Few-layer MXenes material and green fluoride-free synchronous cleavage preparation method thereof
By using functional composite salt for synchronous etching and peeling at high temperatures, the green and efficient preparation of the small layer of MXenes material is achieved, which solves the problems of complex steps and unfriendly environment in the prior art, and improves the electrochemical performance of the material and Application potential.
Patent Information
- Application Number
- CN202411043626.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-31
AI Technical Summary
The prior art is difficult to obtain a small layer of MXenes material in one step. The traditional method requires two steps of etching and layering. The fluorine-free preparation method is complex in operation and difficult to control the surface functional groups of the material. The traditional method uses fluorine-containing solutions that do not meet environmentally friendly requirements. .
Functional composite salt is used for synchronous etching and peeling at high temperature, and metal salt is used as etching agent and expansion agent to achieve etching and layering by the interaction between etching agent and peeling agent, and a small layer of MXenes material is obtained in one step. .
A green and efficient large-scale preparation of small layers of MXenes materials was achieved, which simplified the preparation process, improved the preparation efficiency, and improved the electrochemical performance of the material by introducing -N functional groups and positive charges, expanding the application field.
Smart Images

Figure CN118993076A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of two-dimensional material preparation, and in particular to a few-layer MXenes material and a green fluorine-free simultaneous cleavage preparation method thereof. Background Art
[0002] Two-dimensional transition metal carbides, nitrides and carbonitrides, also known as MXenes, are a new type of two-dimensional material with the molecular formula M n+1 X n T x , where M is an early transition metal, mainly Ti, Nb, V, Cr, Mo, etc.; X represents C, N or CN; T represents a surface functional group, mainly =O, -F, -OH and -Cl, etc. Due to the excellent conductivity, adjustable structure, rich surface chemical properties, optical properties and magnetic properties of MXenes, it has become a very promising two-dimensional material with a wide range of applications in energy storage, catalysis, electromagnetic interference shielding, optoelectronics, sensing and medicine.
[0003] Currently, MXenes materials are usually prepared by selectively etching the A atomic layer in the MAX phase, where A is a third or fourth main group element, such as Al, Si or Ga (M and X represent the corresponding elements in MXenes respectively).
[0004] Traditional preparation methods require the use of fluorine-containing solutions, which do not meet environmental friendliness requirements and are difficult to control the functional groups on the surface of the material. The currently developed fluorine-free preparation routes, such as high-concentration sodium hydroxide or potassium hydroxide, acidic, halogen and electrochemical etching, still rely on aqueous systems, which makes it difficult to regulate the functional groups on the surface of MXenes, and the operating conditions are harsh and the experimental operation is dangerous. Although high-temperature molten salt etching has paved the way for non-aqueous fluorine-free preparation of MXenes, multi-layer MXenes are obtained, and intercalation agents need to be added to peel the materials into a few layers or a single layer. The current fluorine-free etching method is difficult to obtain a few-layer MXenes material in one step. It requires two steps of etching and delamination, which is complicated to operate, and the introduction of intercalation agents may destroy the structure of MXenes and cause defects. Therefore, it is urgent to develop a method suitable for the green, efficient and large-scale preparation of few-layer MXenes materials, develop a "one-step" fluorine-free preparation system, and realize the efficient preparation of few-layer MXenes materials. Summary of the invention
[0005] In view of this, the technical problem to be solved by the present invention is to provide a few-layer MXenes material and a green fluorine-free simultaneous cleavage preparation method thereof, so as to realize the etching and stratification of MAX materials in one step.
[0006] The present invention provides a few-layer MXenes material, wherein the number of layers of the few-layer MXenes material is ≤20 layers, and the few-layer MXenes material comprises a single-layer MXene material.
[0007] In the present invention, the above-mentioned number of layers is limited to Ti3C2T x An atomic layer is defined as one layer. It can be 2 to 20 layers, or it can be a single layer of MXene material.
[0008] Preferably, the few-layer MXenes material of the present invention comprises a single-layer MXene material.
[0009] The presence of single-layer MXene materials improves the overall electrochemical performance of the few-layer MXenes materials, which is expected to expand the application areas of MXenes materials in the future.
[0010] In the present invention, the surface of the few-layer MXenes material is positively charged.
[0011] In the present invention, the surface functional groups of the few-layer MXenes material include -Cl, =O and -N.
[0012] The few-layer MXenes material provided by the present invention is different from the existing multi-layer MXenes with -Cl and =O functional groups. Its surface functional groups include -Cl, =O and -N, and the introduction of -N significantly improves the electrochemical performance of the material.
[0013] Furthermore, the surface of the few-layer MXenes material provided by the present invention carries a positive charge, which is different from the current negatively charged MXenes. The few-layer MXenes material with a positive charge on the surface is expected to expand its application field.
[0014] The present invention provides a green fluorine-free simultaneous cleavage preparation method for a few-layer MXenes material, comprising the following steps:
[0015] The MAX phase material is subjected to a high-temperature reaction in a functional composite salt, and etching and stripping are simultaneously achieved, and a few-layer MXenes material is obtained after washing.
[0016] In the present invention, functional composite salt is used to achieve simultaneous etching-stripping. Preferably, the functional composite salt is a deep eutectic solvent.
[0017] In the present invention, the cleavage refers to simultaneous etching-stripping.
[0018] The above-mentioned etching specifically refers to using an etchant to etch the A atomic layer in the MAX phase to obtain a two-dimensional MXenes material.
[0019] The above-mentioned stripping specifically refers to the decomposition of the stripping agent at high temperature to produce a large amount of gas, which expands the material.
[0020] The etching mechanism of the present invention is as follows:
[0021] Lewis acid etchants with higher redox potentials etch A elements from the MAX phase;
[0022] M1H x +M2AX→M2X+M1+AH y ↑
[0023] The present invention applies functional composite salts to the preparation of few-layer MXenes, using the metal salts therein as etchants, and the stripping agents therein as expansion agents. Due to the interaction between the etchant and the expansion agent, the etchant brings the expansion agent into the interlayer during the etching of the A atomic layer. At high temperatures, the expansion agent decomposes into a large amount of gas, which can play a role in propping up the interlayer. Therefore, the etching and stratification process of the MAX phase of the reaction system is completed in one step, and the etching and stratification can be efficiently achieved during the reaction process, simplifying the preparation process, and directly obtaining few-layer MXenes in one step, which can improve the efficiency of the preparation.
[0024] Preferably, the functional composite salt comprises an etchant and a stripper.
[0025] Preferably, the etchant includes any one or more of metal salts.
[0026] The metal salt preferably includes, but is not limited to, any one or a combination of two or more of SnCl4, GeCl4, InCl3, MnCl2, CdCl2, FeCl2, CoCl2, CuCl2, NiCl2, ZnCl2, AgCl, SnBr4, GeBr4, InBr3, MnBr2, CdBr2, FeBr, CoBr2, CuBr2, NiBr2, ZnBr2, AgBr, SnI4, GeI4, InI3, MnI2, CdI2, FeI2, CoI2, CuI2, NiI2, ZnI2, AgI, etc.
[0027] Preferably, the stripping agent includes but is not limited to any one or a combination of two or more of quaternary ammonium salts, urea, thiourea, N-methyl urea, dimethyl urea, acetamide, bistrifluoromethanesulfonimide, glycerol, adipic acid, citric acid, oxalic acid, ethylenediaminetetraacetic acid, sodium bicarbonate, and ammonium chloride.
[0028] The quaternary ammonium salt preferably includes, but is not limited to, one or more of choline chloride and chlormequat chloride.
[0029] The molar ratio of the MAX material to the etchant is preferably 1:(2-10). If the ratio of the etchant is too low, it will not be conducive to a complete reaction, and if it is too high, it will cause oxidation of the material. The above ratio range can ensure that the reaction proceeds smoothly and the material is not oxidized.
[0030] The molar ratio of the etchant to the stripper is preferably 1:(0.5-5).
[0031] The present invention uses MAX material as raw material, and the present invention has no special limitation on the MAX material. Experimental results show that the method provided by the present invention is applicable to most MAX.
[0032] Preferably, the molecular formula of the MAX phase material is M n+1 AX n , wherein M is preferably any one of Sc, Ti, V, Cr, Mn, Y, Zr, Nb, Mo, La, Hf, Ta, and W, or a combination of two or more thereof; A is preferably a VIIB, VIII, IB, IIB, IIIA, IVA, VA, or VIA group element; X is preferably any one of C and N, or a combination of two thereof; and n is preferably 1, 2, 3, or 4.
[0033] Further preferably, the MAX material includes but is not limited to any one or a combination of two or more of Ti2AlC, Ti2SnC, Ti2GaC, Ti2AlN, Ti3AlC2, Ti3AlN3, Ti3AlCN, Ti3SiC2, Ti3SnC2, Ti4AlN3, Ta2AlC, Ta3AlC2, Ta4AlC3, Nb2AlC, Nb4AlC3, V2AlC, V2GaC, V2GeC, V2ZnC, V2SnC, V4AlC3, VCrAlC, Cr2AlC, Cr2GaC, Cr2GaN, Sc2AlC, Zr2AlC, Zr2SnC, Mo2AlC, Mo2Ga2C, Mo2GaC, Mo2GaN, Mo2Ti2AlC3, Mo2Ti2AlC3, Hf2AlC, Hf2AlN, etc.
[0034] Preferably, in the present invention, the MAX material and the metal salt are first mixed to obtain a mixture A, and then the mixture A and the stripping agent are mixed to obtain a mixture B.
[0035] Then, the mixture B is put into a crucible, and then the crucible is put into a quartz glass tube, an inert gas is introduced, and the sample C is obtained by calcining at a high temperature for a certain period of time.
[0036] The temperature of the high temperature calcination is preferably 400-800°C. In some specific embodiments of the present invention, the temperature of the high temperature calcination is 500°C.
[0037] If the temperature of high-temperature calcination is too low, it will be detrimental to the reaction kinetics, resulting in the material being unable to react or reacting incompletely. If the temperature is too high, the material will oxidize and even break chemical bonds.
[0038] The high temperature calcination time is 30 minutes to 24 hours. In some specific embodiments of the present invention, the high temperature calcination time is 1 hour.
[0039] If the time is too short, it will not be conducive to complete reaction, and if it is too long, it will cause oxidation of the material.
[0040] The high-temperature calcination is preferably carried out in an inert gas atmosphere, and the inert gas is preferably argon.
[0041] After high-temperature calcination, sample C is cooled to room temperature and a detergent is added to remove impurities. The present invention has no special limitation on the detergent, which can be an oxidant well known to those skilled in the art, including but not limited to one or more of ferric chloride, ammonium persulfate, and hydrochloric acid. The detergent can effectively remove the by-products obtained by the reaction.
[0042] Preferably, the washing and impurity removal further comprises drying.
[0043] The present invention has no particular limitation on the drying method, and preferably one or more of vacuum oven drying and freeze dryer drying are used to prevent the material from being overly exposed to the air and causing oxidation of the material.
[0044] The present invention also provides a few-layer MXenes material prepared by the above-mentioned preparation method. The present invention adopts the above-mentioned method to bring new physical and chemical properties to the MXenes material, thereby expanding the storage method and application field of the material to a certain extent.
[0045] The few-layer MXenes material prepared by the present invention can be applied to various fields, such as supercapacitors, alkali metal ion secondary batteries (lithium ion batteries, sodium ion batteries, etc.), catalysis, etc.; the prepared few-layer MXenes material can be used as an electrode material in a supercapacitor, or as a negative electrode material in an alkali metal ion battery, or as an effective carrier of active substances in lithium-sulfur batteries and lithium-air batteries, or as a catalytic material.
[0046] Based on this, the present invention provides a supercapacitor or an alkali metal ion secondary battery, comprising a few-layer MXenes material prepared by the above preparation method.
[0047] Compared with the prior art, the present invention provides a green fluorine-free simultaneous cleavage preparation method for few-layer MXenes materials, comprising the following steps: subjecting MAX phase materials to a high-temperature reaction in a functional composite salt, achieving simultaneous etching and stripping, and obtaining a few-layer MXenes material after washing. The present invention applies functional composite salts to the preparation of few-layer MXenes, and etching and stratification are performed simultaneously without the need for a fluorine-containing solution, thereby achieving a one-step preparation of a few-layer MXenes material. The preparation method is efficient, environmentally friendly, and suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 The scanning electron microscope images and transmission electron microscope images of few-layer MXenes and multi-layer MXenes;
[0049] Figure 2 Atomic force microscopy images of single-layer MXenes;
[0050] Figure 3 EDS spectra of Cl, O, and N of few-layer MXenes;
[0051] Figure 4 The rate performance diagrams of few-layer MXenes and multi-layer MXenes;
[0052] Figure 5 Long cycle performance diagram of few-layer MXenes and multi-layer MXenes;
[0053] Figure 6 Zeta potential diagram of few-layer MXenes and multi-layer MXenes. DETAILED DESCRIPTION
[0054] In order to further illustrate the present invention, the method for preparing few-layer MXenes by a one-step method using a green fluorine-free solvent provided by the present invention is described in detail below in conjunction with the examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the invention.
[0055] All raw materials of the present invention have no particular limitation on their sources, and can be purchased from the market or prepared according to conventional methods known to those skilled in the art.
[0056] Example 1
[0057] (1) mixing the etching raw materials Ti3AlC2 and CuCl2 in a molar ratio of 1:2 to obtain a mixture A, and then mixing the mixture A with 1 molar ratio of urea to obtain a mixture B;
[0058] (2) Place the mixture B in a crucible, then place the crucible in a quartz glass tube, introduce argon gas, and calcine at 500°C for 1 h to obtain sample C;
[0059] (3) After cooling sample C to room temperature, 1 mol of ferric chloride is added to wash and remove impurities to obtain sample D, and then sample D is dried using a freeze dryer to obtain a few-layer MXene material.
[0060] The prepared few-layer MXene material was tested, and the results are as follows Figure 1As shown in Figure a, the left figure is a scanning electron microscope image, and the right figure is a transmission electron microscope image. It can be seen that a few-layer MXene material was prepared in this embodiment, and it contains a single layer of MXene. The results are as follows Figure 2 shown.
[0061] The prepared few-layer MXene material was tested by EDS spectrum, and the results are as follows: Figure 3 As shown, it can be seen that the surface functional groups of the few-layer MXene material prepared by the present invention include -Cl, =O and -N.
[0062] Example 2
[0063] The implementation method is the same as Example 1, except that in step (1), Ti3AlC2 and CuCl2 are evenly mixed in a ratio of 1:3 to prepare a few-layer MXene material.
[0064] Example 3
[0065] The implementation method is the same as Example 1, except that in step (1), Ti3AlC2 and CuCl2 are evenly mixed in a ratio of 1:4 to prepare a few-layer MXene material.
[0066] Example 4
[0067] The implementation method is the same as Example 1, except that in step (1), Ti3AlC2 and CuCl2 are evenly mixed in a ratio of 1:6 to prepare a few-layer MXene material.
[0068] Example 5
[0069] The implementation method is the same as Example 1, except that in step (1), Ti3AlC2 and ZnCl2 are evenly mixed in a ratio of 1:2 to prepare a few-layer MXene material.
[0070] Example 6
[0071] The implementation method is the same as Example 1, except that in step (1), Ti3AlC2 and ZnCl2 are evenly mixed in a ratio of 1:4 to prepare a few-layer MXene material.
[0072] Example 7
[0073] The implementation method is the same as Example 1, except that in step (1), Ti3AlC2 and ZnCl2 are evenly mixed in a ratio of 1:6 to prepare a few-layer MXene material.
[0074] Example 8
[0075] The implementation method is the same as Example 1, except that in step (1), Ti3AlC2 and FeCl2 are evenly mixed in a ratio of 1:3 to prepare a few-layer MXene material.
[0076] Example 9
[0077] The implementation method is the same as Example 1, except that in step (1), Ti3AlC2 and FeCl2 are evenly mixed in a ratio of 1:6 to prepare a few-layer MXene material.
[0078] Example 10
[0079] The implementation method is the same as Example 1, except that in step (1), Ti3AlC2 and CoCl2 are evenly mixed in a ratio of 1:3 to prepare a few-layer MXene material.
[0080] Embodiment 11
[0081] The implementation method is the same as Example 1, except that in step (1), Ti3AlC2 and CoCl2 are evenly mixed in a ratio of 1:6 to prepare a few-layer MXene material.
[0082] Example 12
[0083] The implementation method is the same as Example 1, except that in step (1), Ti3AlC2 and CoCl2 are evenly mixed in a ratio of 1:9 to prepare a few-layer MXene material.
[0084] Example 13
[0085] The implementation method is the same as Example 1, except that, in step (1), mixture A and N-methylurea are uniformly mixed to obtain mixture B, thereby preparing a few-layer MXene material.
[0086] Embodiment 14
[0087] The implementation method is the same as Example 1, except that, in step (1), mixture A and acetamide are uniformly mixed to obtain mixture B, thereby preparing a few-layer MXene material.
[0088] Embodiment 15
[0089] The implementation method is the same as that of Example 1, except that, in step (1), mixture A and bis(trifluoromethanesulfonyl)imide are uniformly mixed to obtain mixture B, thereby preparing a few-layer MXene material.
[0090] Example 16
[0091] The implementation method is the same as that of Example 1, except that, in step (1), mixture A and propylene glycol are uniformly mixed to obtain mixture B, thereby preparing a few-layer MXene material.
[0092] Embodiment 17
[0093] The implementation method is the same as that of Example 1, except that, in step (1), mixture A and adipic acid are uniformly mixed to obtain mixture B, thereby preparing a few-layer MXene material.
[0094] Embodiment 18
[0095] The implementation method is the same as that of Example 1, except that, in step (1), mixture A and sodium bicarbonate are uniformly mixed to obtain mixture B, thereby preparing a few-layer MXene material.
[0096] Embodiment 19
[0097] The implementation method is the same as Example 1, except that in step (1), the high-temperature calcination temperature is 700° C. to prepare a few-layer MXene material.
[0098] Embodiment 20
[0099] The implementation method is the same as Example 1, except that in step (1), the high-temperature calcination time is 4 hours to prepare a few-layer MXene material.
[0100] Embodiment 21
[0101] The implementation method is the same as Example 1, except that in step (1), the reaction raw material is V2AlC, and a few-layer MXene material is prepared.
[0102] Embodiment 22
[0103] The implementation method is the same as Example 1, except that in step (1), the reaction raw material is Ta2AlC, and a few-layer MXene material is prepared.
[0104] Comparative Example 1
[0105] The implementation method is the same as Example 1, except that no stripping agent is added, and a multilayer MXene material is finally obtained.
[0106] The prepared multilayer MXene material was tested and the results were as follows: Figure 1 As shown in Figure b, the left picture is a transmission electron microscope picture, and the right picture is a scanning electron microscope picture. It can be seen that in the system without adding a stripping agent, a multi-layer MXene material was prepared, while adding a stripping agent can obtain a few-layer MXene.
[0107] Electrochemical performance test
[0108] The target materials prepared in Examples 1 to 21 and Comparative Example 1 were respectively applied to lithium ion batteries. The specific steps for preparing the lithium ion batteries are as follows:
[0109] The target material was uniformly mixed with acetylene carbon black and PVDF in a ratio of 70:15:15 (wt.%), applied on a 2cm×2cm copper foil current collector, and dried at 100°C;
[0110] The prepared electrode pieces are placed in the order of negative electrode shell, spring sheet, gasket, negative electrode, diaphragm, positive electrode and positive electrode shell. After a certain amount of electrolyte is added, the assembled capacitor is sealed at a pressure of 50MPa using a sealing machine to obtain a button battery. The button battery is left to stand for 24 hours and the electrochemical performance is tested. The electrolyte used in this embodiment is an organic solution of one mole of lithium hexafluorophosphate (LiPF6) dissolved in ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC).
[0111] The test results are as follows Figure 4 and Figure 5 shown. Figure 4 This is the rate performance diagram of few-layer MXene and multi-layer MXene. Figure 5 This is a graph of the long-cycle performance of few-layer MXene and multi-layer MXene.
[0112] It can be seen that the rate performance and long cycle performance of few-layer MXene are better than those of multi-layer MXene.
[0113] Figure 6 It is the Zeta potential diagram of few-layer MXene and multi-layer MXene. It can be seen that, unlike the existing multi-layer MXene with negative charge on the surface, the few-layer MXene material prepared in the present invention has positive charge on the surface.
[0114] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A few-layer MXenes material, characterized in that: The number of layers of the few-layer MXenes material is ≤20, and the few-layer MXenes material comprises a single-layer MXene material.
2. The few-layer MXenes material according to claim 1, characterized in that: The surface of the few-layer MXenes material is positively charged, and the surface functional groups include -Cl, =O and -N.
3. A green fluorine-free simultaneous cleavage preparation method for a few-layer MXenes material, comprising the following steps: The MAX phase material is subjected to a high-temperature reaction in a functional composite salt to achieve simultaneous etching and stripping, and a few-layer MXenes material is obtained after washing.
4. The method according to claim 3, characterized in that: The molecular formula of the MAX phase material is M n+1 AX n , wherein M is any one of Sc, Ti, V, Cr, Mn, Y, Zr, Nb, Mo, La, Hf, Ta, and W, or a combination of two or more thereof; A is a VIIB, VIII, IIB, IIB, IIIA, IVA, VA, or VIA element; X is any one of C and N, or a combination of two thereof; and n is 1, 2, 3, or 4.
5. The method according to claim 4, characterized in that The MAX material includes any one of Ti2AlC, Ti2SnC, Ti2GaC, Ti2AlN, Ti3AlC2, Ti3AlN3, Ti3AlCN, Ti3SiC2, Ti3SnC2, Ti4AlN3, Ta2AlC, Ta3AlC2, Ta4AlC3, Nb2AlC, Nb4AlC3, V2AlC, V2GaC, V2GeC, V2ZnC, V2SnC, V4AlC3, VCrAlC, Cr2AlC, Cr2GaC, Cr2GaN, Sc2AlC, Zr2AlC, Zr2SnC, Mo2AlC, Mo2Ga2C, Mo2GaC, Mo2GaN, Mo2Ti2AlC3, Mo2Ti2AlC3, Hf2AlC, and Hf2AlN, or a combination of two or more thereof.
6. The method according to claim 3, characterized in that The functional composite salt includes an etchant and a stripper; The etchant includes any one or more of metal salts; The stripping agent includes any one of quaternary ammonium salt, urea, thiourea, N-methyl urea, dimethyl urea, acetamide, bis(trifluoromethanesulfonyl)imide, glycerol, adipic acid, citric acid, oxalic acid, ethylenediaminetetraacetic acid, sodium bicarbonate, and ammonium chloride, or a combination of two or more thereof.
7. The method according to claim 6, characterized in that The metal salt includes any one of SnCl4, GeCl4, InCl3, MnCl2, CdCl2, FeCl2, CoCl2, CuCl2, NiCl2, ZnCl2, AgCl, SnBr4, GeBr4, InBr3, MnBr2, CdBr2, FeBr, CoBr2, CuBr2, NiBr2, ZnBr2, AgBr, SnI4, GeI4, InI3, MnI2, CdI2, FeI2, CoI2, CuI2, NiI2, ZnI2, and AgI, or a combination of two or more thereof.
8. The method according to claim 6, characterized in that The molar ratio of the MAX material to the etchant is 1:(2-10); The molar ratio of the etchant to the stripper is 1:(0.5-5).
9. The method according to claim 3, characterized in that: The temperature of the high temperature reaction is 400-800°C and the time is 30min-24h; The high temperature reaction is carried out in an inert gas atmosphere.
Citation Information
Patent Citations
Etching method of MXene material
CN114408873A
Method for preparing MXene two-dimensional material with phosphorus functional group in gas phase
CN117466297A
Method for modifying functional groups on surface of MXene material
CN117602623A
Method for HF-free facile and rapid synthesis of mxenes related compounds
US20200399771A1