Glass fiber reinforced plastic waste recycling method and plate manufactured through glass fiber reinforced plastic waste recycling method
By crushing and mixing the resin-containing glass fiber of fiberglass waste with resin, and adopting molding and other molding processes, the problems of high energy consumption and complex process in the existing technology are solved, and efficient recycling of fiberglass waste and high-strength boards are realized. production.
Patent Information
- Application Number
- CN202411031121.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art is difficult to effectively recycle and utilize the resin blocks and flashes generated in the production process of fiberglass. The high-temperature melting process consumes energy and is complex, so it cannot effectively solve the recycling problem of fiberglass scrap.
By crushing and mixing the resin-containing glass fiber part in the fiberglass waste, the sheet is made by molding, vacuum or hand-paste molding, avoiding the use of high-temperature curing resin, and realizing pure physical recycling.
It realizes efficient recycling and reuse of fiberglass scrap, reduces process complexity and energy consumption, produces high-strength boards, and can adjust the performance of the boards according to the resin addition ratio and molding method.
Smart Images

Figure CN118990862A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of recycling glass fiber composite materials, and relates to a method for recycling glass fiber reinforced plastic waste and a manufacturing plate. Background Art
[0002] During the production of FRP, a large amount of waste is generated, which can be divided into:
[0003] (1) Leftovers from cutting of raw materials, such as glass fiber waste and guide nets;
[0004] (2) The resin-containing guide net and bag film produced by product demoulding;
[0005] (3) Leftovers from the product cutting process, such as flash and resin blocks;
[0006] (4) Grinding dust during product assembly;
[0007] (5) scrapped products;
[0008] Among them, waste 1, due to the improvement of the industrialization level of FRP, very little waste is generated in the current production process;
[0009] Waste 2 can be recycled using methods that have already been industrialized in the plastics industry;
[0010] Waste 3, there is currently no mature recycling method, and the industry pays for it to be treated as solid waste;
[0011] Waste 4, the grinding dust will float randomly and mix with the dust on the ground, making it difficult to recycle. In addition, due to the maturity of the process, the amount of grinding is very small;
[0012] Waste 5: The probability of defective products in the production of mature products is very low and almost non-existent, with only some products used for testing and products that fail on site.
[0013] Therefore, the bulk of the waste is waste 2, but waste 2 already has a mature industrial chain, and it is necessary to recycle the second largest waste 3. The current mainstream recycling methods include chemical method, physical method, combustion method, etc.
[0014] The prior art selects blade iron powder, acrylonitrile-butadiene-styrene copolymer (ABS) resin, polyethylene, and calcium powder, crushes them in a certain proportion, heats and melts them to make manhole covers, but it is necessary to use iron powder, ABS resin, polyethylene, and calcium powder, heat and melt them for recycling, mainly for waste 5, and mainly uses high-temperature melting to combine the waste.
[0015] The existing technology shreds the guide net as filler, cuts the fiberglass scraps into long strips as reinforcement, cuts the fiberglass cloth into pieces as coupling agent, crushes the cured resin as filler, uses grinding dust as thickener, and divides the injection hose into sections as reinforcement. The mixture is mixed in a certain proportion, and the reinforcement material is arranged in a certain way and molded. Although all the waste materials are used, they need to be recycled into products in a certain combination, and each component needs to be processed. The production process needs to be stopped frequently to evenly place the fiberglass scrap reinforcement, and the process is cumbersome.
[0016] The existing technology uses high-temperature resin, glass fiber waste, waste particles of orthophthalic unsaturated polyester casting materials and / or grinding dust as the main materials, adds resin additives as auxiliary materials, mixes and puts into a mold for heating and molding, but uses resin waste particles and glass fiber waste in combination with high-temperature resin to make product recycling, mainly for waste 1 and waste 4.
[0017] The existing technology mixes waste wind turbine blade materials within a preset size range with thermoplastic materials to 150-200°C to obtain molding materials, but waste blade materials with fixed size sheets of 5-50mm are used in combination with thermoplastic resin recycling, mainly using high-temperature melting to combine waste materials.
[0018] The prior art heats the thermoplastic resin to above the softening temperature, adds zinc stearate and graphene, mixes and performs the first extrusion molding process to obtain a raw material plate, spreads recycled fiberglass fiber waste on one side, and then takes another raw material plate to cover it. After multiple extrusion molding and curing processes, the air duct is obtained. However, this patent uses thermoplastic resin, which needs to be heated to the softening temperature before mixing, and needs to be kept heated during the period, which requires a large amount of energy consumption; this patent only uses glass fiber waste, which is a recycling of raw materials, and various flash, resin blocks, and scrapped products generated after the blade is formed cannot be recycled. Summary of the invention
[0019] The purpose of the present invention is to provide a method for recycling and reusing FRP waste and making plates in order to overcome at least one defect of the above-mentioned prior art. The present invention facilitates the recycling of the resin-containing glass fiber portion of FRP waste.
[0020] The purpose of the present invention can be achieved by the following technical solutions:
[0021] One of the technical solutions of the present invention is to provide a method for recycling glass fiber reinforced plastic waste, the method comprising the following steps:
[0022] S1. Waste pretreatment,
[0023] Crushing the resin-containing glass fiber portion of the FRP waste to obtain scraps;
[0024] S2, mixed resin,
[0025] The chips and the resin are mixed evenly to obtain a mixture;
[0026] S3, filler,
[0027] pouring the mixture into a mold, laying out the mixture, compression molding, vacuum forming, hand lay-up, or extrusion molding to make a sheet;
[0028] S4, demoulding,
[0029] The product is separated from the mold to obtain a sheet.
[0030] Furthermore, in step S1, the part containing resin glass fiber in the FRP waste is selected from one or more of flash, scrapped products, cutting scraps, resin blocks, and structural rubber blocks, the mass content of the resin glass fiber is 30-100%, and the maximum particle size of the debris is 1-20 mm.
[0031] As a preferred technical solution, in step S1, the resin glass fiber-containing portion of the FRP waste is cut into a size smaller than that of the shredder, and then fed into the shredder to be torn into pieces, and then the torn pieces are fed into a pulverizer to obtain debris.
[0032] Furthermore, in step S2, the resin is selected from one or more of unsaturated polyester resin, vinyl ester resin, diallyl phthalate resin, phenolic resin, and bisphenol A epoxy resin;
[0033] The mass ratio of chips to resin is (1-4):1;
[0034] The temperature of mixing the chips and the resin is room temperature and the time is 5-10 minutes.
[0035] Further, after the resin and the curing agent are evenly mixed in step S2, the chips and the resin are evenly mixed, and if the resin does not need to be cured, the curing agent does not need to be added;
[0036] In step S4, the product is separated from the mold and then left to solidify.
[0037] Furthermore, the curing agent is selected from one or more of methyl ethyl ketone peroxide, catechol, aliphatic diamines, and aliphatic polyamines, and some high temperature curing resins do not need to add a curing agent;
[0038] The amount of curing agent added is 0.5-3% of the resin mass, which mainly affects the curing time;
[0039] The temperature of mixing the resin and the curing agent is room temperature or the curing temperature of the resin. Some resins need to be heated and cured to reach the curing temperature for 5-10 minutes.
[0040] The temperature of the static curing is room temperature, and the time is 30-90 minutes.
[0041] Furthermore, when compression molding is adopted in step S3, the mixture is first pre-compacted at 0.05-1MPa and room temperature for 5-10 minutes, and then compression molded at 1-20MPa and room temperature or resin curing temperature for 30-90 minutes until the mixture is formed. Some resins need to be heated and cured to reach the curing temperature.
[0042] Furthermore, when vacuum forming is adopted in step S3, vacuum pressure of 0.6-2MPa and room temperature or resin curing temperature are maintained for 30-120min until forming, and some resins need to be heated and cured to reach the curing temperature.
[0043] Furthermore, a surface layer is laid on the surface of the mixture before forming in step S3 or after forming in step S4.
[0044] Furthermore, the surface layer is selected from one or more of cloth and felt, the material of the surface layer is glass fiber, the cloth is selected from one or more of uniaxial cloth, biaxial cloth, and multi-axial cloth, and the felt is selected from one or more of chopped strand mat and continuous mat.
[0045] One of the technical solutions of the present invention is to provide a plate made by recycling waste FRP materials, and the plate is made by adopting the method for recycling waste FRP materials.
[0046] As a preferred technical solution, the damaged plate can be used as waste and remade into a new plate according to the above steps.
[0047] Compared with the prior art, the present invention has the following beneficial effects:
[0048] (1) The present invention directly uses the waste of glass fiber containing resin (including flash and resin blocks) of glass fiber reinforced plastics, and can be recycled purely physically without adding a curing agent;
[0049] (2) The prior art mainly utilizes high-temperature molten waste, which is too costly. The waste recycling process of the present invention only requires processing into scraps, which is simple in process and can be molded at room temperature without using high-temperature curing resin;
[0050] (3) After molding, the present invention can obtain a high-strength board, and the strength of the board can be adjusted according to the resin addition ratio, the size of the debris, the molding pressure, the surface layer strength and the molding method. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 Schematic diagram of the process of recycling and reusing glass fiber reinforced plastic waste in Examples 1 to 5 of the present invention. DETAILED DESCRIPTION
[0052] The present invention is described in detail below in conjunction with specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and a specific operation process, but the protection scope of the present invention is not limited to the following embodiments.
[0053] Unless otherwise specified, the equipment used in the following examples are all conventional equipment in the art; the reagents used are all commercially available products or prepared by conventional methods in the art unless otherwise specified. Anything not described in detail in the following examples can be achieved by conventional experimental means in the art.
[0054] Embodiments 1 to 5:
[0055] A method for recycling glass fiber reinforced plastic waste, such as Figure 1 As shown, the specific steps are as follows:
[0056] S1. Waste pretreatment,
[0057] First, the resin glass fiber-containing parts of the FRP waste are screened out, such as flash, scrapped products, and cutting scraps, cut into a size smaller than the shredder feed size, and then put into the shredder to tear into pieces, and then put the shredded pieces into the crusher to obtain scraps;
[0058] S2, mixed resin,
[0059] Weigh the resin, combine with the curing agent (if the resin is not cured by adding a curing agent, such as high temperature curing, then no curing agent is needed) and mix and stir evenly for 5 minutes at room temperature (if the heat-curing resin needs to be heated to the curing temperature). Generally, the amount of curing agent added is 2% of the resin mass, which mainly affects the curing time. The chips and resin are mixed and stirred evenly at room temperature for 5 minutes;
[0060] S3, filler,
[0061] Pour the mixture into the mold, lay a single layer of the mixture, pre-compact the mixture at 0.1 MPa and room temperature for 5 minutes, then press and compact the mixture at a given pressure and room temperature for 60 minutes until it is cured (if the resin is cured at high temperature, the mold needs to be heated while compacting);
[0062] S4, demoulding,
[0063] Remove the product from the mold and check the appearance. If a smooth surface is required, a layer of cloth or felt can be applied by hand. Let it stand and cure at room temperature for 60 minutes to obtain a 280×280×10mm board. If the board is damaged, it can be used as waste and remade according to the above steps.
[0064] In this embodiment, the mass content of resin-containing glass fiber in the FRP waste is 50±10%, the resin is TM-25 orthophthalic unsaturated polyester resin, the curing agent is Akzo V388 (methyl ethyl ketone peroxide), and the surface layer is biaxial cloth of glass fiber.
[0065] A plate made by recycling glass fiber reinforced plastic waste adopts the above-mentioned recycling method to make the plate.
[0066] The effects of different resin addition ratios, crumb sizes and molding pressures on the compressive strength in Examples 1 to 5 are shown in Table 1.
[0067] Table 1 Effect of different resin addition ratios, crumb size and molding pressure on compression strength in Examples 1 to 5
[0068]
[0069] As shown in Table 1, the lowest compression strength of the plates in Examples 1 to 5 is 5.6 MPa, which is relatively high. The compression strength is affected by the molding pressure, the size of the chips, and the resin addition ratio. The greater the molding pressure, the coarser the chips, the higher the resin content, and the greater the compression strength.
[0070] Examples 6 to 17:
[0071] A method for recycling glass fiber reinforced plastic waste, the specific steps are as follows:
[0072] S1. Waste pretreatment,
[0073] First, the resin glass fiber-containing parts of the FRP waste are screened out, such as flash, scrapped products, and cutting scraps, cut into a size smaller than the shredder feed size, and then put into the shredder to tear into pieces, and then put the shredded pieces into the crusher to obtain scraps;
[0074] S2, mixed resin,
[0075] The resin was weighed, and the chips and the resin were mixed and stirred evenly at room temperature for 5 minutes to obtain a mixture;
[0076] S3, filler,
[0077] Pour the mixture into a mold, lay multiple layers of the mixture, and lay one or more surface layers of cloth or felt between the multiple layers of the mixture for spacing. The board can be made by combining compression molding, vacuum molding, hand lay-up molding, extrusion molding, etc. (the strength of the board is limited by the strength of the resin, and different resins will produce different strengths);
[0078] S4, demoulding,
[0079] The product is separated from the mold to obtain a single-layer mixture of 500×500×6 mm and a board with surface layers laid on both sides. After the board is damaged, it can be used as waste and remade into a board according to the above steps.
[0080] In this embodiment, the mass content of resin-containing glass fiber in the FRP waste is 50±10%, the mass of the debris is 1.8kg, the resin is TM-25 orthophthalic unsaturated polyester resin, the mass of the resin is 0.6kg, the mass ratio of debris to resin is 3:1, the vacuum forming conditions are 1MPa negative pressure, room temperature vacuum pressure maintenance for 90min until forming, and the material of the surface layer is glass fiber.
[0081] A plate made by recycling glass fiber reinforced plastic waste adopts the above-mentioned recycling method to make the plate.
[0082] The effects of different crumb sizes, surface layer strengths and molding methods on tensile strength and tensile modulus in Examples 6 to 11 are shown in Table 2.
[0083] Table 2 Effect of different chip sizes, surface layer strength and molding methods on tensile strength and tensile modulus in Examples 6 to 11
[0084]
[0085] The effects of different crumb sizes, surface layer strengths and molding methods on tensile strength and tensile modulus in Examples 12 to 17 are shown in Table 3.
[0086] Table 3 Effect of different crumb sizes, surface layer strength and molding methods on tensile strength and tensile modulus in Examples 12 to 17
[0087]
[0088] As shown in Table 2 and Table 3, the tensile strength of the plates in Examples 6 to 17 is as low as 36 MPa, and the tensile modulus is as low as 2.0 GPa, which are relatively high. The size of the debris, the surface layer strength and the forming method will affect the tensile strength. The finer the debris, the better the surface layer strength, the greater the tensile strength, and the tensile strength of the vacuum lay-up is slightly greater than that of the hand lay-up.
[0089] Examples 18 to 20:
[0090] A method for recycling glass fiber reinforced plastic waste, the specific steps are as follows:
[0091] S1. Waste pretreatment,
[0092] First, the resin glass fiber-containing parts of the FRP waste are screened out, such as flash, scrapped products, and cutting scraps, cut into a size smaller than the shredder feed size, and then put into the shredder to tear into pieces, and then put the shredded pieces into the crusher to obtain scraps;
[0093] S2, mixed resin,
[0094] The resin was weighed, and the chips and the resin were mixed and stirred evenly at room temperature for 5 minutes to obtain a mixture;
[0095] S3, filler,
[0096] Pour the mixture into the mold, lay a single layer of the mixture, pre-compact the mixture at 0.1MPa and room temperature for 5 minutes, and then mold-compact the mixture at 1MPa and 80℃ for 30 minutes until it is cured;
[0097] S4, demoulding,
[0098] The product is separated from the mold to obtain a 500×500×8mm plate. If the plate is damaged, it can be used as waste and remade according to the above steps.
[0099] In this embodiment, the mass content of resin-containing glass fiber in the FRP waste is 50±10%, the mass of the scraps is 1.8 kg, the resin is phenolic resin BR2130, the mass of the resin is 0.45 kg, and the mass ratio of the scraps to the resin is 4:1.
[0100] A plate made by recycling glass fiber reinforced plastic waste adopts the above-mentioned recycling method to make the plate.
[0101] The effects of different crumb sizes on tensile strength in Examples 18 to 20 are shown in Table 4.
[0102] Table 4 Effect of different chip sizes on tensile strength in Examples 18 to 20
[0103] Example 18 19 20 Maximum particle size of debris (mm) 6 12 20 Minimum tensile strength of sheet material (MPa) 9.8 7.3 3.1
[0104] As shown in Table 4, the tensile strength of the plates in Examples 18 to 20 is as low as 3.1 MPa, which is relatively high. The size of the chips will affect the tensile strength. The finer the chips, the greater the tensile strength.
[0105] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A method for recycling glass fiber reinforced plastic waste, characterized in that: The method comprises the following steps: S1. Waste pretreatment, Crushing the resin-containing glass fiber portion of the FRP waste to obtain scraps; S2, mixed resin, The chips and the resin are mixed evenly to obtain a mixture; S3, filler, pouring the mixture into a mold, laying out the mixture, compression molding, vacuum forming, hand lay-up, or extrusion molding to make a sheet; S4, demoulding, The product is separated from the mold to obtain a sheet.
2. A method for recycling glass fiber reinforced plastic waste according to claim 1, characterized in that: In step S1, the resin-containing glass fiber in the FRP waste is selected from one or more of flash, scrapped products, cutting scraps, resin blocks, and structural adhesive blocks, the mass content of the resin-containing glass fiber is 30-100%, and the maximum particle size of the debris is 1-20 mm.
3. The method for recycling glass fiber reinforced plastic waste according to claim 1, characterized in that: In step S2, the resin is selected from one or more of unsaturated polyester resin, vinyl ester resin, diallyl phthalate resin, phenolic resin, and bisphenol A epoxy resin; The mass ratio of chips to resin is (1-4):1; The temperature of mixing the chips and the resin is room temperature and the time is 5-10 minutes.
4. The method for recycling glass fiber reinforced plastic waste according to claim 1, characterized in that: After the resin and curing agent are evenly mixed in step S2, the chips and resin are evenly mixed; In step S4, the product is separated from the mold and then left to solidify.
5. A method for recycling glass fiber reinforced plastic waste according to claim 4, characterized in that: The curing agent is selected from one or more of methyl ethyl ketone peroxide, catechol, aliphatic diamines, and aliphatic polyamines; The amount of the curing agent added is 0.5-3% of the resin mass; The temperature of mixing the resin and the curing agent is room temperature or the resin curing temperature, and the time is 5-10 minutes; The temperature of the static curing is room temperature, and the time is 30-90 minutes.
6. The method for recycling glass fiber reinforced plastic waste according to claim 1, characterized in that: When compression molding is adopted in step S3, the mixture is pre-compacted at 0.05-1 MPa and room temperature for 5-10 minutes, and then compression molding is performed at 1-20 MPa and room temperature or the resin curing temperature for 30-90 minutes.
7. The method for recycling glass fiber reinforced plastic waste according to claim 1, characterized in that: When vacuum forming is adopted in step S3, the vacuum pressure is maintained at 0.6-2 MPa, room temperature or resin curing temperature for 30-120 minutes.
8. The method for recycling glass fiber reinforced plastic waste according to claim 1, characterized in that: Before forming in step S3 or after forming in step S4, a surface layer is laid on the surface of the mixture.
9. A method for recycling glass fiber reinforced plastic waste according to claim 8, characterized in that: The surface layer is selected from one or more of cloth and felt, the material of the surface layer is glass fiber, the cloth is selected from one or more of uniaxial cloth, biaxial cloth, and multiaxial cloth, and the felt is selected from one or more of chopped strand mat and continuous mat.
10. A method for recycling fiberglass waste to make plates, characterized in that: The plate is manufactured by using the method for recycling and reusing waste glass fiber reinforced plastics as described in any one of claims 1 to 9.
Citation Information
Cited By
Glass fiber composite material recycling device and method
CN121103814A