Production process of formaldehyde purification plate
By using formaldehyde decomposition gel prepared by using materials such as sodium phytate in the production of formaldehyde purified plates, the problems of complex production and poor formaldehyde absorption in the prior art are solved, and the effect of reducing production costs and improving safety is achieved.
Patent Information
- Application Number
- CN202411053153.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing formaldehyde purification board production process steps are complicated, resulting in high production costs and poor formaldehyde absorption effect of the formaldehyde decomposition solution on the substrate. Formaldehyde may still enter the indoor environment, endangering human health.
Formaldehyde is prepared by mixing sodium phytate, activated carbon, sodium p-aminobenzenesulfonate, titanium dioxide, methylside, ethylenediaminetetraacetic acid, ethyl acetate, dicyandiamide, carbohydrazide, sodium thiosulfate, glycerol and distilled water. Decompose the glue solution and apply it evenly on both sides of the substrate. Through pressing and drying treatment, ensure that the glue solution is fully fitted with the substrate and absorbs formaldehyde.
It simplifies the production process, reduces costs, and effectively absorbs formaldehyde released from the substrate, improves the safety of use, reduces the risk of formaldehyde entering the indoor environment, and protects human health.
Smart Images

Figure CN118991202A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of plate processing, in particular to a production process of a formaldehyde purification plate. Background Art
[0002] In recent years, with the improvement of people's living standards, people have higher and higher requirements for the environmental protection of interior decoration. The amount of board materials used in decoration and furniture making is very large, so the environmental performance of indoor boards largely determines the indoor air quality.
[0003] There are many standards for boards, and the environmental restrictions are mainly in terms of formaldehyde emission. Currently, the most recognized environmentally friendly board on the market is the formaldehyde-free board certified by the US NAF. From the formula to the production process, the formaldehyde emission is strictly controlled to ≤ 0.3mg / m. This type of board requires the formaldehyde emission to be as low as possible to reduce the release of formaldehyde into the environment.
[0004] The current formaldehyde purification board has complicated production steps, which increases the production cost. The formaldehyde decomposition glue has a poor effect on absorbing the formaldehyde released by the substrate. During the later use of the substrate, a large amount of formaldehyde still enters the indoor environment, which will invisibly endanger human health.
[0005] Therefore, a production process of formaldehyde purification plate is proposed to solve the above-mentioned problems. Summary of the invention
[0006] The purpose of the present invention is to provide a production process of a formaldehyde purification plate to solve the problems raised in the above background technology.
[0007] To achieve the above-mentioned purpose, the present invention provides the following technical solution: a production process of a formaldehyde purification plate, the specific steps of the production process of the formaldehyde purification plate are as follows:
[0008] Step 1: Select the substrate: Select the corresponding type of plate according to the later use needs, cut it, grind the cut edge after cutting, and grind and polish the upper and lower surfaces of the substrate plate;
[0009] Step 2: Preparation of formaldehyde decomposition glue: prepare 5-7 parts of sodium phytate, 2-3 parts of activated carbon, 2-5 parts of sodium p-aminobenzenesulfonate, 0.2-1 parts of titanium dioxide, 1-4 parts of methyl glycoside, 0.5-2 parts of ethylenediaminetetraacetic acid, 2-5 parts of ethyl acetate, 10-12 parts of dicyandiamide, 13-15 parts of carbohydrazide, 13-15 parts of sodium thiosulfate, 14-15 parts of glycerol, 50-100 parts of distilled water, and 20-30 parts of hydrochloric acid; select a 500 ml A container is prepared, and sodium phytate, activated carbon, sodium p-aminobenzenesulfonate, titanium dioxide, methyl glycoside, ethylenediaminetetraacetic acid, ethyl acetate, dicyandiamide, carbohydrazide, sodium thiosulfate, glycerol and distilled water are added to the container, and heated and stirred until they are completely dissolved with each other to form a transparent solution; then, hydrochloric acid solution is added dropwise, the pH value of the reaction system is controlled to be between 1 and 3, and the reaction temperature is maintained at about 80-90° C.; stirring is continued, and the reaction system gradually thickens to form a formaldehyde decomposition glue solution;
[0010] Step 3: Decorative film processing: the formaldehyde decomposition glue prepared in the previous step is evenly applied to both sides of the decorative film through a coating device, and the unevenly applied areas are processed to make the applied thickness uniform;
[0011] Step 4: Assemble: Lay the decorative film coated with formaldehyde decomposition glue on the two side walls of the substrate, and use a pressing device to squeeze the decorative film after laminating to ensure that the decorative film and the side walls of the substrate are completely in contact and squeeze out the bubbles between them, and then place them in a drying device, control the temperature of the drying device at 100-120 degrees Celsius, and continue drying for 10-20 minutes;
[0012] Step 5: Edge wrapping: Grind and trim the edges of the pressed sheets, and then wrap the edges after the processing is completed.
[0013] Preferably, the substrate includes activated carbon substrate, aniline substrate and glass fiber substrate.
[0014] Preferably, the thickness of the substrate is 20-25 mm, and the thickness of the formaldehyde decomposing glue applied is controlled to be 0.1-0.12 mm.
[0015] Preferably, after the formaldehyde decomposition glue is applied, the substrate needs to be immersed in the preservative liquid for 10-12 minutes. The preparation steps of the preservative liquid are as follows: 10-18 parts of ammonium acryloyldimethyltaurate / VP copolymer, 20-40 parts of sodium fluoride, 30-60 parts of ammonium bifluoride, 10-20 parts of potassium permanganate, and 40-50 parts of potassium chromate are selected as raw materials, mixed with each other and stirred for 5-10 minutes, 15-25 parts of zinc phosphate, 8-18 parts of sodium nitrate, 5-12 parts of praseodymium chloride, 10-16 parts of ethylenediaminetetraacetic acid, 7-14 parts of malic acid, 8-12 parts of sodium dodecylbenzene sulfate, 6-13 parts of nickel sulfate, and 15-25 parts of triethanolamine are added to the mixed solution, and stirred again for 1-4 minutes to obtain the formaldehyde decomposition glue.
[0016] Preferably, the edging is achieved by using a wooden edging strip and gluing it to the side wall of the base plate.
[0017] Preferably, in the step 2, after sodium phytate, activated carbon, sodium p-aminobenzenesulfonate, titanium dioxide, glycoside, ethylenediaminetetraacetic acid, ethyl acetate, dicyandiamide, carbohydrazide, sodium thiosulfate, glycerol and distilled water are mixed, the heating temperature needs to be controlled at 20-30 degrees Celsius.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] During the production and preparation of the board material, the present application evenly applies formaldehyde-decomposing glue on both sides of the substrate. The formaldehyde-decomposing glue is prepared by mixing sodium phytate, activated carbon, sodium p-aminobenzenesulfonate, titanium dioxide, glycoside, ethylenediaminetetraacetic acid, ethyl acetate, dicyandiamide, carbohydrazide, sodium thiosulfate, propylene glycol, distilled water and hydrochloric acid. It can effectively absorb the formaldehyde released by the substrate during use to avoid inhalation by residents, increase safety in later use, and ensure human health. The production process steps involved in the present application are simple, which reduces the processing cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The figure is a flow chart of the steps of the method of the present invention. DETAILED DESCRIPTION
[0021] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] In the description of the present invention, it is necessary to understand that the terms "upper", "lower", "front", "back", "left", "right", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0023] See also Figure 1 , the present invention provides a technical solution:
[0024] A production process of a formaldehyde purification plate, the specific steps of the production process of the formaldehyde purification plate are as follows:
[0025] Step 1: Select the substrate: Select the corresponding type of plate according to the later use needs, cut it, grind the cut edge after cutting, and grind and polish the upper and lower surfaces of the substrate plate;
[0026] Step 2: Preparation of formaldehyde decomposition glue: prepare 5-7 parts of sodium phytate, 2-3 parts of activated carbon, 2-5 parts of sodium p-aminobenzenesulfonate, 0.2-1 parts of titanium dioxide, 1-4 parts of methyl glycoside, 0.5-2 parts of ethylenediaminetetraacetic acid, 2-5 parts of ethyl acetate, 10-12 parts of dicyandiamide, 13-15 parts of carbohydrazide, 13-15 parts of sodium thiosulfate, 14-15 parts of glycerol, 50-100 parts of distilled water, and 20-30 parts of hydrochloric acid; select a 500 ml A container is prepared, and sodium phytate, activated carbon, sodium p-aminobenzenesulfonate, titanium dioxide, methyl glycoside, ethylenediaminetetraacetic acid, ethyl acetate, dicyandiamide, carbohydrazide, sodium thiosulfate, glycerol and distilled water are added to the container, and heated and stirred until they are completely dissolved with each other to form a transparent solution; then, hydrochloric acid solution is added dropwise, the pH value of the reaction system is controlled to be between 1 and 3, and the reaction temperature is maintained at about 80-90° C.; stirring is continued, and the reaction system gradually thickens to form a formaldehyde decomposition glue solution;
[0027] Step 3, decorative film processing: the formaldehyde decomposition glue prepared in the previous step is evenly applied to both sides of the decorative film through a coating device, and the unevenly applied areas are processed to make the applied thickness uniform. The thickness of the substrate is 20-25 mm, and the applied thickness of the formaldehyde decomposition glue is controlled to be 0.1-0.12 mm. After the substrate is coated with the formaldehyde decomposition glue, it needs to be placed in the preservative liquid and soaked for 10-12 minutes. The preparation steps of the preservative liquid are as follows: Select the raw material ammonium acryloyldimethyltaurate / VP 10-18 parts of copolymer, 20-40 parts of sodium fluoride, 30-60 parts of ammonium bifluoride, 10-20 parts of potassium permanganate, and 40-50 parts of potassium chromate are mixed and stirred for 5-10 minutes, and 15-25 parts of zinc phosphate, 8-18 parts of sodium nitrate, 5-12 parts of praseodymium chloride, 10-16 parts of ethylenediaminetetraacetic acid, 7-14 parts of malic acid, 8-12 parts of sodium dodecylbenzene sulfate, 6-13 parts of nickel sulfate, and 15-25 parts of triethanolamine are added to the mixed solution, and stirred again for 1-4 minutes to obtain a formaldehyde decomposition glue solution;
[0028] Step 4: Assemble: Lay the decorative film coated with formaldehyde decomposition glue on the two side walls of the substrate, and use a pressing device to squeeze the decorative film after laminating to ensure that the decorative film and the side walls of the substrate are completely in contact and squeeze out the bubbles between them, and then place them in a drying device, control the temperature of the drying device at 100-120 degrees Celsius, and continue drying for 10-20 minutes;
[0029] Step 5: Edge wrapping: Grind and trim the edges of the pressed sheets, and then wrap the edges after the processing is completed.
[0030] The types of substrates include activated carbon substrates, aniline substrates and glass fiber substrates. The activated carbon substrates are mainly composed of high-quality activated carbon powder and paraffin and other raw materials, have good adsorption properties, and can effectively remove harmful substances in the air, such as formaldehyde, benzene substances, odors, etc., to achieve the effect of purifying the air; the aniline substrate is a polymer material, which is polymerized from aniline, formaldehyde and other raw materials, has good physical and mechanical properties and chemical stability, can adsorb and decompose harmful substances in the air, and improve indoor air quality; the glass fiber substrate is composed of glass fiber and resin and other raw materials, has high physical strength and chemical stability, can effectively adsorb and decompose harmful substances in the air, and has good air purification function;
[0031] The edge binding is achieved by using a wooden edge binding strip and gluing it to the side wall of the base plate.
[0032] In the step 2, after sodium phytate, activated carbon, sodium p-aminobenzenesulfonate, titanium dioxide, glycoside, ethylenediaminetetraacetic acid, ethyl acetate, dicyandiamide, carbohydrazide, sodium thiosulfate, glycerol and distilled water are mixed, the heating temperature needs to be controlled at 20-30 degrees Celsius.
[0033] Embodiment 1:
[0034] The specific steps of the formaldehyde purification board production process are as follows:
[0035] Step 1: Select the substrate: Select the corresponding type of plate according to the later use needs, cut it, grind the cut edge after cutting, and grind and polish the upper and lower surfaces of the substrate plate;
[0036] Step 2, preparation of formaldehyde decomposition glue: prepare 5 parts of sodium phytate, 2 parts of activated carbon, 2 parts of sodium p-aminobenzenesulfonate, 0.2 parts of titanium dioxide, 1 part of methyl glycoside, 0.5 parts of ethylenediaminetetraacetic acid, 2 parts of ethyl acetate, 10 parts of dicyandiamide, 13 parts of carbohydrazide, 13 parts of sodium thiosulfate, 14 parts of glycerol, 50 parts of distilled water, and 20 parts of hydrochloric acid; select a 500 ml container, and add sodium phytate, activated carbon, sodium p-aminobenzenesulfonate, titanium dioxide, methyl glycoside, ethylenediaminetetraacetic acid, ethyl acetate, dicyandiamide, carbohydrazide, sodium thiosulfate, glycerol and distilled water to the container, heat and stir until they are completely dissolved to form a transparent solution; then, add hydrochloric acid solution dropwise, control the pH value of the reaction system between 1-3, and maintain the reaction temperature at about 80°C; continue stirring, the reaction system gradually thickens to form a formaldehyde decomposition glue;
[0037] Step 3: Decorative film processing: the formaldehyde decomposition glue prepared in the previous step is evenly applied to both sides of the decorative film through a coating device, and the unevenly applied areas are processed to make the applied thickness uniform;
[0038] Step 4: Assemble: Lay the decorative film coated with formaldehyde decomposition glue on the two side walls of the substrate, and use a pressing device to squeeze the decorative film after laminating to ensure that the decorative film and the side walls of the substrate are completely in contact and squeeze out the bubbles between them, and then place them in a drying device, control the temperature of the drying device at 100 degrees Celsius, and continue drying for 10 minutes;
[0039] Step 5: Edge wrapping: Grind and trim the edges of the laminated sheets, and then wrap the edges after the processing is completed;
[0040] Embodiment 2:
[0041] The specific steps of the formaldehyde purification board production process are as follows:
[0042] Step 1: Select the substrate: Select the corresponding type of plate according to the later use needs, cut it, grind the cut edge after cutting, and grind and polish the upper and lower surfaces of the substrate plate;
[0043] Step 2, preparation of formaldehyde decomposition glue: prepare 5-7 parts of sodium phytate, 2-3 parts of activated carbon, 3.5 parts of sodium p-aminobenzenesulfonate, 0.6 parts of titanium dioxide, 2.5 parts of methyl glycoside, 1.25 parts of ethylenediaminetetraacetic acid, 3.5 parts of ethyl acetate, 11 parts of dicyandiamide, 14.5 parts of carbohydrazide, 14 parts of sodium thiosulfate, 14.5 parts of glycerol, 75 parts of distilled water, and 25 parts of hydrochloric acid; select a 500 ml container, and add sodium phytate, activated carbon, sodium p-aminobenzenesulfonate, titanium dioxide, methyl glycoside, ethylenediaminetetraacetic acid, ethyl acetate, dicyandiamide, carbohydrazide, sodium thiosulfate, glycerol and distilled water to the container, heat and stir until they are completely dissolved to form a transparent solution; then, add hydrochloric acid solution dropwise, control the pH value of the reaction system between 1-3, and maintain the reaction temperature at about 85°C; continue stirring, the reaction system gradually thickens to form a formaldehyde decomposition glue;
[0044] Step 3: Decorative film processing: the formaldehyde decomposition glue prepared in the previous step is evenly applied to both sides of the decorative film through a coating device, and the unevenly applied areas are processed to make the applied thickness uniform;
[0045] Step 4: Assemble: Lay the decorative film coated with formaldehyde decomposition glue on the two side walls of the substrate, and use a pressing device to squeeze the decorative film after laminating to ensure that the decorative film and the side walls of the substrate are completely in contact and squeeze out the bubbles between them, and then place them in a drying device, control the temperature of the drying device at 110 degrees Celsius, and continue drying for 15 minutes;
[0046] Step 5: Edge wrapping: Grind and trim the edges of the laminated sheets, and then wrap the edges after the processing is completed;
[0047] Embodiment 3:
[0048] The specific steps of the formaldehyde purification board production process are as follows:
[0049] Step 1: Select the substrate: Select the corresponding type of plate according to the later use needs, cut it, grind the cut edge after cutting, and grind and polish the upper and lower surfaces of the substrate plate;
[0050] Step 2, preparation of formaldehyde decomposition glue: prepare 7 parts of sodium phytate, 3 parts of activated carbon, 5 parts of sodium p-aminobenzenesulfonate, 1 part of titanium dioxide, 4 parts of methyl glycoside, 2 parts of ethylenediaminetetraacetic acid, 5 parts of ethyl acetate, 12 parts of dicyandiamide, 15 parts of carbohydrazide, 15 parts of sodium thiosulfate, 15 parts of glycerol, 100 parts of distilled water, and 30 parts of hydrochloric acid; select a 500 ml container, and add sodium phytate, activated carbon, sodium p-aminobenzenesulfonate, titanium dioxide, methyl glycoside, ethylenediaminetetraacetic acid, ethyl acetate, dicyandiamide, carbohydrazide, sodium thiosulfate, glycerol and distilled water to the container, heat and stir until they are completely dissolved to form a transparent solution; then, add hydrochloric acid solution dropwise, control the pH value of the reaction system between 1-3, and maintain the reaction temperature at about 90°C; continue stirring, the reaction system gradually thickens to form a formaldehyde decomposition glue;
[0051] Step 3: Decorative film processing: the formaldehyde decomposition glue prepared in the previous step is evenly applied to both sides of the decorative film through a coating device, and the unevenly applied areas are processed to make the applied thickness uniform;
[0052] Step 4: Assemble: Lay the decorative film coated with formaldehyde decomposition glue on the two side walls of the substrate, and use a pressing device to squeeze the decorative film after laminating to ensure that the decorative film and the side walls of the substrate are completely in contact and squeeze out the bubbles between them, and then place them in a drying device, control the temperature of the drying device at 120 degrees Celsius, and continue drying for 20 minutes;
[0053] Step 5: Edge wrapping: Grind and trim the edges of the pressed sheets, and then wrap the edges after the processing is completed.
[0054] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. For those skilled in the art, it is obvious that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention; therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is limited by the attached claims rather than the above description. Therefore, it is intended to include all changes within the meaning and scope of the equivalent elements of the claims in the present invention, and any figure marks in the claims should not be regarded as limiting the claims involved.
[0055] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A production process for formaldehyde purification plate, characterized in that: The specific steps of the formaldehyde purification board production process are as follows: Step 1: Select the substrate: Select the corresponding type of plate according to the later use needs, cut it, grind the cut edge after cutting, and grind and polish the upper and lower surfaces of the substrate plate; Step 2: Preparation of formaldehyde decomposition glue: prepare 5-7 parts of sodium phytate, 2-3 parts of activated carbon, 2-5 parts of sodium p-aminobenzenesulfonate, 0.2-1 parts of titanium dioxide, 1-4 parts of methyl glycoside, 0.5-2 parts of ethylenediaminetetraacetic acid, 2-5 parts of ethyl acetate, 10-12 parts of dicyandiamide, 13-15 parts of carbohydrazide, 13-15 parts of sodium thiosulfate, 14-15 parts of glycerol, 50-100 parts of distilled water, and 20-30 parts of hydrochloric acid; select a 500 ml A container is prepared, and sodium phytate, activated carbon, sodium p-aminobenzenesulfonate, titanium dioxide, methyl glycoside, ethylenediaminetetraacetic acid, ethyl acetate, dicyandiamide, carbohydrazide, sodium thiosulfate, glycerol and distilled water are added to the container, and heated and stirred until they are completely dissolved with each other to form a transparent solution; then, hydrochloric acid solution is added dropwise, the pH value of the reaction system is controlled to be between 1 and 3, and the reaction temperature is maintained at about 80-90° C.; stirring is continued, and the reaction system gradually thickens to form a formaldehyde decomposition glue solution; Step 3: Decorative film processing: the formaldehyde decomposition glue prepared in the previous step is evenly applied to both sides of the decorative film through a coating device, and the unevenly applied areas are processed to make the applied thickness uniform; Step 4: Assemble: Lay the decorative film coated with formaldehyde decomposition glue on the two side walls of the substrate, and use a pressing device to squeeze the decorative film after laminating to ensure that the decorative film and the side walls of the substrate are completely in contact and squeeze out the bubbles between them, and then place them in a drying device, control the temperature of the drying device at 100-120 degrees Celsius, and continue drying for 10-20 minutes; Step 5: Edge wrapping: Grind and trim the edges of the pressed sheets, and then wrap the edges after the processing is completed.
2. The production process of a formaldehyde purification plate according to claim 1, characterized in that: The substrate may include activated carbon substrate, aniline substrate and glass fiber substrate.
3. The production process of a formaldehyde purification plate according to claim 1, characterized in that: The thickness of the substrate is 20-25 mm, and the thickness of the formaldehyde decomposition glue is controlled to be 0.1-0.12 mm.
4. The production process of a formaldehyde purification plate according to claim 1, characterized in that: After the formaldehyde decomposition glue is applied, the substrate needs to be immersed in the preservative liquid for 10-12 minutes. The preparation steps of the preservative liquid are as follows: 10-18 parts of ammonium acryloyldimethyltaurate / VP copolymer, 20-40 parts of sodium fluoride, 30-60 parts of ammonium bifluoride, 10-20 parts of potassium permanganate, and 40-50 parts of potassium chromate are selected as raw materials, mixed with each other and stirred for 5-10 minutes, 15-25 parts of zinc phosphate, 8-18 parts of sodium nitrate, 5-12 parts of praseodymium chloride, 10-16 parts of ethylenediaminetetraacetic acid, 7-14 parts of malic acid, 8-12 parts of sodium dodecylbenzene sulfate, 6-13 parts of nickel sulfate, and 15-25 parts of triethanolamine are added to the mixed solution, and the mixture is stirred again for 1-4 minutes to obtain the formaldehyde decomposition glue.
5. The production process of a formaldehyde purification plate according to claim 1, characterized in that: The edge binding is achieved by using a wooden edge binding strip and gluing it to the side wall of the base plate.
6. The production process of a formaldehyde purification plate according to claim 1, characterized in that: In the step 2, after sodium phytate, activated carbon, sodium p-aminobenzenesulfonate, titanium dioxide, glycoside, ethylenediaminetetraacetic acid, ethyl acetate, dicyandiamide, carbohydrazide, sodium thiosulfate, glycerol and distilled water are mixed, the heating temperature needs to be controlled at 20-30 degrees Celsius.
Citation Information
Patent Citations
Formaldehyde-purification anticorrosion eco-plate and preparation method thereof
CN105058516A
Formaldehyde decomposition liquid
CN107019989A
Preparation method for anti-corrosion boards
CN108035503A