Doping and coating co-modified precursor as well as preparation method and application thereof

By doping Zr, Al, Ti, and La with fluoride coating, the problems of long lithium-ion migration paths and poor rate performance of single-crystal ternary cathode materials are solved, improving the electrochemical performance and stability of the materials, making them suitable for large-scale production of lithium-ion batteries.

CN118993176APending Publication Date: 2024-11-22JINGMEN GEM NEW MATERIAL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411239145.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Single-crystal ternary cathode materials in lithium-ion batteries suffer from long lithium-ion migration paths and poor rate performance. Furthermore, existing coating methods are uneven and require more sintering cycles, and the improvement effect of doping elements is limited.

Method used

A ternary hydroxide is doped with at least two elements selected from Zr, Al, Ti and La, and fluoride and ternary hydroxide are used for synergistic coating. Doping and coating are achieved in a reactor by co-precipitation to form a precursor of core and coating layer.

Benefits of technology

It improves the kinetic performance and structural stability of cathode materials, enhances discharge capacity, cycle performance and rate performance, simplifies the process, reduces costs, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993176A_ABST
    Figure CN118993176A_ABST
Patent Text Reader

Abstract

The invention discloses a doped and coated co-modified precursor as well as a preparation method and application thereof. The doped and coated co-modified precursor comprises an inner core and a coating layer, the inner core is a ternary hydroxide containing a doping element M, the M comprises at least two of Zr, Al, Ti and La, the coating layer comprises a fluoride and the ternary hydroxide, the mass ratio of the fluoride in the coating layer is greater than 50%, and the fluoride comprises tungsten fluoride. The ternary hydroxide is doped with at least two of Zr, Al, Ti and La, and the fluoride containing tungsten fluoride and the ternary hydroxide are cooperatively coated, so that the doping and coating effects of the precursor in the subsequent preparation process of the positive electrode material can be improved, and the dynamic performance and the structural stability are improved; and the discharge capacity, the cycle performance and the rate capability of the positive electrode material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of batteries and relates to a doping, coating and co-modified precursor and a preparation method and application thereof. Background Art

[0002] With the rapid development of the electric vehicle industry in recent years, people's demand for high energy density lithium-ion batteries has increased day by day. The positive electrode material is the key to improving the energy density of lithium-ion batteries. Among them, the nickel-rich ternary positive electrode material LiNi x Co y Mn 1-x-y O2 (0.6≤x<1) has advantages such as high energy density and long cycle life, and occupies an important position in the power battery market. However, the traditional polycrystalline nickel-rich ternary positive electrode has problems such as poor structural stability and rapid capacity decay. The single crystal strategy can effectively solve the above problems.

[0003] The single-crystal ternary positive electrode material is composed of individual micron-sized particles, has high mechanical strength, is not easy to break during the electrode sheet rolling process, and will not produce intercrystalline cracks during the charge and discharge cycle. It has better cycle stability and is a high-performance positive electrode material that is expected to partially replace polycrystalline ternary positive electrode materials.

[0004] However, the application of single-crystal ternary cathode materials also faces some challenges. For example, the single crystal particle size is large and the lithium ion migration path is long, resulting in poor rate performance. To this end, researchers have tried to modify the single-crystal ternary cathode materials by doping and coating, which can effectively alleviate the above problems and optimize their electrochemical performance. Ion doping focuses on improving the lithium ion diffusion kinetics and the stability of the lattice structure, while surface coating focuses on alleviating electrolyte-cathode interface side reactions and improving interface stability. The combination of doping and coating can more comprehensively improve the performance of single-crystal ternary cathode materials. However, in terms of coating, the coating elements are mostly added during the sintering stage, which not only increases the number of sintering times, but also the coated materials are not uniform. Moreover, the improvement effect of doping elements on single-crystal cathode materials needs further study.

[0005] Therefore, providing a precursor suitable for single crystal positive electrode materials to effectively improve the kinetic properties of single crystal positive electrode materials and improve their stability and rate performance is a technical problem that needs to be solved urgently. Summary of the invention

[0006] In view of the above problems existing in the prior art, the object of the present invention is to provide a doping-coating-coated co-modified precursor and a preparation method and application thereof.

[0007] To achieve the above object, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a doped-coated co-modified precursor, the doped-coated co-modified precursor comprising a core and a coating layer, the core being a ternary hydroxide containing a doping element M, M comprising at least two of Zr, Al, Ti and La, the coating layer comprising fluoride and ternary hydroxide, the mass proportion of the fluoride in the coating layer being greater than 50%, and the fluoride comprising tungsten fluoride.

[0009] The present invention adopts at least two of Zr, Al, Ti and La to dope the ternary hydroxide, and uses fluoride and ternary hydroxide for synergistic coating, which can improve the doping and coating effects of the precursor in the subsequent process of preparing positive electrode materials, improve the kinetic performance and structural stability, thereby improving the discharge capacity, cycle performance and rate performance of the positive electrode material.

[0010] The coating layer of the present invention uses fluoride as the main component, which can effectively stabilize the structure of the material and help improve the kinetic performance of the positive electrode material, thereby enhancing the performance of the positive electrode material. This is because: fluoride can form a coating layer on the surface of the material, which has a stronger effect of resisting the corrosion of the positive electrode material by the electrolyte decomposition product HF, reduces the dissolution of Ni and Co, inhibits the side reaction between the positive electrode material and the electrolyte, reduces the irreversible phase change on the surface of the material, and improves the stability of the material; moreover, F - The electronegativity of the positive electrode material is relatively large, so the metal ions in the positive electrode material and F - The bond strength between them is stronger, which can make its structure more stable, which shows that metal fluorides have better stability. In addition, metal fluorides have high theoretical specific capacity, low price, wide source, non-toxicity and good safety. At the same time, since fluorides include tungsten fluoride, on the basis of the above effects, after co-precipitation, the tungsten element will exist at the surface interface of the core, which supports the spatial structure of the precursor. The tungsten element uniformly doped in the surface interface area diffuses into the interior of the particles during the sintering process and is evenly distributed, which is conducive to further stabilizing the surface activity of the material.

[0011] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.

[0012] Preferably, the ternary hydroxide is nickel-cobalt-manganese hydroxide.

[0013] Preferably, the molar percentage of the doping element M in the core is 0.05-0.4, for example, it can be 0.05, 0.06, 0.08, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35 or 0.4.

[0014] Preferably, the fluoride further includes at least one of aluminum fluoride, cobalt fluoride, magnesium fluoride and sodium fluoride.

[0015] Preferably, based on the total mass of the ternary hydroxide in the doping-coating-coated co-modified precursor (excluding doping elements and fluorides), the content of the fluoride is 0.01-1%, for example, it can be 0.01%, 0.02%, 0.05%, 0.07%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, 0.55%, 0.6%, 0.65%, 0.7%, 0.75%, 0.8%, 0.85%, 0.9% or 1%, etc.

[0016] Preferably, based on the total mass of the ternary hydroxide in the doping-coating-coated co-modified precursor (excluding doping elements and fluorides), the content of tungsten fluoride is 0.01-0.3%, for example, it can be 0.01%, 0.02%, 0.05%, 0.07%, 0.1%, 0.15%, 0.2%, 0.25% or 0.3%, etc.

[0017] In a second aspect, the present invention provides a method for preparing a doping-coating-coated co-modified precursor as described in the first aspect, the preparation method comprising the following steps:

[0018] (1) adding a ternary mixed salt solution, a doping element salt solution, a precipitant solution and a complexing agent solution into a reactor for coprecipitation reaction, and stopping feeding when the particle size reaches a preset particle size of the inner core;

[0019] (2) The doping element salt solution is replaced with a fluoride solution, and the coprecipitation reaction is continued to obtain a doping, coating and co-modified precursor.

[0020] In the method of the present invention, when the coprecipitation reaction is continued in step (2), the precipitant solution, the complexing agent solution and the ternary mixed salt solution are still in the state of being introduced. In one embodiment, the types and parameter control of the above three solutions are the same as step (1).

[0021] The method of the present invention utilizes the method of coprecipitation to perform doping and coating in stages, which can realize uniform doping of doping elements in the ternary precursor and uniform coating of its surface, merge the precursor doping and coating processes, and realize the co-modification of doping and coating of the precursor through simple coprecipitation in the reactor, omit the equipment for secondary treatment of precursor or positive electrode material particles in the conventional coating process, and do not need to take out the precursor from the coprecipitation reactor and transfer it to other devices for coating operation, simplify the process flow, reduce costs, and be suitable for large-scale industrial production. Moreover, the precursor prepared by the method of the present invention has uniform particle size and good consistency, and the positive electrode material prepared by the method has high interface stability and less residual alkali, which helps to improve the electrochemical performance of the material.

[0022] Preferably, the concentration of the ternary mixed salt solution in step (1) is 80-120 g / L, for example, it can be 80 g / L, 85 g / L, 90 g / L, 95 g / L, 100 g / L, 105 g / L, 110 g / L, 115 g / L or 120 g / L, etc.

[0023] Preferably, the feed rate of the ternary mixed salt solution in step (1) is 8 to 10 L / h, for example, 8 L / h, 8.5 L / h, 9 L / h, 9.5 L / h or 10 L / h.

[0024] Preferably, the concentration of the doping element salt solution in step (1) is 0.01-0.05 mol / L, for example, it can be 0.01 mol / L, 0.02 mol / L, 0.03 mol / L, 0.04 mol / L or 0.05 mol / L.

[0025] Preferably, the feed rate of the doping element salt solution in step (1) is 1 to 2 L / h, for example, 1 L / h, 1.2 L / h, 1.4 L / h, 1.5 L / h, 1.8 L / h or 2 L / h.

[0026] Preferably, the mass concentration of the precipitant solution in step (1) is 20-50%, for example, it can be 20%, 22%, 25%, 27%, 30%, 35%, 40%, 45%, 48% or 50%, etc.

[0027] Preferably, the feed rate of the precipitant solution in step (1) is 1.5 to 3 L / h, for example, 1.5 L / h, 1.6 L / h, 1.8 L / h, 2 L / h, 2.2 L / h, 2.5 L / h, 2.7 L / h or 3 L / h, etc.

[0028] Preferably, the mass concentration of the complexing agent solution in step (1) is 10-30%, for example, it can be 10%, 12%, 14%, 15%, 17%, 20%, 23%, 26%, 28% or 30%.

[0029] Preferably, the feeding rate of the complexing agent solution in step (1) is 0.5 to 3 L / h, for example, it can be 0.5 L / h, 0.6 L / h, 0.8 L / h, 1 L / h, 1.2 L / h, 1.5 L / h, 1.7 L / h, 2 L / h, 2.2 L / h, 2.4 L / h, 2.6 L / h, 2.8 L / h or 3 L / h, etc.

[0030] Preferably, the coprecipitation reaction time in step (1) is 24 to 48 hours, for example, it can be 24 hours, 26 hours, 28 hours, 30 hours, 32 hours, 35 hours, 38 hours, 40 hours, 42 hours, 45 hours, 46 hours or 48 hours.

[0031] Preferably, the coprecipitation reaction in step (1) is accompanied by stirring, and the stirring speed is 100 to 500 r / min, for example, it can be 100 r / min, 150 r / min, 200 r / min, 250 r / min, 300 r / min, 350 r / min, 400 r / min, 450 r / min or 500 r / min.

[0032] Preferably, the temperature of the coprecipitation reaction in step (1) is controlled within the range of 55-60°C, and the temperature may be, for example, 55°C, 56°C, 57°C, 58°C or 60°C.

[0033] Preferably, the pH of the coprecipitation reaction in step (1) is controlled within the range of 10.0 to 12.0, and the pH may be, for example, 10.0, 10.2, 10.3, 10.5, 10.7, 11.0, 11.3, 11.6, 11.8 or 12.0.

[0034] In one embodiment, the preset particle size of the inner core is a particle size D50=2-5 μm, for example, 2 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm or 5 μm.

[0035] Preferably, the concentration of the fluoride solution in step (2) is 10-20 g / L, for example, it can be 10 g / L, 12 g / L, 13 g / L, 15 g / L, 16 g / L, 17 g / L, 18 g / L, 19 g / L or 20 g / L.

[0036] Preferably, the feeding rate of the fluoride solution in step (2) is 2 to 4 L / h, for example, 2 L / h, 2.2 L / h, 2.5 L / h, 2.7 L / h, 3 L / h, 3.5 L / h or 4 L / h.

[0037] Preferably, the feeding rate of the fluoride solution is 8 to 10 L / h, for example, 8 L / h, 8.5 L / h, 9 L / h, 9.5 L / h or 10 L / h.

[0038] As a preferred technical solution of the preparation method of the present invention, the time for continuing the coprecipitation reaction in step (2) is 0.5 to 3 hours, for example, it can be 0.5 hours, 1 hour, 1.5 hours, 2 hours, 2.5 hours or 3 hours.

[0039] Preferably, the process of continuing the coprecipitation reaction in step (2) is accompanied by stirring, and the stirring speed is 100-500 r / min, for example, it can be 100 r / min, 150 r / min, 200 r / min, 250 r / min, 300 r / min, 350 r / min, 400 r / min, 450 r / min or 500 r / min.

[0040] Preferably, the temperature of the continued coprecipitation reaction in step (2) is controlled in the range of 55-60°C, for example, 55°C, 56°C, 57°C, 58°C, 59°C or 60°C.

[0041] Preferably, the pH of the continued coprecipitation reaction in step (2) is controlled within the range of 10.0 to 12.0, and the pH may be, for example, 10.0, 10.2, 10.3, 10.5, 10.7, 11.0, 11.3, 11.6, 11.8 or 12.0.

[0042] Preferably, after the coprecipitation reaction in step (2) is completed, the product is washed and dried to obtain a precursor powder.

[0043] In a third aspect, the present invention provides a positive electrode material, which is prepared by the doping, coating and co-modified precursor described in the first aspect.

[0044] Preferably, the positive electrode material is a high-nickel single crystal positive electrode material, wherein the molar content of nickel is greater than or equal to 0.6, for example, it can be 0.6, 0.62, 0.63, 0.65, 0.66, 0.67, 0.68, 0.7, 0.72, 0.74, 0.75, 0.77, 0.78, 0.8, 0.82, 0.83, 0.85, 0.88 or 0.9, etc.

[0045] Since the precursor has a coating layer, the main component of which is fluoride, the cathode material prepared using the precursor has good structural stability, because the surface coating of fluoride can effectively reduce the side reaction between the electrode material and the electrolyte and improve the performance of the material. At the same time, the tungsten fluoride in the fluoride can be used for doping during the sintering process. The tungsten element diffuses into the interior of the particles during the sintering process, and the fluorine element tends to be enriched on the surface and evenly distributed, which is beneficial to improving the performance of the material.

[0046] In a fourth aspect, the present invention provides a method for preparing the positive electrode material as described in the third aspect, comprising the following steps:

[0047] The doped, coated and co-modified precursor is mixed with lithium salt and sintered to obtain the positive electrode material.

[0048] The present invention does not specifically limit the type of lithium salt, including but not limited to one or more of lithium oxide, lithium carbonate, lithium nitrate, lithium chloride and lithium acetate.

[0049] Preferably, the molar ratio of the lithium salt to the doping-coating-coated co-modified precursor is (1.03-1.06):1, for example, it can be 1.03:1, 1.04:1, 1.05:1 or 1.06:1.

[0050] Preferably, the mixing speed is 500-1100 r / min, for example, it can be 500 r / min, 550 r / min, 600 r / min, 650 r / min, 700 r / min, 750 r / min, 800 r / min, 850 r / min, 900 r / min, 950 r / min, 1000 r / min, 1050 r / min or 1100 r / min, etc.; the mixing time is 5-20 min, for example, it can be 5 min, 8 min, 10 min, 12 min, 15 min, 17 min or 20 min, etc.

[0051] Preferably, the sintering atmosphere is an oxygen-containing atmosphere, for example, an oxygen atmosphere.

[0052] Preferably, the sintering temperature is 800-900°C, for example, it can be 800°C, 820°C, 840°C, 860°C, 880°C or 900°C; the sintering time is 12-22h, for example, it can be 12h, 13h, 13.5h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h or 22h.

[0053] In a fifth aspect, the present invention provides a battery, comprising the positive electrode material described in the third aspect.

[0054] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0055] Compared with the prior art, the present invention has the following beneficial effects:

[0056] (1) The present invention uses at least two of Zr, Al, Ti and La to dope the ternary hydroxide, and uses fluoride containing tungsten fluoride and the ternary hydroxide for synergistic coating, which can improve the doping and coating effects of the precursor in the subsequent preparation of the positive electrode material, improve the kinetic performance and structural stability, thereby improving the discharge capacity, cycle performance and rate performance of the positive electrode material.

[0057] (2) The method of the present invention utilizes the method of coprecipitation to perform doping and coating in stages, which can achieve uniform doping of doping elements in the ternary precursor and uniform coating of its surface, merge the precursor doping and coating processes, and achieve co-modification of the precursor by simple coprecipitation in the reactor, omit the equipment for secondary treatment of the precursor or positive electrode material particles in the conventional coating process, and do not need to take the precursor out of the coprecipitation reactor and transfer it to other devices for coating operations, simplifying the process flow, reducing costs, and being suitable for large-scale industrial production. Moreover, the precursor prepared by the method of the present invention has uniform particle size and good consistency, and the positive electrode material prepared by the method has high interface stability and less residual alkali, which helps to improve the electrochemical performance of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] Figure 1 3 is a scanning electron microscope image of the single crystal positive electrode material prepared in Example. DETAILED DESCRIPTION

[0059] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.

[0060] The specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0061] Example 1

[0062] This embodiment provides a doping-coating-coating-modified ternary precursor, the doping-coating-coating-modified ternary precursor comprising a core and a coating layer, the core being nickel-cobalt-manganese hydroxide containing a doping element M, M comprising Zr and Al, the molar percentage of the doping element M in the core being 0.35, and the molar ratio of Zr to Al being 2:1;

[0063] The coating layer contains fluoride and nickel-cobalt-manganese hydroxide, the fluoride is tungsten fluoride, the mass proportion of the fluoride in the coating layer is 60%, and the mass proportion of the nickel-cobalt-manganese hydroxide is 40%;

[0064] Based on the total mass of the ternary hydroxide in the doped, coated and co-modified ternary precursor, the content of tungsten fluoride is 0.1%.

[0065] This embodiment also provides a method for preparing the above-mentioned doping-coating-coated modified ternary precursor, comprising the following steps:

[0066] (1) A 100 g / L nickel-cobalt-manganese mixed salt solution (nickel, cobalt and manganese elements all come from sulfate, and the molar ratio of Ni, Co and Mn is 8:1:1), a 0.03 mol / L doping element salt solution (doping elements all come from sulfate), a 30% NaOH solution and a 20% ammonia solution were added to a reactor at a feed rate of 10 L / h, 1.5 L / h, 2 L / h and 1 L / h, respectively, for a coprecipitation reaction for 30 h. The parameters during the coprecipitation reaction were controlled as follows: the temperature was 55° C., the stirring speed was 300 r / min, the pH was controlled in the range of 10.0 to 12.0, and the feeding was stopped when the particle size D50 reached 5 μm;

[0067] (2) The doping element salt solution is replaced with a fluoride solution with a concentration of 15 g / L (feed rate is 3 L / h), and the nickel cobalt manganese salt solution, NaOH solution and ammonia solution are still introduced, and the following parameters are controlled: temperature is 55°C, stirring speed is 300 r / min, pH is controlled in the range of 11.0 to 12.0, and the coprecipitation reaction is continued for 2 hours to obtain a doped, coated and co-modified ternary precursor.

[0068] This embodiment also provides a single crystal positive electrode material, which is prepared using the above-mentioned precursor, and the preparation method thereof includes the following steps:

[0069] Lithium carbonate and the above-mentioned ternary precursor are mixed in a molar ratio of 1.05:1 (mixing speed is 800r / min, mixing time is 10min), and high-temperature sintering is performed in an oxygen atmosphere at a sintering temperature of 850°C and a sintering time of 18h. After naturally cooling to room temperature, a single crystal positive electrode material can be obtained.

[0070] Figure 1 From the scanning electron microscope (SEM) image of the single crystal positive electrode material prepared in this embodiment, it can be seen that it has uniform size, high crystallinity and good monodispersity.

[0071] Example 2

[0072] This embodiment provides a doping-coating co-modified precursor, the doping-coating co-modified precursor comprising a core and a coating layer, the core being nickel-cobalt-manganese hydroxide containing a doping element M, M comprising Zr and W, the molar percentage of the doping element M in the core being 0.25, and the molar ratio of Zr to W being 1:1;

[0073] The coating layer contains fluoride and nickel-cobalt-manganese hydroxide, the fluoride is tungsten fluoride, the mass proportion of the fluoride in the coating layer is 70%, and the mass proportion of the nickel-cobalt-manganese hydroxide is 30%;

[0074] Based on the total mass of the ternary hydroxide in the doping, coating and co-modified precursor, the content of tungsten fluoride is 0.2%.

[0075] This embodiment also provides a method for preparing the above-mentioned doping-coating-coated co-modified precursor, comprising the following steps:

[0076] (1) A nickel-cobalt-manganese mixed salt solution with a concentration of 80 g / L (nickel, cobalt and manganese elements all come from sulfate, and the molar ratio of Ni, Co and Mn is 8:1:1), a doping element salt solution with a concentration of 0.05 mol / L (the doping elements all come from sulfate), a NaOH solution with a mass concentration of 45% and an ammonia solution with a mass concentration of 10% were added to a reactor at a feed rate of 8 L / h, 1.0 L / h, 3 L / h and 3 L / h, respectively, for a coprecipitation reaction for 40 hours. The parameters during the coprecipitation reaction were controlled as follows: the temperature was 60° C., the stirring speed was 500 r / min, the pH was controlled in the range of 10.0 to 11.0, and the feeding was stopped when the particle size D50 reached 4 μm;

[0077] (2) The doping element salt solution is replaced with a fluoride solution with a concentration of 18 g / L (feed rate is 2.8 L / h), and the nickel cobalt manganese salt solution, NaOH solution and ammonia solution are still introduced, and the following parameters are controlled: temperature is 60°C, stirring speed is 500 r / min, pH is controlled in the range of 10.0 to 11.0, and the coprecipitation reaction is continued for 1 hour to obtain a doped, coated and co-modified precursor.

[0078] This embodiment also provides a single crystal positive electrode material, which is prepared using the above-mentioned precursor, and the preparation method thereof includes the following steps:

[0079] Lithium chloride and the above-mentioned ternary precursor are mixed in a molar ratio of 1.03:1 (mixing speed is 1000r / min, mixing time is 20min), and high-temperature sintering is performed in an oxygen atmosphere at a sintering temperature of 900°C and a sintering time of 12h. After naturally cooling to room temperature, a single crystal positive electrode material can be obtained.

[0080] Example 3

[0081] This embodiment provides a doping-coating-coating-modified ternary precursor, the doping-coating-coating-modified ternary precursor comprising a core and a coating layer, the core being nickel-cobalt-manganese hydroxide containing a doping element M, M comprising Zr, Al and La, the molar percentage of the doping element M in the core being 0.3, and the molar ratio of Zr, Al and La being 3:1:1;

[0082] The coating layer contains fluoride and nickel-cobalt-manganese hydroxide, the fluoride is tungsten fluoride and aluminum fluoride, the mass ratio of tungsten fluoride to aluminum fluoride is 1:1, the mass proportion of fluoride in the coating layer is 80%, and the mass proportion of nickel-cobalt-manganese hydroxide is 20%;

[0083] Based on the total mass of the ternary hydroxide in the doped, coated and co-modified ternary precursor, the content of tungsten fluoride is 0.3%.

[0084] This embodiment also provides a method for preparing the above-mentioned doping-coating-coated modified ternary precursor, comprising the following steps:

[0085] (1) A 120 g / L nickel-cobalt-manganese mixed salt solution (nickel, cobalt and manganese elements all come from sulfate, and the molar ratio of Ni, Co and Mn is 8:1:1), a 0.02 mol / L doping element salt solution (doping elements all come from sulfate), a 20% NaOH solution and a 20% ammonia solution were added to a reactor at a feed rate of 9 L / h, 2 L / h, 3 L / h and 2 L / h, respectively, for a coprecipitation reaction for 30 h. The parameters during the coprecipitation reaction were controlled as follows: the temperature was 58° C., the stirring speed was 200 r / min, the pH was controlled in the range of 10.5 to 11.5, and the feeding was stopped when the particle size D50 reached 2 μm;

[0086] (2) The doping element salt solution is replaced with a fluoride solution with a concentration of 12 g / L (feed rate is 3.2 L / h), and the nickel cobalt manganese salt solution, NaOH solution and ammonia solution are still introduced, and the following parameters are controlled: temperature is 55°C, stirring speed is 300 r / min, pH is controlled in the range of 10.5 to 11.5, and the coprecipitation reaction is continued for 3 hours to obtain a doped, coated and co-modified ternary precursor.

[0087] This embodiment also provides a single crystal positive electrode material, which is prepared using the above-mentioned precursor, and the preparation method thereof includes the following steps:

[0088] Lithium carbonate and the above-mentioned ternary precursor are mixed in a molar ratio of 1.04:1 (mixing speed is 600r / min, mixing time is 20min), and high-temperature sintering is performed in an oxygen atmosphere at a sintering temperature of 800°C and a sintering time of 22h. After naturally cooling to room temperature, a single crystal positive electrode material can be obtained.

[0089] Example 4

[0090] The difference between this embodiment and embodiment 1 is that the molar percentage of the doping element M in the core is 0.02.

[0091] Example 5

[0092] The difference between this embodiment and embodiment 1 is that the molar percentage of the doping element M in the core is 0.6.

[0093] Example 6

[0094] The difference between this embodiment and embodiment 1 is that, based on the total mass of the ternary hydroxide in the doping-coating-coated co-modified ternary precursor, the content of the tungsten fluoride is 0.4%.

[0095] Example 7

[0096] The difference between this embodiment and embodiment 1 is that the fluorides are tungsten fluoride and cobalt fluoride, and based on the total mass of the ternary hydroxide in the doped, coated and co-modified ternary precursor, the contents of tungsten fluoride and cobalt fluoride are both 0.05%.

[0097] Comparative Example 1

[0098] The difference between this comparative example and Example 1 is that tungsten fluoride is replaced by aluminum fluoride.

[0099] Comparative Example 2

[0100] The difference between this comparative example and Example 1 is that the doping element is Zr, and the total content of the doping element is the same as that in Example 1.

[0101] Comparative Example 3

[0102] The difference between this comparative example and Example 1 is that the doping element is Al, and the total content of the doping element is the same as that in Example 1.

[0103] Comparative Example 4

[0104] The difference between this comparative example and Example 1 is that the mass proportion of fluoride in the coating layer is 40%, and the mass proportion of nickel-cobalt-manganese hydroxide is 60%.

[0105] Battery Assembly:

[0106] The ternary precursors prepared in the above embodiments and comparative examples and lithium salt lithium hydroxide were mixed and ground in a mortar at a molar ratio of 1:1.04 for 40 minutes. In an oxygen atmosphere, the temperature was raised from room temperature to 850°C at a heating rate of 5°C / min. After calcination and heat preservation at this temperature for 16 hours, the temperature was naturally cooled to room temperature to obtain the corresponding ternary positive electrode material.

[0107] The above positive electrode material, conductive carbon black SP (purchased from TIMCAL), and polyvinylidene fluoride PVDF (brand HSV900) were mixed in a mass ratio of 90:5:5, and the solvent was N-methylpyrrolidone. The slurry was evenly coated on the aluminum foil with a scraper with a coating gap of 100μm. After coating, it was first dried at 120℃, then rolled, and finally the dried electrode was cut into Φ12 circular electrode sheets. After vacuum drying at 120℃, the electrode sheet was weighed to obtain the button half-cell positive electrode sheet.

[0108] The negative electrode is made of Φ14 lithium metal sheet.

[0109] The separator is a Φ19 PP microporous membrane (Celgard2400).

[0110] The electrolyte used was a lithium battery basic electrolyte, which was a mixed solvent of EC and DEC in a 1:1 volume ratio, and 1.1 mol / L LiPF6 was added.

[0111] The positive electrode sheet, the metal lithium sheet, the separator and the electrolyte are assembled to obtain a button battery.

[0112] The above-provided lithium-ion battery was subjected to a performance test under the constant current charge and discharge mode and a voltage range of 2.5 to 4.5V.

[0113] Discharge capacity test: Charge at 0.1C until 4.3V is terminated;

[0114] Rate performance test: Charge and discharge cycle tests were carried out at 0.1C, 0.2C, 0.5C, 1C, 2C and 5C respectively. After 5 cycles at each rate, the battery returned to the 0.1C rate and the capacity retention rate was calculated based on the capacity loss to compare the rate performance.

[0115] Cyclic performance test: The charge and discharge test was carried out at 1C, and the material capacity after 50 cycles was statistically analyzed to obtain the cycle capacity retention rate. The constant current was charged at room temperature and discharged at room temperature 25°C and 55°C. The results are shown in Table 1.

[0116] Table 1

[0117]

[0118] As can be seen from Table 1, the present invention uses at least two of Zr, Al, Ti and La to dope the ternary hydroxide, and uses fluoride containing tungsten fluoride and the ternary hydroxide for synergistic coating, which can improve the doping and coating effects of the precursor in the subsequent preparation of the positive electrode material, improve the kinetic performance and structural stability, and improve the discharge capacity, cycle performance and rate performance of the positive electrode material.

[0119] At the same time, through the comparison between Example 1 and Examples 4-5, it can be seen that in the preparation process of the doped coated co-modified ternary positive electrode material described in the present invention, the doping amount of the M element will affect its performance. If the doping amount of the M element is too low, the structural collapse of the material cannot be effectively suppressed, and the structural stability of the material decreases; if the doping amount of the M element is too high, it will affect the energy density of the positive electrode material, because the dopant is a non-electrochemically active substance and does not participate in the electrochemical process, which will also cause the performance of the material to be significantly reduced.

[0120] By comparing Example 1 with Example 6, it can be seen that in the preparation process of the doped and coated co-modified ternary positive electrode material described in the present invention, the coating amount of tungsten fluoride will affect its performance. When the coating amount is too high, the thicker coating layer may be not conducive to the storage of lithium and will affect the electrochemical properties of the material.

[0121] By comparing Example 1 with Comparative Example 1, it can be seen that in the preparation process of the doped coated co-modified ternary positive electrode material described in the present invention, the performance effect of using tungsten fluoride as a coating layer is better than that of aluminum fluoride. When tungsten fluoride is used as a coating layer, it can simultaneously affect the interior and interface of the material. The tungsten element can regulate the growth morphology of the primary particles, causing them to develop into an elongated shape, and can maintain the stability of the internal structure together with the doping element. When aluminum fluoride is used as a coating layer, the aluminum element does not enter the interior of the material structure, but forms a film on the surface of the particles, and the stability of the material cannot be significantly improved.

[0122] By comparing Example 1 with Comparative Examples 2-3, it can be seen that in the preparation process of the doped and coated co-modified ternary positive electrode material described in the present invention, the performance effect of dual-element doping is better than that of doping with a single element. When the dual elements are co-doped, a synergistic effect will be produced, thereby improving the performance of the ternary positive electrode material.

[0123] By comparing Example 1 with Comparative Example 4, it can be seen that when fluoride is not the main component in the coating layer, it will affect the electrochemical properties of the material. The fluoride content is too low to achieve effective coating and cannot resist the penetration of electrolyte. The dissolution of transition metals leads to reduced stability.

[0124] The applicant declares that the present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A doping, coating and co-modified precursor, characterized in that: The doping-coating-coated co-modified precursor includes a core and a coating layer, the core is a ternary hydroxide containing a doping element M, M includes at least two of Zr, Al, Ti and La, the coating layer contains fluoride and ternary hydroxide, the mass proportion of the fluoride in the coating layer is greater than 50%, and the fluoride includes tungsten fluoride.

2. The doping-coating-coated co-modified precursor according to claim 1, characterized in that: The ternary hydroxide is nickel-cobalt-manganese hydroxide; Preferably, the molar percentage of the doping element M in the core is 0.05 to 0.4; Preferably, the fluoride further comprises at least one of aluminum fluoride, cobalt fluoride, magnesium fluoride and sodium fluoride; Preferably, based on the total mass of the ternary hydroxide in the doping-coating-coated co-modified precursor, the content of the fluoride is 0.01-1%; Preferably, based on the total mass of the ternary hydroxide in the doping-coating-coated co-modified precursor, the content of the tungsten fluoride is 0.01-0.3%.

3. A method for preparing a doping-coating-coated co-modified precursor as claimed in claim 1 or 2, characterized in that: The preparation method comprises the following steps: (1) adding a ternary mixed salt solution, a doping element salt solution, a precipitant solution and a complexing agent solution into a reactor for coprecipitation reaction, and stopping feeding when the particle size reaches a preset particle size of the inner core; (2) The doping element salt solution is replaced with a fluoride solution, and the coprecipitation reaction is continued to obtain a doping, coating and co-modified precursor.

4. The preparation method according to claim 3, characterized in that: The concentration of the ternary mixed salt solution in step (1) is 80-120 g / L; Preferably, the feed rate of the ternary mixed salt solution in step (1) is 8 to 10 L / h; Preferably, the concentration of the doping element salt solution in step (1) is 0.01 to 0.05 mol / L; Preferably, the feeding rate of the doping element salt solution in step (1) is 1 to 2 L / h; Preferably, the mass concentration of the precipitant solution in step (1) is 20-50%; Preferably, the feed rate of the precipitant solution in step (1) is 1.5 to 3 L / h; Preferably, the mass concentration of the complexing agent solution in step (1) is 10-30%; Preferably, the feeding rate of the complexing agent solution in step (1) is 0.5 to 3 L / h.

5. The preparation method according to claim 3 or 4, characterized in that: The coprecipitation reaction time in step (1) is 24 to 48 hours; Preferably, the coprecipitation reaction in step (1) is accompanied by stirring, and the stirring speed is 100 to 500 r / min; Preferably, the temperature of the coprecipitation reaction in step (1) is controlled within the range of 55 to 60°C; Preferably, the pH of the coprecipitation reaction in step (1) is controlled within the range of 10.0 to 12.

0.

6. The preparation method according to any one of claims 3 to 5, characterized in that: The concentration of the fluoride solution in step (2) is 10 to 20 g / L; Preferably, the feeding rate of the fluoride solution in step (2) is 2 to 4 L / h; Preferably, the coprecipitation reaction time in step (2) is 0.5 to 3 hours; Preferably, the coprecipitation reaction in step (2) is continued with stirring, and the stirring speed is 100 to 500 r / min; Preferably, the temperature of the continued coprecipitation reaction in step (2) is controlled within the range of 55 to 60°C; Preferably, the pH of the continued coprecipitation reaction in step (2) is controlled within the range of 10.0 to 12.

0.

7. A positive electrode material, characterized in that: The positive electrode material is prepared by the doping, coating and co-modified precursor according to claim 1 or 2; Preferably, the positive electrode material is a high-nickel single crystal positive electrode material, wherein the molar content of nickel is greater than or equal to 0.

6.

8. A method for preparing a positive electrode material as claimed in claim 7, characterized in that: The preparation method comprises the following steps: The doped, coated and co-modified precursor is mixed with lithium salt and sintered to obtain the positive electrode material.

9. The method for preparing the positive electrode material according to claim 8, characterized in that: The molar ratio of the lithium salt to the doping-coating-coated co-modified precursor is (1.03-1.06):1; Preferably, the mixing speed is 500-1100 r / min, and the mixing time is 5-20 min; Preferably, the sintering atmosphere is an oxygen-containing atmosphere; Preferably, the sintering temperature is 800-900° C., and the sintering time is 12-22 hours.

10. A battery, characterized in that: The battery comprises the positive electrode material according to claim 7.