanol;

[0104] The drying temperature is 50-60°C and the drying time is 6-12 hours;

[0105] The concentration of Na2S·9H2O aqueous solution is 0.02-0.05 g / mL;

[0106] The volume ratio of Na2S·9H2O aqueous solution to dimethylformamide is 1:3-5;

[0107] The mass ratio of hydrophobic nano-chalcopyrite to Na2S·9H2O aqueous solution is 1.5-2:1.

[0108] An embodiment of the present invention provides a polydopamine-modified nano-chalcopyrite material, which is prepared based on the above-mentioned preparation method.

[0109] An embodiment of the present invention provides an application of a polydopamine-modified nano-chalcopyrite material in killing bacteria under a visible light aqueous system.

[0110] Please note that Figure 3 , Figure 3This is a photothermal effect diagram of the polydopamine-modified nano-chalcopyrite material in Example 1 within 90 seconds. As can be seen from the figure, the photothermal catalyst has good photothermal performance, and can reach 80°C within 90 seconds under visible light, overcoming the limitations of single photocatalysis and single thermal catalysis, and showing the significant advantages of photothermal synergistic catalysis. Therefore, the application of polydopamine-modified nano-chalcopyrite material in photothermal synergistic killing of bacteria in visible light water phase system has great potential.

[0111] Bacteria include Escherichia coli, Staphylococcus aureus, Salmonella, etc. In the fields of medical wastewater treatment, polydopamine-modified nano-chalcopyrite materials have broad application potential as bactericidal catalysts.

[0112] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments and drawings. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.

[0113] Example 1

[0114] The embodiment of the present invention provides a polydopamine modified nano chalcopyrite material, and the preparation method comprises the following steps:

[0115] S11, mixing 1 mmol of CuI, 1 mmol of FeCl3 and 90 mmol of oleylamine to obtain a second mixture;

[0116] S12, heating the second mixture under vacuum to a temperature of 100° C., and continuously stirring for 1.5 h to react;

[0117] S13, heating the second mixture to 150° C. under a nitrogen atmosphere, and stirring at a rotation speed of 160 rpm for 20 min to react;

[0118] S14, dissolving elemental sulfur in a 1-octadecene solution at a temperature of 50° C. to obtain a 0.5 mmol / mL elemental sulfur 1-octadecene solution;

[0119] The second mixture was stirred at a constant temperature at a rotation speed of 160 rpm, and 3 mL of a 1-octadecene solution of elemental sulfur was quickly injected for mixing, and after maintaining for 10 minutes, the mixture was centrifuged at a rotation speed of 5000 rpm for 2 minutes to obtain a third mixture;

[0120] S15, after cooling to room temperature under room temperature environment, washing the third mixture precipitate twice with a mixture of ethanol and toluene in a volume ratio of 1:1, and vacuum drying at a temperature of 50° C. for 6 hours to obtain hydrophobic nano chalcopyrite;

[0121] S16, dissolving 0.1 g of Na2S·9H2O in 5 mL of ultrapure water to obtain a Na2S·9H2O aqueous solution, and adding 15 mL of dimethylformamide to the Na2S·9H2O aqueous solution to form a ligand exchange solution;

[0122] 0.2 g of hydrophobic nano-chalcopyrite was dispersed in 10 mL of cyclohexane, the ligand exchange solution was added and stirred, centrifuged at 5000 rpm for 5 min, washed with ethanol, dried at 60° C. for 6 h, and then ground to obtain hydrophilic nano-chalcopyrite;

[0123] S1. Ultrasonic dispersion of 100 mg of dopamine hydrochloride and 100 mg of hydrophilic nano-chalcopyrite into 100 mL of Tris-HCL (tris(hydroxymethyl)aminomethane hydrochloride)) solution, mixing and magnetically stirring at 30° C. for 6 h to form a first mixture;

[0124] S2. The first mixture was centrifuged at a rotation speed of 8000 rpm for 5 min, washed, dried at a temperature of 60° C. for 12 h, and then ground to obtain a polydopamine-modified nano-chalcopyrite material (CuFeS 2 / PDA).

[0125] Example 2

[0126] The embodiment of the present invention provides a polydopamine modified nano chalcopyrite material, and the preparation method comprises the following steps:

[0127] S11, 4 mmol of CuI, 4 mmol of FeCl3 and 480 mmol of oleylamine were mixed and stirred to obtain a second mixture;

[0128] S12, heating the second mixture under vacuum to a temperature of 120° C., and continuously stirring for 2 h to react;

[0129] S13, heating the second mixture to 180° C. under a nitrogen atmosphere, and stirring at a rotation speed of 160 rpm for 40 min to react;

[0130] S14, dissolving elemental sulfur in a 1-octadecene solution at a temperature of 60° C. to obtain a 0.7 mmol / mL elemental sulfur 1-octadecene solution;

[0131] The second mixture was stirred at a constant temperature at a rotation speed of 150 rpm, and 15 mL of a 1-octadecene solution of elemental sulfur was quickly injected for mixing, and after maintaining for 20 minutes, the mixture was centrifuged at a rotation speed of 8000 rpm for 5 minutes to obtain a third mixture;

[0132] S15, after cooling to room temperature under room temperature environment, washing the third mixture precipitate twice with a mixture of ethanol and toluene in a volume ratio of 1:2, and vacuum drying at a temperature of 60° C. for 6 h to obtain hydrophobic nano chalcopyrite;

[0133] S16, dissolving 0.25 g of Na2S·9H2O in 5 mL of ultrapure water to obtain a Na2S·9H2O aqueous solution, and adding 25 mL of dimethylformamide to the Na2S·9H2O aqueous solution to form a ligand exchange solution;

[0134] 0.375 g of hydrophobic nano-chalcopyrite was dispersed in 7.5 mL of cyclohexane, the ligand exchange solution was added and stirred, centrifuged at 8000 rpm for 5 min, washed with ethanol, dried at 60° C. for 12 h, and then ground to obtain hydrophilic nano-chalcopyrite;

[0135] S1, ultrasonically dispersing 200 mg of dopamine hydrochloride and 100 mg of hydrophilic nano-chalcopyrite into 100 mL of Tris-HCL (tris(hydroxymethyl)aminomethane hydrochloride)) solution, mixing and magnetically stirring at a temperature of 50° C. for 12 h to form a first mixture;

[0136] S2. The first mixture was centrifuged at a rotation speed of 8000 rpm for 5 min, washed, dried at a temperature of 80° C. for 24 h, and then ground to obtain a polydopamine-modified nano-chalcopyrite material (CuFeS 2 / PDA).

[0137] Example 3

[0138] The embodiment of the present invention provides a polydopamine modified nano chalcopyrite material, and the preparation method comprises the following steps:

[0139] S11, mixing and stirring 1 mmol of CuI, 1 mmol of FeCl3 and 100 mmol of oleylamine to obtain a second mixture;

[0140] S12, heating the second mixture under vacuum to a temperature of 110° C., and continuously stirring for 2 h to react;

[0141] S13, heating the second mixture to 160° C. under a nitrogen atmosphere, and stirring at a rotation speed of 150 rpm for 30 min to react;

[0142] S14, dissolving elemental sulfur in a 1-octadecene solution at a temperature of 55° C. to obtain a 0.6 mmol / mL elemental sulfur 1-octadecene solution;

[0143] The second mixture was stirred at a constant temperature at a rotation speed of 150 rpm, and 5 mL of a 1-octadecene solution of elemental sulfur was quickly injected for mixing, and after maintaining for 15 minutes, the mixture was centrifuged at a rotation speed of 8000 rpm for 5 minutes to obtain a third mixture;

[0144] S15, after cooling to room temperature under room temperature environment, washing the third mixture precipitate twice with a mixture of ethanol and toluene in a volume ratio of 1:1, and vacuum drying at a temperature of 60° C. for 6 h to obtain hydrophobic nano chalcopyrite;

[0145] S16, dissolving 0.1 g of Na2S·9H2O in 5 mL of ultrapure water to obtain a Na2S·9H2O aqueous solution, and adding 20 mL of dimethylformamide to the Na2S·9H2O aqueous solution to form a ligand exchange solution;

[0146] 0.2 g of hydrophobic nano-chalcopyrite was dispersed in 15 mL of cyclohexane, a ligand exchange solution was added and stirred, centrifuged at 8000 rpm for 5 min, washed with ethanol, dried at 60° C. for 10 h, and then ground to obtain hydrophilic nano-chalcopyrite;

[0147] S1. Ultrasonic dispersion of 150 mg of dopamine hydrochloride and 100 mg of hydrophilic nano-chalcopyrite into 100 mL of Tris-HCL (tris(hydroxymethyl)aminomethane hydrochloride)) solution, mixing and magnetically stirring at 40° C. for 8 h to form a first mixture;

[0148] S2. Centrifuge the first mixture at 8000 rpm for 5 min, wash and dry at 70° C. for 18 h, and then grind to obtain polydopamine-modified nano-chalcopyrite material (CuFeS 2 / PDA).

[0149] Comparative Example 1

[0150] The comparative example of the present invention provides a nano chalcopyrite material, and the preparation method comprises the following steps:

[0151] S10, dissolving 0.25 g of Na2S·9H2O in 5 mL of ultrapure water to obtain a Na2S·9H2O aqueous solution, and adding 25 mL of dimethylformamide to the Na2S·9H2O aqueous solution to form a ligand exchange solution;

[0152] S11, 4 mmol of CuI, 4 mmol of FeCl3 and 480 mmol of oleylamine were mixed and stirred to obtain a second mixture;

[0153] S12, heating the second mixture under vacuum to a temperature of 120° C., and continuously stirring for 2 h to react;

[0154] S13, heating the second mixture to 180° C. under a nitrogen atmosphere, and stirring at a rotation speed of 160 rpm for 40 min to react;

[0155] S14, dissolving elemental sulfur in a 1-octadecene solution at a temperature of 60° C. to obtain a 0.7 mmol / mL elemental sulfur 1-octadecene solution;

[0156] The second mixture was stirred at a constant temperature at a rotation speed of 150 rpm, and 15 mL of a 1-octadecene solution of elemental sulfur was quickly injected for mixing, and after maintaining for 20 minutes, the mixture was centrifuged at a rotation speed of 8000 rpm for 5 minutes to obtain a third mixture;

[0157] S15, after cooling to room temperature under room temperature environment, washing the third mixture precipitate twice with a mixture of ethanol and toluene in a volume ratio of 1:2, and vacuum drying at a temperature of 60° C. for 6 h to obtain hydrophobic nano chalcopyrite;

[0158] S16. Disperse 0.375 g of hydrophobic nano-chalcopyrite in 7.5 mL of cyclohexane, add ligand exchange solution and stir, centrifuge at 8000 rpm for 5 min, wash with ethanol, dry at 60° C. for 12 h, and then grind to obtain nano-chalcopyrite material.

[0159] Performance Testing

[0160] The polydopamine-modified nano-chalcopyrite materials of Examples 1-3 and the nano-chalcopyrite material of Comparative Example 1 were experimentally tested for their bactericidal properties.

[0161] Figure 4 The figure shows the killing effect of the polydopamine-modified nano-chalcopyrite material in Example 1 on cefotaxime-resistant Escherichia coli within 90 seconds. As can be seen from the figure, the photothermal catalyst has a highly efficient killing effect, achieving complete killing within 90 seconds. The experimental results show that the CuFeS2 / PDA composite photothermal catalyst prepared by the present invention is a new type of material with efficient sterilization and good photothermal performance. It can be used as a sterilization catalyst in the fields of medical wastewater treatment and has a wide range of application potentials.

[0162] Figure 1 This is an electron microscope image of the polydopamine-modified nano-chalcopyrite material of Example 2 of the present invention. Figure 2 This is an electron microscope image of the nano-chalcopyrite material of comparative example 1 of the present invention. It can be seen that in the polydopamine-modified nano-chalcopyrite material of the present invention, PDA is loaded on the nano-chalcopyrite material to form a nano-coat, and the thickness of PDA is 1.7 nm.

[0163] Figure 5The figure shows the killing effect of the polydopamine-modified nano-chalcopyrite material in Example 2 and the nano-chalcopyrite material in Comparative Example 1 on Staphylococcus aureus within 4 minutes. As can be seen from the figure, 7 log cfu / mL of Staphylococcus aureus was completely killed within 4 minutes, indicating that the polydopamine-modified nano-chalcopyrite material has a good killing effect in other bacterial liquid systems, while the bacterial concentration of the chalcopyrite material not modified by PDA is still around 5 log cfu / mL at 4 minutes;

[0164] Figure 6 The figure is a graph showing the killing effect of polydopamine-modified nano-chalcopyrite material on polymyxin B-resistant Escherichia coli within 10 minutes in Example 3. As can be seen from the figure, 8 log of polymyxin B-resistant Escherichia coli were completely killed within 10 minutes, indicating that the polydopamine-modified nano-chalcopyrite material has an inactivation effect on more than one type of resistant bacteria, reflecting the extensive sterilization of the material.

[0165] As described above, the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing polydopamine modified nano chalcopyrite material, It is characterized in that The following steps are involved: S1, dispersing dopamine hydrochloride and hydrophilic nano chalcopyrite into an alkaline solution, mixing and stirring to form a first mixture; S2. Centrifuging, washing and drying the first mixture to obtain a polydopamine-modified nano-chalcopyrite material.

2. The preparation method according to claim 1, It is characterized in that The hydrophilic nano-chalcopyrite is prepared from the hydrophobic nano-chalcopyrite by a water phase conversion method, and the hydrophobic nano-chalcopyrite is prepared by a hot injection method.

3. The preparation method according to claim 2, It is characterized in that The hydrophobic nano chalcopyrite is prepared by a hot injection method, which specifically includes the following steps: S11, mixing and stirring the cuprous compound, the ferric compound and oleylamine to obtain a second mixture; S12, heating the second mixture under vacuum until the temperature reaches a first preset threshold range, and continuing stirring until the time reaches a second preset threshold range; S13, heating the second mixture under a nitrogen atmosphere until the temperature reaches a third preset threshold range, and continuing stirring until the time reaches a fourth preset threshold range; S14, stirring the second mixture at a constant temperature, injecting a 1-octadecene solution of elemental sulfur to mix, and centrifuging to obtain a third mixture; S15, after cooling to room temperature under room temperature environment, washing the third mixture, and drying to obtain hydrophobic nano chalcopyrite.

4. The preparation method according to claim 3, It is characterized in that The cuprous compound is one or more of CuI and cuprous acetate; The ferric iron compound is FeCl 3 、Fe(acac) 3 One or more of .

5. The preparation method according to claim 2, It is characterized in that The hydrophilic nano-chalcopyrite is prepared from the hydrophobic nano-chalcopyrite by a water phase conversion method, which specifically includes the following steps: S16, dispersing the hydrophobic nano-chalcopyrite in a dispersant, adding a ligand exchange solution, stirring, centrifuging, washing and drying to obtain the hydrophilic nano-chalcopyrite; The preparation method of the ligand exchange solution comprises the following steps: Will Na 2 S.9H 2 O dissolves in water to give Na 2 S.9H 2 O aqueous solution, in the Na 2 S.9H 2 O aqueous solution to form the ligand exchange solution.

6. The preparation method according to claim 1, It is characterized in that In S1, the molar ratio of the dopamine hydrochloride to the hydrophilic nano-chalcopyrite is 1 to 2:1; The stirring time is 6 to 12 hours, and the stirring temperature is 30 to 50° C.; In S2, the centrifugal speed is 5000-8000 rpm, and the centrifugal time is 2-5 min; the drying temperature is 60-80° C., and the drying time is 12-24 h.

7. The preparation method according to claim 3, It is characterized in that In the S11, the CuI, FeCl 3 The molar ratio with oleylamine is 1:1:90-120; In the S12, the first preset threshold range is 100-120°C, and the second preset threshold range is 1.5-2h; In the S13, the third preset threshold range is 150-180°C, and the fourth preset threshold range is 20-40min; In the S14, the method for preparing the 1-octadecene solution of elemental sulfur comprises the following steps: dissolving elemental sulfur in a 1-octadecene solution at a temperature of 50 to 60° C. to obtain the 1-octadecene solution of elemental sulfur; The concentration of the 1-octadecene solution of elemental sulfur is 0.5-0.7 mmol / m, and the elemental sulfur is mixed with CuI, FeCl 3 The molar ratio is 2:1:1; the elemental sulfur is one or more of sulfur powder, dodecanethiol and hexamethyldisilathione; The stirring speed is 150-160 rpm, and the stirring time is 10-20 min; In the S15, the washing is performed by washing with a mixture of ethanol and toluene; the volume ratio of the ethanol to the toluene is 1 to 2:1; The drying temperature is 50-60° C., and the drying time is 6-12 hours.

8. The preparation method according to claim 5, It is characterized in that In S16, the dispersant is one or more of cyclohexane and hexane; the concentration of the dispersant is 0.02 to 0.05 g / mL; The centrifugal speed is 5000-8000 rpm, and the centrifugal time is 2-5 min; The cleaning is carried out by using ethanol; The drying temperature is 50-60°C and the drying time is 6-12h; The Na 2 S.9H 2 The concentration of O aqueous solution is 0.02-0.05 g / mL; The Na 2 S.9H 2 The volume ratio of the O aqueous solution to the dimethylformamide is 1:3-5; The hydrophobic nano chalcopyrite and the Na 2 S.9H 2 The mass ratio of O aqueous solution is 1.5 to 2:

1.

9. A polydopamine modified nano chalcopyrite material, It is characterized in that It is prepared based on the preparation method according to any one of claims 1 to 8.

10. Use of the polydopamine modified nano-chalcopyrite material according to claim 9 to kill bacteria under visible light aqueous system.

Citation Information

Patent Citations

  • Polydopamine modified transition metal chalcogenide nano-sheet and preparation method thereof

    CN108408780A

  • Preparation method and application of polydopamine-modified magnetic nanoparticle

    CN110142035A

  • Copper nanoparticle-loaded polydopamine-modified flaky MoS2 nano antibacterial agent as well as preparation method and application of copper nanoparticle-loaded polydopamine-modified flaky MoS2 nano antibacterial agent

    CN114009447A

  • Manufacturing method for chalcopyrite nanoparticles

    WO2015008858A1