Binding method for pure tungsten and tungsten alloy target material and copper back plate
The intermediate layer after electroless nickel plating is improved by vacuum hot press diffusion welding technology, and the welding strength and welding rate of pure tungsten and tungsten alloy targets and copper backplate are solved, and the low welding rate and welding rate in the existing process are solved. High cost problem, efficient component processing is achieved.
Patent Information
- Application Number
- CN202411106444.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-22
AI Technical Summary
The binding process of the existing pure tungsten and tungsten alloy targets and copper back plates has problems such as low welding rate, poor welding strength, complex process flow and high cost, which cannot meet the needs of high-performance components.
The intermediate layer after fine grinding and ultrasonic cleaning is used for electroless nickel plating. Combined with vacuum hot press diffusion welding technology, a nickel plating film intermediate layer is formed, and vacuum hot press diffusion welding is carried out in a hot press sintering furnace to reduce the temperature and increase the nickel Element diffusion rate.
The bonding strength and welding rate of pure tungsten and tungsten alloy targets and copper backplate are improved, and the impact of solder on purity and the operational complexity and cost of thermal isostatic diffusion welding is avoided, thus achieving more efficient component processing.
Smart Images

Figure CN118989547A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for binding a pure tungsten or tungsten alloy target material to a copper back plate, and belongs to the technical field of preparation of metal target materials. Background Art
[0002] In the semiconductor industry, target products are composed of target materials and backing plates. The backing plates play a supporting role when the target assembly is assembled to the sputtering base and have the function of conducting heat. For pure tungsten or tungsten-based alloy targets, copper alloy materials with sufficient strength, high thermal conductivity and electrical conductivity are usually selected as the backing plates.
[0003] At present, pure tungsten or tungsten-based alloy target and copper alloy back plate are mainly welded by solder and diffusion welding, and a pure tungsten or tungsten-based alloy target assembly is formed after the welding solidifies. For example, CN111014930A discloses a two-step hot isostatic pressing diffusion welding method for a tungsten target assembly, wherein the welding method adopts hot isostatic pressing diffusion welding to successfully connect the tungsten target, the Al intermediate layer and the copper back plate, and finally obtain a tungsten target assembly. The hot isostatic pressing diffusion welding method can ensure that the tungsten target assembly will not desolder or drop the target during the sputtering process, and has high welding strength and good welding quality; and CN112846171A discloses a powder intermediate layer and a method for hot isostatic pressing diffusion welding of tungsten targets using the powder intermediate layer, wherein the powder intermediate layer is changed from a traditional single-type metal powder to a composite type powder, and the intermediate layer powder is composed of pure Ti, Al and Cu powders, and the purpose is to improve the welding strength and welding rate between the target and the back plate, and finally obtain a welding strength higher than 150MPa and a welding rate>99.7%. CN106378507A discloses a welding method for a tungsten-titanium target assembly, which utilizes multiple solder coatings and surfactant treatments, and can improve the welding strength and bonding rate of the tungsten-titanium target assembly compared to traditional solder welding.
[0004] However, at present, the binding process of pure tungsten and tungsten alloy targets and copper backing plates is mainly through solder welding and hot isostatic pressing, which has problems such as low welding rate, poor welding strength, complex process flow and high cost. Therefore, it cannot meet the needs of high-performance pure tungsten and tungsten alloy target components. Summary of the invention
[0005] In order to solve the problems existing in the existing process of binding pure tungsten and tungsten alloy targets with copper backing plates, the present invention provides a method for binding pure tungsten and tungsten alloy targets with copper backing plates, and the method specifically comprises the following steps:
[0006] (1) The welding middle layer is finely polished and ultrasonically cleaned, and then the middle layer is plated with nickel film by a chemical nickel plating method to obtain a nickel-plated middle layer.
[0007] (2) The pure tungsten or tungsten alloy target and the copper backing plate are finely ultrasonically cleaned and vacuum dried.
[0008] (3) placing the pure tungsten or tungsten alloy target, the nickel-plated film intermediate layer and the copper back plate into a hot pressing sintering furnace for vacuum hot pressing diffusion welding, and finally obtaining a pure tungsten and tungsten alloy target assembly.
[0009] Preferably, the intermediate layer in step (1) is titanium foil, aluminum foil or nickel foil.
[0010] Preferably, the purity of the titanium foil, aluminum foil and nickel foil is 99.9% and the thickness is 1-4 μm.
[0011] Preferably, the composition and content of the nickel plating solution used in the chemical nickel plating method in step (1) are: 10g / L~40g / L nickel chloride, 10g / L~40g / L nickel sulfate, and 5~20g / L citric acid; the chemical nickel plating is carried out in a water bath at 50~80°C.
[0012] Preferably, the reducing agent used in the chemical electroplating method in step (1) is one or more of hydrazine hydrate, formaldehyde, potassium sodium tartrate, glyoxal, sodium borohydride, acetal or tannic acid mixed in any proportion.
[0013] Preferably, the vacuum drying conditions in step (2) are 80-100° C. and the time is 2-5 h.
[0014] Preferably, the vacuum hot pressing diffusion welding parameters in step (3) are: diffusion welding temperature of 400°C to 700°C, holding time of 3h to 6h, welding pressure of 20 to 50MPa, vacuum degree of <10 -3 Pa, heating rate 10℃ / min.
[0015] Beneficial Effects of the Invention
[0016] (1) The present invention reduces the temperature of vacuum hot pressing diffusion welding by chemically plating nickel on the intermediate metal layer, thereby increasing the diffusion rate of nickel in pure tungsten and tungsten alloy targets and copper backing plates, thereby increasing the bonding strength and welding rate of vacuum hot pressing diffusion welding.
[0017] (2) The present invention achieves welding of pure tungsten and tungsten alloy target materials and copper backing plates by diffusion of nickel plating during vacuum hot pressing diffusion welding without using a sheath and solder, thereby avoiding the influence of solder on the purity of pure tungsten and tungsten alloy target materials prepared by powder metallurgy. At the same time, it also avoids the problems of excessive deformation and processing difficulty of subsequent pure tungsten and tungsten alloy target materials and copper backing plates caused by sheath leakage and operation complexity during hot isostatic pressing diffusion welding, thereby achieving the purpose of reducing the diffusion welding cost and processing difficulty of the target material and copper backing plate. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 The present invention is a process flow chart of the method for binding the pure tungsten and tungsten alloy target material to the copper back plate. DETAILED DESCRIPTION
[0019] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. However, the following embodiments are merely simple examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0020] Example 1
[0021] A method for bonding a pure tungsten target material to a copper backing plate, the process flow is as follows Figure 1 As shown, the specific steps include:
[0022] (1) Finely polished and ultrasonically cleaned aluminum foil (thickness 2 μm) was added to a nickel plating solution prepared by 10 g / L nickel chloride, 10 g / L nickel sulfate, and 5 g / L citric acid, and then an excess amount of reducing agent potassium sodium tartrate was added to react. The reaction was carried out in a 60° C. water bath. After the reaction was completed, it was repeatedly washed with deionized water until neutral, to obtain a nickel-plated intermediate layer aluminum foil layer.
[0023] (2) The pure tungsten target and the copper back plate are finely ultrasonically cleaned and vacuum dried at 80°C for 3 hours.
[0024] (3) The pure tungsten target, nickel-plated film intermediate layer and copper back plate are placed in a hot pressing sintering furnace for vacuum hot pressing diffusion welding. The welding temperature range is 500°C, the holding time is 3h, the welding pressure is 30MPa, and the vacuum degree is <10 -3 Pa, heating rate 10℃ / min, after welding, pure tungsten and tungsten alloy target components are finally obtained. The properties of the target are shown in Table 1.
[0025] Example 2
[0026] A method for binding a tungsten-titanium alloy target material to a copper back plate, the process flow is as follows Figure 1 As shown, the specific steps include:
[0027] (1) A titanium foil (3 μm thick) after fine grinding and ultrasonic cleaning was added to a nickel plating solution prepared by 20 g / L nickel chloride, 20 g / L nickel sulfate, and 10 g / L citric acid, and then an excess of potassium sodium tartrate, a reducing agent, was added to react in a 70° C. water bath. After the reaction was completed, it was repeatedly washed with deionized water until it was neutral, thereby obtaining a nickel-plated intermediate layer aluminum foil layer.
[0028] (2) The tungsten-titanium alloy target and the copper back plate are finely ultrasonically cleaned and vacuum dried at 90°C for 5 hours.
[0029] (3) The tungsten-titanium alloy target, the nickel-plated film intermediate layer and the copper back plate are placed in a hot pressing sintering furnace for vacuum hot pressing diffusion welding. The welding temperature range is 600°C, the holding time is 3h, the welding pressure is 40MPa, and the vacuum degree is <10 -3 Pa, heating rate 10℃ / min, after welding, pure tungsten and tungsten alloy target components are finally obtained. The properties of the target are shown in Table 1.
[0030] Example 3
[0031] A method for binding a tungsten-copper alloy target material to a copper backing plate, the process flow is as follows Figure 1 As shown, the specific steps include:
[0032] (1) Finely polished and ultrasonically cleaned nickel foil (thickness 4 μm) was added to a nickel plating solution prepared by 40 g / L nickel chloride, 40 g / L nickel sulfate, and 20 g / L citric acid, and then an excess amount of reducing agent potassium sodium tartrate was added to react. The reaction was carried out in a water bath at 80° C. After the reaction was completed, it was repeatedly washed with deionized water until it was neutral, thereby obtaining a nickel-plated intermediate layer aluminum foil layer.
[0033] (2) The tungsten-copper alloy target and the copper back plate are finely ultrasonically cleaned and vacuum dried at 100°C for 3 hours.
[0034] (3) The tungsten-copper alloy target, the nickel-plated film intermediate layer and the copper back plate are placed in a hot pressing sintering furnace for vacuum hot pressing diffusion welding. The welding temperature range is 600°C, the holding time is 5h, the welding pressure is 30MPa, and the vacuum degree is <10 -3 Pa, heating rate 10℃ / min, after welding, pure tungsten and tungsten alloy target components are finally obtained. The properties of the target are shown in Table 1.
[0035] Example 4
[0036] A method for binding a tungsten-silicon alloy target material to a copper back plate, the process flow is as follows Figure 1 As shown, the specific steps include:
[0037] (1) Finely polished and ultrasonically cleaned aluminum foil (thickness 4 μm) was added to a nickel plating solution prepared by 20 g / L nickel chloride, 20 g / L nickel sulfate, and 10 g / L citric acid, and then an excess amount of reducing agent potassium sodium tartrate was added to react. The reaction was carried out in a water bath at 80° C. After the reaction was completed, it was repeatedly washed with deionized water until it was neutral, thereby obtaining a nickel-plated intermediate layer aluminum foil layer.
[0038] (2) The tungsten silicon alloy target and the copper back plate are finely ultrasonically cleaned and vacuum dried at 80°C for 4 hours.
[0039] (3) Place the tungsten silicon alloy target, nickel-plated film intermediate layer and copper back plate into a hot pressing sintering furnace for vacuum hot pressing diffusion welding. The welding temperature range is 600°C, the holding time is 5h, the welding pressure is 50MPa, and the vacuum degree is <10 -3 Pa, heating rate 10℃ / min, after welding, pure tungsten and tungsten alloy target components are finally obtained. The properties of the target are shown in Table 1.
[0040] Comparative Example 1
[0041] The difference between Comparative Example 1 and Example 1 is that no intermediate layer is used, and the pure tungsten target and the copper back plate are directly subjected to vacuum hot pressing diffusion welding. The other preparation processes are the same as those of Example 1.
[0042] By comparing the welding strength and welding rate of the pure tungsten target assembly of Example 1 and Comparative Example 1, it is found from the relevant data in Table 1 that the presence of the nickel-plated aluminum foil layer can improve the welding strength and welding rate of the pure tungsten alloy target assembly. This is because compared with other welding processes, the nickel grain size of the nickel-plated layer is finer and the defect density is higher, which is conducive to the diffusion of nickel elements into the pure tungsten target and the copper backing plate under high temperature and high pressure conditions, thereby achieving an improvement in the welding strength and welding rate between the pure tungsten target and the copper backing plate.
[0043] Comparative Example 2
[0044] For comparison, the difference between Comparative Example 2 and Example 1 is that chemical nickel plating is not performed on the intermediate layer aluminum foil, and the remaining steps are the same as those of Example 1.
[0045] By comparing the welding strength and welding rate of the pure tungsten target assembly of Example 1 and Comparative Example 2, it is found from the relevant data in Table 1 that the presence of the nickel plating layer can improve the welding strength and welding rate of the tungsten-titanium alloy target assembly. This is because the surface of the aluminum foil has not been nickel-plated, and the mechanical welding of the pure tungsten target and the copper backing plate is performed by thermoplastic deformation of the aluminum element itself, resulting in that its welding strength and welding rate are not as good as the combined welding effect of nickel diffusion welding and thermoplastic deformation.
[0046] Table 1 Comparison of welding process and performance of Example 1 to Example 4 and Comparative Example 1 to Comparative Example 2
[0047] Welding strength (MPa) Welding rate (%) Example 1 167 99.1 Example 2 1 58 98.7 Example 3 181 98.8 Example 4 165 99.2 Comparative Example 1 98 85.7 Comparative Example 2 104 88.3
[0048] The above-mentioned embodiments are only several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the scope of disclosure and protection of the present invention.
Claims
1. A method for binding a pure tungsten or tungsten alloy target to a copper back plate, characterized in that: The method specifically comprises the following steps: (1) finely grinding and ultrasonically cleaning the welding middle layer, and then plating the middle layer with nickel by a chemical nickel plating method to obtain a nickel-plated middle layer; (2) fine ultrasonic cleaning and vacuum drying of the pure tungsten or tungsten alloy target and the copper backing plate; (3) placing the pure tungsten or tungsten alloy target, the nickel-plated film intermediate layer and the copper back plate into a hot pressing sintering furnace for vacuum hot pressing diffusion welding, and finally obtaining a pure tungsten or tungsten alloy target assembly.
2. The method for binding the pure tungsten and tungsten alloy target material to the copper back plate according to claim 1, characterized in that: The tungsten target material is pure tungsten or tungsten alloy.
3. The method for binding pure tungsten and tungsten alloy target materials to a copper back plate according to claim 1, characterized in that: The intermediate layer in step (1) is titanium foil, aluminum foil or nickel foil.
4. The method for binding pure tungsten and tungsten alloy targets to a copper back plate according to claim 3, characterized in that: The purity of the titanium foil, aluminum foil and nickel foil is 99.9% and the thickness is 1-4 μm.
5. The method for binding pure tungsten and tungsten alloy target materials to a copper back plate according to claim 1, characterized in that: The composition and content of the nickel plating solution used in the chemical nickel plating method in step (1) are: 10g / L-40g / L nickel chloride, 10g / L-40g / L nickel sulfate, and 5-20g / L citric acid; the chemical nickel plating is carried out in a water bath at 50-80°C.
6. The method for binding pure tungsten and tungsten alloy target materials to a copper back plate according to claim 1, characterized in that: The reducing agent used in the chemical electroplating method of step (1) is one or more of hydrazine hydrate, formaldehyde, potassium sodium tartrate, glyoxal, sodium borohydride, acetal or tannic acid mixed in any proportion.
7. The method for binding pure tungsten and tungsten alloy targets to a copper back plate according to claim 1, characterized in that: The vacuum drying conditions described in step (2) are 80-100° C. and the time is 2-5 hours.
8. The method for binding pure tungsten and tungsten alloy targets to a copper back plate according to claim 1, characterized in that: The vacuum hot pressing diffusion welding parameters in step (3) are: the diffusion welding temperature is 400° C. to 700° C., and the insulation time is 3 h to 6 h.
9. The method for binding pure tungsten and tungsten alloy target materials to a copper back plate according to claim 1, characterized in that: The vacuum hot pressing diffusion welding parameters in step (3) are: welding pressure is 20-50MPa, vacuum degree is less than 10 -3 Pa, heating rate 10℃ / min.
Citation Information
Patent Citations
Heterogeneous metal connecting method for tungsten, copper and alloy thereof
CN101704160A
Manufacture method of target structure
CN102586743A
Tungsten target diffusion welding method and target assembly
CN107971620A
Vacuum brazing method for tungsten target material
CN115319219A
Tantalum or tungsten target-copper alloy backing plate assembly and production method therefor
US20030134143A1