Method for adsorbing and recycling precious metals in water-based sample

Through the combination adsorbent of microalgae-mycelium balls without chemical pretreatment, the problems of high preparation costs and difficult solid-liquid separation in the prior art are solved, and high-efficiency and low-consumption gold ion adsorption and separation are achieved, which is suitable for large-scale production application.

CN118993350AActive Publication Date: 2024-11-22TSINGHUA UNIVERSITY
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411147601.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-22
Estimated Expiration
2044-08-20

AI Technical Summary

Technical Problem

Existing bioadsorbents require chemical pretreatment and modification and curing when recycling precious metals in water, resulting in high preparation costs, complex processes and difficult to produce and apply on a large scale. At the same time, the solid-liquid separation cost of microbial cells or nanoscale adsorbent materials is high and High energy consumption.

Method used

Using a combination of microalgae-mycelium sphere adsorbent without chemical pretreatment and modification, the secretion of extracellular polymers under the stimulation of gold ions by fungal and microalgae cell surface functional groups to achieve in situ flocculation of microalgae cells and Mycelium spheres combine to form large granular algae symbionts, and the adsorption and flocculation process are carried out simultaneously, reducing preparation time and cost.

Benefits of technology

It improves the adsorption performance and separation efficiency of gold ions, achieves fast and low-consumption solid-liquid separation, reduces the cost of large-scale production applications, and eliminates the need for additional time and space to preserve algae symbiotic particles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993350A_ABST
    Figure CN118993350A_ABST
Patent Text Reader

Abstract

The invention discloses a method for adsorbing and recovering precious metals in a water-based sample. The invention provides a method for adsorbing and recovering precious metals in a water-based sample, which comprises the following steps: adding an adsorbent into the water-based sample, the adsorbent comprising microalgae and mycelium pellets; adsorbing the precious metal in the water-based sample, wherein the adsorbent is adopted to adsorb the precious metal in the water-based sample and flocculate the microalgae cells synchronously. The technical problems that the use cost is high, secondary pollution is serious and solid-liquid separation of tiny biological cells or crushed and ground micron-scale and nano-scale adsorption materials is difficult due to the fact that biological adsorbents often need chemical pretreatment, modification and solidification are solved, and the technical scheme is provided for shortening the preparation time of the adsorbents, saving the occupied area and reducing the production cost. Adsorption and flocculation processes are performed synchronously, and rapid selective adsorption of gold ions and synchronous, efficient and low-consumption separation of microalgae cells are realized by using a simple biological mixed system of mycelium pellets and microalgae combination.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of wastewater treatment, and relates to a method for adsorbing and recovering precious metals in an aqueous sample, and in particular to a method for utilizing mycelium balls to fix microalgae for synchronous adsorption, removal and recovery of precious metal ions in wastewater. Background Art

[0002] Gold (Au), as an important precious metal, is widely used in electroplating, electronics, catalysis and other industrial fields. With the increasing demand for gold in the industrial field and the limited sources of gold in natural ores, the discharge of wastewater containing gold ions has become a major threat to the environment and resource sustainability. Therefore, it is of great significance to recover gold from secondary resources. At present, a large number of technologies have been developed to enrich and extract gold ions from wastewater, such as chemical deposition, solvent extraction, membrane separation, ion exchange, electrodialysis and adsorption. In particular, the adsorption method has a significant effect on the recovery of gold ions in low-concentration wastewater. The gold ions are first adsorbed by the adsorbent, and then the loaded gold ions are stripped off during the desorption process and concentrated in a smaller desorption solution to improve energy efficiency and reduce the operating cost of the next stage of electrolysis.

[0003] The adsorption method mainly uses activated carbon, clay minerals, silica gel materials, nano zero-valent iron, natural polymer materials, etc. to prepare adsorbents, and then adsorb precious metal ions in water. However, there are also some problems. For example, although activated carbon has high adsorption efficiency for heavy metals, it has high cost of use, difficulty in regeneration, and cannot be reused; although clay minerals are widely present in nature, the effect of removing heavy metals is poor; although nano zero-valent iron and metal organic frameworks have high removal efficiency for heavy metals, they have poor stability and are greatly affected by the environment. The biological adsorption method has broad application prospects in the treatment and recovery of precious metal wastewater due to its advantages of low cost, high removal rate, easy regeneration, simple operation, and no secondary pollution. The most important biological adsorbents in the biological adsorption method have a wide range of sources, and common ones include fungi, bacteria, algae, and agricultural and forestry wastes. In particular, the surface of microbial cells such as algae, bacteria, and fungi have rich functional groups that can be used as binding sites for gold ions, which play an important role in the adsorption, removal, and recovery of precious metals from aqueous solutions.

[0004] At present, although there are many studies on the use of biosorbents to remove and recover precious metals in water, there are also some potential problems such as difficulty in solid-liquid separation, low mechanical strength, slow adsorption rate, and poor reusability. In particular, separating tiny cells such as algae, bacteria, and fungi or synthetic and modified nano- and micro-scale adsorbent materials from dilute solutions is still a huge challenge, especially for their large-scale application, traditional separation methods such as centrifugation, filtration, flotation, and chemical flocculation are too costly and energy-intensive.

[0005] In the prior art, the sources of biosorbents used to adsorb and recover gold ions in wastewater are mainly bacteria and agricultural and forestry wastes. Reference 1 uses a manganese oxide-producing bacterium Lysinibaeillus sp.M14 to adsorb trivalent gold ions in water. Its adsorption capacity is only 21 mg / g within 1 hour at room temperature and pressure, and it is difficult to separate the bacterial cells into solid and liquid. Reference 2 uses modified mangosteen residue (particles below 40 mesh) to adsorb gold ions in wastewater. Its adsorption capacity is 100 mg / g within 24 hours at room temperature and pressure, and the energy consumption of solid-liquid separation of micron-sized particles is large. Reference 3 uses acid pretreatment of poultry eggshells-protein hydrolysis-modification and solidification to form a water-soluble adsorption material to adsorb gold ions in wastewater. The maximum adsorption capacity of ions is 628 mg / g, but the required temperature is relatively high at 55°C; Reference 4 uses mycelial balls to flocculate microalgae cells to form algae-bacteria symbiotic particles, and then uses these preformed algae-bacteria symbiotic particles as adsorbents to adsorb gold ions in wastewater. The maximum adsorption capacities within 6 hours at room temperature and pressure are 104 mg / g (active algae-bacteria symbiotic particles) and 112 mg / g (freeze-dried algae-bacteria symbiotic particles), respectively. However, additional time and space are required to prepare and preserve the algae-bacteria symbiotic particles, which is not conducive to their large-scale production and application.

[0006] Therefore, there is an urgent need to develop an economical and efficient biosorption method with high affinity for gold ions, good sedimentation performance, and easy separation from wastewater.

[0007] Citations

[0008] Reference 1: CN103421702A

[0009] Reference 2: CN102534211A

[0010] Reference 3: CN103191701A

[0011] Reference 4: Na Shen and Evans MNChirwa, 2020. Live and lyophilizedfungi-algae pellets as novel biosorbents for gold recovery: Critical parameters, isotherm, kinetics and regeneration studies, Bioresource Technology, 306, 123041. Summary of the invention

[0012] Problem that the invention aims to solve

[0013] Although the prior art, such as those cited in References 1 to 3, has attempted to recover precious metals from water bodies, as mentioned above, existing biosorbents often require chemical pretreatment, modification and solidification processes, which makes the adsorbent preparation cost high, the process complex, and the secondary pollution serious, which greatly limits the large-scale production and application of these adsorbent materials. In addition, separating tiny biological cells or crushed and ground micron and nano-scale adsorbent materials from the solution is still a huge challenge, especially for its large-scale application, traditional separation methods such as centrifugation, filtration, flotation and chemical flocculation are too expensive and energy-intensive. Although the method of preparing microalgae and mycelial balls into algae-bacteria symbiotic particles in advance (i.e., preformed algae-bacteria symbiotic particles) in Reference 4 shows a certain potential for gold ion adsorption, its adsorption performance needs to be improved, and this method of separating the flocculation and adsorption processes requires additional time and space to prepare and preserve the algae-bacteria symbiotic particles, which is not conducive to its large-scale production and application.

[0014] In order to overcome the above-mentioned problems of the prior art, the present invention provides a method for recovering gold ions from wastewater by combining microalgae and mycelium balls without any chemical pretreatment and modification and curing treatment, and synchronously flocculating microalgae. The method utilizes the rich functional groups on the surface of fungi and microalgae cells and the fact that both secrete more extracellular polymers under the stimulation of gold ions, which not only improves the adsorption performance of microalgae and fungi for gold ions, but also allows microalgae cells to be quickly fixed on mycelium balls to form stable algae-bacteria symbiotic particles with larger particle size in situ, thus achieving efficient, low-cost and rapid solid-liquid separation. Compared with preformed algae-bacteria symbiotic particles and microalgae or fungi adsorbing gold ions alone, the method for in-situ formation of algae-bacteria symbiotic particles provided by the present invention not only improves the adsorption performance of gold ions, but also combines the adsorption and flocculation processes, and does not require additional time and space to prepare and preserve algae-bacteria symbiotic particles, shortening the preparation time of the adsorbent, saving floor space, and reducing its large-scale production and application costs.

[0015] Solutions for solving problems

[0016] [1]. A method for recovering precious metals from an aqueous sample by adsorption, wherein the method comprises:

[0017] The step of adding an adsorbent to the aqueous sample, wherein the adsorbent comprises microalgae and mycelium pellets, and before the adsorbent is added to the aqueous sample, the microalgae and mycelium pellets in the adsorbent do not flocculate and do not form symbiotic particles;

[0018] a step of adsorbing precious metals in an aqueous sample, using the adsorbent to adsorb precious metals in the aqueous sample;

[0019] Preferably, the precious metal includes gold, cobalt and nickel; more preferably, the precious metal is gold;

[0020] Preferably, in the step of adsorbing precious metals in the aqueous sample, while the adsorbent adsorbs the precious metals in the aqueous sample, the microalgae and mycelial balls in the adsorbent flocculate to form symbiotic particles.

[0021] [2] The method according to [1], wherein before the step of adding the adsorbent to the aqueous sample, it also includes a step of adjusting the pH, wherein the pH value of the aqueous sample is adjusted to 2 to 5, preferably 2 to 4.

[0022] [3] The method according to [1] or [2], wherein the mass ratio of the mycelial pellet to the microalgae is 1:1 to 10, preferably 1:1 to 5, based on dry weight.

[0023] [4] The method according to any one of [1] to [3], wherein the particle size of the mycelial pellet is 5 to 15 mm, preferably 8 to 12 mm;

[0024] Optionally, the mycelial pellet is an active mycelial pellet or a freeze-dried mycelial pellet.

[0025] [5] The method according to any one of [1] to [4], wherein the microalgae is in the form of a suspension;

[0026] Preferably, the absorbance of the microalgae suspension at 680 nm is 0.5 to 2, preferably 0.8 to 1.5.

[0027] [6] The method according to any one of [1] to [5], wherein the mycelial pellet is a mycelial pellet formed from fungi or bacteria;

[0028] Optionally, the fungus is selected from at least one of filamentous fungi and yeast;

[0029] Optionally, the bacteria are selected from at least one of actinomycetes, iron bacteria and sulfur bacteria;

[0030] Preferably, the fungus is selected from at least one of Aspergillus niger, Aspergillus oryzae, Rhizopus oryzae, Cladosporium cladosporoides and Aspergillus nidulans;

[0031] More preferably, the fungus comprises Aspergillus niger;

[0032] and / or,

[0033] The microalgae is selected from at least one of freshwater microalgae, red algae and brown algae;

[0034] Preferably, the microalgae is selected from at least one of Tetradesmus obliquus, Chlorella vulgaris, Chlorococcum ellipsoideum, and Phaeodactylum tricornutum; more preferably, the microalgae includes Tetradesmus obliquus.

[0035] [7] The method according to any one of [1] to [6], wherein the aqueous sample is a water sample;

[0036] Optionally, the water sample is selected from at least one of water samples from a water environment, industrial wastewater, mining and mineral processing wastewater, domestic water, solid digestion solution and eluent.

[0037] [8] The method according to any one of [1] to [7], wherein after the step of adsorbing the precious metal in the aqueous sample, it also includes a step of recovering the precious metal, wherein:

[0038] A desorption liquid is added to the adsorbent obtained in the step of adsorbing the precious metals in the aqueous sample to desorb the precious metals from the adsorbent.

[0039] [9]. An adsorbent, wherein the adsorbent comprises microalgae and mycelial pellets;

[0040] Optionally, based on dry weight, the mass ratio of the mycelial pellet to the microalgae is 1:1 to 10, preferably 1:1 to 5;

[0041] Optionally, the particle size of the mycelium pellet is 5 to 15 mm, preferably 8 to 12 mm;

[0042] Optionally, the mycelial pellet is an active mycelial pellet or a freeze-dried mycelial pellet;

[0043] Optionally, the microalgae is in the form of a suspension; preferably, the absorbance of the microalgae suspension at 680 nm is 0.5 to 2, preferably 0.8 to 1.5;

[0044] Preferably, before using the adsorbent, the microalgae and mycelial balls in the adsorbent have not been flocculated and have not formed symbiotic particles.

[0045]

[10] The adsorbent according to [9], wherein the mycelial pellet is a mycelial pellet formed from fungi or bacteria;

[0046] Optionally, the fungus is selected from at least one of filamentous fungi and yeast;

[0047] Optionally, the bacteria are selected from at least one of actinomycetes, iron bacteria and sulfur bacteria;

[0048] Preferably, the fungus is selected from at least one of Aspergillus niger, Aspergillus oryzae, Rhizopus oryzae, Cladosporium cladosporoides and Aspergillus nidulans;

[0049] More preferably, the fungus comprises Aspergillus niger;

[0050] and / or,

[0051] The microalgae is selected from at least one of freshwater microalgae, red algae and brown algae;

[0052] Preferably, the microalgae is selected from at least one of Tetradesmus obliquus, Chlorella vulgaris, Chlorococcum ellipsoideum, and Phaeodactylum tricornutum;

[0053] More preferably, the microalgae comprises Tetradesmus obliquus.

[0054]

[11] . A device for adsorbing and recovering precious metals in an aqueous sample, wherein the device comprises the adsorbent as described in [9] or

[10] ;

[0055] Preferably, the precious metals include gold, cobalt and nickel;

[0056] More preferably, the precious metal is gold.

[0057]

[12] Use of the adsorbent described in [9] or

[10] for adsorbing and recovering precious metals in aqueous samples;

[0058] Preferably, the precious metals include gold, cobalt and nickel;

[0059] More preferably, the precious metal is gold.

[0060] Effects of the Invention

[0061] The present invention overcomes the technical problems that the biosorbent often needs chemical pretreatment and modification and solidification, resulting in high use cost and serious secondary pollution, as well as the difficulty in solid-liquid separation of tiny biological cells or micron and nano-scale adsorption materials after crushing and grinding. In order to shorten the preparation time of the adsorbent, save floor space, and reduce production costs, the adsorption and flocculation processes are carried out simultaneously, and the rapid selective adsorption of gold ions and the synchronous, efficient, and low-cost separation of microalgae cells are achieved through a simple biological mixed system of mycelium balls and microalgae. The rich functional groups on the surfaces of fungi and microalgae cells and the secretion of more extracellular polymers by both under the stimulation of gold ions not only improve the adsorption performance of gold ions, but also a large number of microalgae cells are captured by mycelium balls in situ flocculation, stably forming large-particle algae-bacteria symbionts of 9-10 mm, and no additional time and space are required to prepare and preserve algae-bacteria symbiotic particles, thereby reducing the cost of large-scale production and application, thereby realizing an economical and efficient bioadsorption method with high gold ion affinity, good sedimentation performance, and easy separation from wastewater. BRIEF DESCRIPTION OF THE DRAWINGS

[0062] Figure 1 Showing active fungal mycelium pellets ( Figure 1 A) and freeze-dried fungal mycelium pellets ( Figure 1 B) Schematic diagram of flocculation microalgae adsorption and recovery of gold ions in wastewater.

[0063] Figure 2 A time-concentration curve showing the flocculation efficiency of gold ions and microalgae in Example 1 of the present invention and Comparative Examples 1, 2, and 3. Figure 2 The upper middle part shows the microalgae-active Aspergillus niger particle combination; Figure 2 The bottom shows the combination of microalgae and freeze-dried Aspergillus niger particles)

[0064] Figure 3 The time-concentration curves of gold ions in Example 2 of the present invention and Comparative Examples 4 and 5 are shown.

[0065] Figure 4 A schematic diagram showing the recovery of gold ions from PCB wastewater by mycelial pellet-fixed microalgae in Example 4 of the present invention. DETAILED DESCRIPTION

[0066] Various exemplary embodiments, features and aspects of the present invention will be described in detail below. The word "exemplary" used here means "used as an example, embodiment or illustrative". Any embodiment described here as "exemplary" is not necessarily interpreted as being superior or better than other embodiments.

[0067] In addition, in order to better illustrate the present invention, numerous specific details are provided in the following specific embodiments. It should be understood by those skilled in the art that the present invention can be implemented without certain specific details. In other examples, methods, means, equipment and steps well known to those skilled in the art are not described in detail in order to highlight the subject matter of the present invention.

[0068] Unless otherwise stated, the units used in this specification are all international standard units, and the numerical values ​​and numerical ranges appearing in the present invention should be understood to include the inevitable systematic errors in industrial production.

[0069] In this specification, the word "may" includes both performing a certain process and not performing a certain process.

[0070] In this specification, the references to "some specific / preferred embodiments", "other specific / preferred embodiments", "embodiments", etc., mean that the specific elements (e.g., features, structures, properties and / or characteristics) described in connection with the embodiments are included in at least one embodiment described herein, and may or may not exist in other embodiments. In addition, it should be understood that the elements may be combined in various embodiments in any suitable manner.

[0071] In this specification, the numerical range expressed using "a numerical value A to a numerical value B" means a range including the endpoints numerical values ​​A and B.

[0072] In this specification, when "normal temperature" or "room temperature" is used, the temperature may be about 15-30°C. DETAILED DESCRIPTION OF THE INVENTION

[0074]

[0075] In some aspects of the present invention, a method for recovering precious metals in an aqueous sample by adsorption is provided, wherein the method comprises:

[0076] The step of adding an adsorbent to the aqueous sample, wherein the adsorbent comprises microalgae and mycelium pellets, and before the adsorbent is added to the aqueous sample, the microalgae and mycelium pellets in the adsorbent do not flocculate and do not form symbiotic particles;

[0077] The step of adsorbing precious metals in the aqueous sample comprises using the adsorbent to adsorb the precious metals in the aqueous sample.

[0078] In some preferred embodiments, in the step of adsorbing precious metals in the aqueous sample, while the adsorbent adsorbs the precious metals in the aqueous sample, the microalgae and mycelial balls in the adsorbent flocculate to form symbiotic particles.

[0079] Compared with the existing method of preparing microalgae and mycelial balls into algae-fungus symbiotic particles in advance, the method of the present invention for adsorbing precious metals and simultaneously flocculating microalgae cells not only improves the adsorption performance of precious metals, but also combines the adsorption and flocculation processes. It does not require additional time and space to prepare and preserve the algae-fungus symbiotic particles, and is more advantageous in its large-scale production and application.

[0080] Procedure for adding sorbent to aqueous samples

[0081] (Mycelium ball)

[0082] In the present invention, there is no particular limitation on the source of the mycelial pellets, and for example, the source may be a fungus or a bacterium that can form mycelial pellets when cultured in a liquid medium with aeration, stirring or shaking.

[0083] In some embodiments, the fungus may be selected from at least one of filamentous fungi and yeast.

[0084] In some preferred embodiments, the fungus is selected from at least one of Aspergillus niger, Aspergillus oryzae, Rhizopus oryzae, Cladosporium cladosporoides and Aspergillus nidulans.

[0085] In some more preferred embodiments, the fungus comprises Aspergillus niger. Aspergillus niger can be purchased commercially, for example, from the China Industrial Microbiological Culture Collection Administration Center, exemplarily, the strain number is CICC 2487.

[0086] In other embodiments, the bacteria are selected from at least one of actinomycetes, iron bacteria, and sulfur bacteria.

[0087] In the present invention, fungal mycelium balls, also called fungal particles, are a special fermentation form of fungi (such as filamentous fungi), that is, under the conditions of sufficient oxygen and nutrients, low viscosity of the culture medium, and appropriate directional shear hydraulic strength, the germinated filamentous fungal spores form mycelium, which are entangled with each other to form a spherical mycelium aggregate with a dense surface and loose interior.

[0088] In some embodiments of the present invention, the particle size of the mycelial ball is 5 to 15 mm, preferably 8 to 12 mm, and more preferably 9 to 10 mm. At this particle size, when the precious metals (such as gold ions) in the aqueous sample are adsorbed and recovered, the algae-bacteria symbiotic particles formed in situ are easily separated from the wastewater and can be quickly settled to the bottom of the reactor within a few seconds, without the need for other high-energy separation methods such as centrifugation, filtration and flotation.

[0089] In some embodiments of the present invention, the mycelial pellet is an active mycelial pellet or a freeze-dried mycelial pellet. In some preferred embodiments, the mycelial pellet is an active mycelial pellet, and the adsorbent using the active mycelial pellet has higher adsorption efficiency and adsorption capacity than the adsorbent using the freeze-dried mycelial pellet.

[0090] (Microalgae)

[0091] In the present invention, there is no particular requirement for the selection of the microalgae, as long as the microalgae can be flocculated and captured by mycelial pellets (eg, fungal mycelial pellets, more specifically, filamentous fungal mycelial pellets).

[0092] In some embodiments, the microalgae is selected from at least one of freshwater microalgae, red algae, and brown algae.

[0093] In some preferred embodiments, the microalgae is selected from at least one of Tetradesmus obliquus, Chlorella vulgaris, Chlorococcumellipsoideum and Phaeodactylum tricornutum.

[0094] In some more preferred embodiments, the microalgae include Tetradesmus obliquus. Tetradesmus obliquus can be purchased commercially, for example, from the Freshwater Algae Seed Bank of the Chinese Academy of Sciences, and the exemplary algae species number is FACHB-12.

[0095] In some embodiments, the microalgae is in the form of a suspension. Exemplarily, the suspension is a suspension of microalgae in water. In some preferred embodiments, the absorbance of the microalgae suspension at 680 nm is 0.5 to 2, preferably 0.8 to 1.5, and more preferably 1.1 to 1.3. When the microalgae suspension is used in combination with mycelial balls as an adsorbent in the form of a suspension, especially at the above absorbance, the adsorption efficiency and adsorption capacity of the adsorbent for precious metals (such as gold ions) can be improved.

[0096] (Ratio of mycelium balls to microalgae)

[0097] In some embodiments, in the adsorbent, the mass ratio of the mycelial pellet to the microalgae, based on dry weight, is 1: 1 to 10, preferably 1: 1 to 5. Within the above mass ratio range, the adsorbent has better adsorption efficiency, adsorption capacity, etc.

[0098] (Precious Metals)

[0099] In some embodiments, the precious metal includes gold, cobalt and nickel. In some preferred embodiments, the precious metal is gold. As demonstrated in Example 4, in the method of the present invention, the adsorbent used has a strong selective adsorption capacity for gold.

[0100] (Aqueous samples)

[0101] The aqueous sample applicable to the present invention is not particularly limited, and can be an aqueous sample of any source and type. In some specific embodiments, the aqueous sample can be a water sample.

[0102] In some specific embodiments, the water sample can be industrial wastewater (such as printed circuit board wastewater in the embodiment), mining and mineral processing wastewater, domestic water (such as tap water, drinking water, drinking water, etc.), various solid digestion solutions, eluents, etc.

[0103] Steps for adsorption of precious metals from aqueous samples

[0104] In the present invention, in the step of adsorbing the precious metals in the aqueous sample, an adsorbent is used to adsorb the precious metals in the aqueous sample.

[0105] In some embodiments, the adsorption of precious metals in aqueous samples by adsorbents is performed at room temperature, preferably at 25±2° C. At this temperature, it is beneficial to improve the adsorption efficiency and adsorption capacity of the adsorbent for precious metals (such as gold ions).

[0106] In the present invention, there is no particular limitation on the container or equipment used when using an adsorbent to adsorb precious metals (such as gold ions) in an aqueous sample, as long as the adsorbent can be in full contact with the aqueous sample to facilitate the adsorption of the precious metals in the aqueous sample.

[0107] For example, in some specific embodiments, the step of adsorbing precious metals in the aqueous sample can be carried out in an orbital shaker, for example, at a rotation speed of 150 to 500 rpm, preferably 200 to 400 rpm. In other specific embodiments, the step of adsorbing precious metals in the aqueous sample can be carried out in a tower upflow reactor, and an air compressor is used at the bottom of the reactor for aeration.

[0108] The method for adsorbing and recovering precious metals in aqueous samples provided by the present invention has high adsorption efficiency, and therefore, the step of adsorbing precious metals in aqueous samples can be completed within 10 hours, preferably within 8 hours, and more preferably within 6 hours. As demonstrated in Example 3, using the method of the present invention, the adsorption rate of gold ions by the microalgae-active fungal particle combination within 3 hours reaches 98.8%.

[0109] Steps to adjust pH

[0110] In some embodiments, before the step of adding an adsorbent to the aqueous sample, a step of adjusting the pH is also included, wherein the initial pH value of the aqueous sample is adjusted to 2-5, preferably 2-4 (e.g., 2, 2.5, 3, 3.5, 4), more preferably 3.5±0.3.

[0111] At this pH value, the adsorption efficiency and adsorption capacity of the adsorbent for gold ions can be improved.

[0112] In the present invention, the initial pH value of the aqueous sample refers to the pH value of the aqueous sample before the adsorbent is added to the aqueous sample (eg, a solution containing gold ions).

[0113] In the present invention, there is no particular limitation on the acidic or alkaline reagent used to adjust the initial pH value of the aqueous sample, and acidic or alkaline regulators commonly used in the art can be used. In some specific embodiments, HCl and / or NaOH can be used.

[0114] Steps to recover precious metals

[0115] In the present invention, after the step of adsorbing the precious metals in the aqueous sample, the step of recovering the precious metals from the adsorbent may also be included. In the desorption process, the precious metal ions loaded on the adsorbent are stripped and released into a desorption solution with a smaller volume by using a desorbent (such as acid, alkali, complex, etc.) to reduce the cost and energy consumption of the subsequent recovery process (such as electrolysis). Electrolysis is one of the common methods for recovering elemental metals from a desorption solution containing precious metal ions. Under the action of direct current, gold ions migrate to the cathode and precipitate on the cathode. When the cathode precipitates gold and accumulates to a certain amount, the cathode is taken out and the elemental gold is recovered after washing. In some specific embodiments, thiourea, acid, alkali and chelating agent are added to the adsorbent (i.e., algae-bacteria symbiotic particles loaded with precious metals, such as gold ions) obtained in the step of adsorbing the precious metals in the aqueous sample as a desorption solution, so as to desorb the precious metals from the adsorbent.

[0116] In some specific embodiments, before the step of recovering precious metals, a step of washing the adsorbent is further included, specifically, the adsorbent is washed with deionized water.

[0117] In some preferred embodiments, the desorption liquid (thiourea) is an acidic desorption liquid, and its pH is below 3, preferably below 2, more preferably below 1, such as 0.7.

[0118] In some specific embodiments, the desorption time is within 3 hours, preferably within 2 hours, more preferably within 1 hour, for example, 30 minutes. As demonstrated in Example 4, 1M acidic thiourea (pH = 0.7) can strip 92.12% of gold ions from algae-bacteria symbiotic particles within 30 minutes. The thiourea desorption solution containing gold ions is placed in an electrolytic cell by electrolysis. Under the action of direct current, the gold ions migrate to the cathode and precipitate on the cathode. When the cathode precipitated gold accumulates to a certain amount, the cathode is taken out and washed to recover the elemental gold.

[0119] <Adsorbent>

[0120] In some aspects of the present invention, an adsorbent is provided, wherein the adsorbent comprises microalgae and mycelial pellets. Before using the adsorbent, the microalgae and mycelial pellets in the adsorbent do not flocculate and do not form symbiotic particles.

[0121] (Mycelium ball)

[0122] In the present invention, there is no particular limitation on the source of the mycelial pellets, and for example, the source may be a fungus or a bacterium that can form mycelial pellets when cultured in a liquid medium with aeration, stirring or shaking.

[0123] In some embodiments, the fungus may be selected from at least one of filamentous fungi and yeast.

[0124] In some preferred embodiments, the fungus is selected from at least one of Aspergillus niger, Aspergillus oryzae, Rhizopus oryzae, Cladosporium cladosporoides and Aspergillus nidulans.

[0125] In some more preferred embodiments, the fungus comprises Aspergillus niger. In other embodiments, the bacteria are selected from at least one of actinomycetes, iron bacteria and sulfur bacteria.

[0126] In some embodiments of the present invention, the particle size of the mycelial ball is 5 to 15 mm, preferably 8 to 12 mm, and more preferably 9 to 10 mm. At this particle size, when the precious metals (such as gold ions) in the aqueous sample are adsorbed and recovered, the algae-bacteria symbiotic particles formed in situ are easily separated from the wastewater and can be quickly settled to the bottom of the reactor within a few seconds, without the need for other high-energy separation methods such as centrifugation, filtration and flotation.

[0127] In some embodiments of the present invention, the mycelial pellet is an active mycelial pellet or a freeze-dried mycelial pellet. In some preferred embodiments, the mycelial pellet is an active mycelial pellet, and the adsorbent using the active mycelial pellet has higher adsorption efficiency and adsorption capacity than the adsorbent using the freeze-dried mycelial pellet.

[0128] (Microalgae)

[0129] In the present invention, there is no particular requirement for the selection of the microalgae, as long as the microalgae can be flocculated and captured by mycelial pellets (eg, fungal mycelial pellets, more specifically, filamentous fungal mycelial pellets).

[0130] In some embodiments, the microalgae is selected from at least one of freshwater microalgae, red algae, and brown algae.

[0131] In some preferred embodiments, the microalgae is selected from at least one of Tetradesmus obliquus, Chlorella vulgaris, Chlorococcumellipsoideum and Phaeodactylum tricornutum.

[0132] In some more preferred embodiments, the microalgae comprises Tetradesmus obliquus.

[0133] In some embodiments, the microalgae is in the form of a suspension. Exemplarily, the suspension is a suspension of microalgae in water. In some preferred embodiments, the absorbance of the microalgae suspension at 680 nm is 0.5 to 2, preferably 0.8 to 1.5, and more preferably 1.1 to 1.3. When the microalgae suspension is used in combination with mycelial balls as an adsorbent in the form of a suspension, especially at the above absorbance, the adsorption efficiency and adsorption capacity of the adsorbent for precious metals (such as gold ions) can be improved.

[0134] (Ratio of mycelium balls to microalgae)

[0135] In some embodiments, in the adsorbent, the mass ratio of the mycelial pellet to the microalgae, based on dry weight, is 1: 1 to 10, preferably 1: 1 to 5. Within the above mass ratio range, the adsorbent has better adsorption efficiency, adsorption capacity, etc.

[0136] <Device>

[0137] In some aspects of the present invention, a device for adsorbing and recovering precious metals in an aqueous sample is provided, wherein the device comprises an adsorbent as described in the above section <Adsorbent>.

[0138] In some embodiments, the precious metal includes gold, cobalt and nickel. In some preferred embodiments, the precious metal is gold.

[0139] <Purpose>

[0140] In some aspects of the present invention, the adsorbent as described in the above section <Adsorbent> is used to adsorb and recover precious metals in aqueous samples.

[0141] In some embodiments, the precious metal includes gold, cobalt and nickel. In some preferred embodiments, the precious metal is gold.

[0142] Example

[0143] The embodiments of the present invention will be described in detail below in conjunction with the examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If no specific conditions are specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0144] The experimental materials in the subsequent reference examples and embodiments are as follows:

[0145] Tetradesmus obliquus: provided by the School of Life Sciences and Technology, Shanghai Jiao Tong University. Tetradesmus obliquus can also be purchased from the Freshwater Algae Species Bank of the Chinese Academy of Sciences, for example, algae species number FACHB-12.

[0146] Aspergillus niger: provided by the Forestry and Agricultural Biotechnology Institute (FABI) of the University of Pretoria, South Africa. Aspergillus niger can also be purchased from the China Industrial Microbiological Culture Collection Administration Center, for example, strain number CICC2487.

[0147] The formula of BG-11 medium is shown in Table 1 below:

[0148] Table 1 BG-11 culture medium formula (1L)

[0149]

[0150] Potato dextrose agar (PDA): 200g potatoes, 20g glucose, 20g agar, 5g peptone, 3g potassium dihydrogen phosphate, 1.5g magnesium sulfate, 1000ml water.

[0151] Potato dextrose liquid medium (PDB): 200 g potatoes, 20 g glucose, 5 g peptone, 3 g potassium dihydrogen phosphate, 1.5 g magnesium sulfate, and 1000 ml water.

[0152] Thiourea: purchased from Merck.

[0153] Reference Example: The exemplary technical scheme of the method for adsorbing and recovering precious metals in aqueous samples provided by the present invention is as follows:

[0154] Microalgae culture: Freshwater microalgae Tetradesmus obliquus was used. To achieve faster growth, the pure strain was cultured in sterilized BG-11 medium with a pH of 7 at room temperature (25 ± 2 °C) and 60 μmol m -2 s -1 The culture was stirred under a light intensity of 1.5 and air aeration to provide CO 2 . After 7 days of growth, the algae strain was diluted to the corresponding concentration with sterile deionized water.

[0155] Formation of fungal mycelial balls: The filamentous fungus Aspergillus niger was used. The pure strain of Aspergillus niger was placed on a sterilized potato dextrose agar (PDA) plate and cultured at an angle in a 28°C incubator for 7 days for activation. When collecting spores, 10 mL of sterile water was added to the above PDA plate, and the fungal spore suspension was collected with a sterile syringe and then diluted to 50 mL with sterile water for use. The spore suspension was used as an inoculum to culture fungal particles, and the Aspergillus niger spore suspension was prepared with sterile water to an initial concentration of about 7.2 × 10 3 Spores / mL, the number of spores in the suspension was counted using an optical microscope, and the suspension was cultured in a potato dextrose liquid medium (PDB) at pH 4, and shaken in an orbital shaker at 28°C and 120 rpm. After 4 to 5 days of culture, mycelial balls with a particle size of 9 to 10 mm were formed, which were thoroughly rinsed with sterile deionized water and used as active fungal particles; the above active fungal particles were freeze-dried using a freeze dryer and stored under dry conditions at room temperature as freeze-dried fungal particles.

[0156] Adsorption and recovery of gold ions in wastewater by combination of microalgae and fungi particles: dilute the microalgae Tetradesmus obliquus suspension to an absorbance of 1.2 at 680nm, and add 35mg (by dry weight) of active or freeze-dried fungi particles with a particle size of 9-10mm to the microalgae suspension (the dry weight ratio of fungi to microalgae is 1:2). The algae liquid and active or freeze-dried fungi particles are respectively put into 100mL of HAuCl4 gold ion solution with an initial pH of 3.5 and an initial concentration of 100mg / L, and shaken at 250rpm in an orbital shaker for 6h at 25±2℃. The initial pH is adjusted by HCl and NaOH, as shown in FIG. Figure 1 shown.

[0157] Example 1

[0158] The initial concentration was 7.2×10 3 Spores / mL Aspergillus niger spore suspension was cultured in potato dextrose liquid medium (PDB) at pH 4 and shaken in an orbital shaker at 28°C and 120rpm. After 4-5 days of culture, fungal mycelium balls with a particle size of 9-10mm were formed. They were thoroughly rinsed with sterile deionized water, and one portion was used as active fungal particles for later use; another portion of active fungal particles was freeze-dried and stored in a freeze dryer and used as freeze-dried fungal particles for later use. The freshwater microalgae Tetradesmus obliquus concentrated by centrifugation was diluted with sterile deionized water to an absorbance of 1.2 at 680nm, and 2 portions of 100ml OD 680nm =1.2 The above algae liquid was centrifuged and concentrated and used as fresh algae liquid. Weigh 35 mg of dry weight, 9-10 mm active and freeze-dried Aspergillus niger particles, respectively, and then add the above microalgae-active Aspergillus niger particle combination and microalgae-freeze-dried Aspergillus niger particle combination to 100 mL of HAuCl4 solution with an initial pH of 3.5 and an initial concentration of 80 mg / L, respectively, and shake at 250 rpm in an orbital shaker at room temperature 25±2°C for 6 hours. Samples were taken at 60, 120, 180, 240, 300, and 360 minutes, and the samples were centrifuged at 8000 rpm for 5 minutes. The supernatant was taken and the gold ion concentration was determined by atomic absorption spectrometer. The results are as follows Figure 2 shown.

[0159] Comparative Example 1

[0160] Same as Example 1, except that the initial pH of the solution is 2. The initial concentration is 7.2×10 3Spores / mL Aspergillus niger spore suspension was cultured in potato dextrose liquid medium (PDB) at pH 4 and shaken in an orbital shaker at 28°C and 120rpm. After 4-5 days of culture, fungal mycelium balls with a particle size of 9-10mm were formed. They were thoroughly rinsed with sterile deionized water, and one portion was used as active fungal particles for later use; another portion of active fungal particles was freeze-dried and stored in a freeze dryer and used as freeze-dried fungal particles for later use. The freshwater microalgae Tetradesmus obliquus concentrated by centrifugation was diluted with sterile deionized water to an absorbance of 1.2 at 680nm, and 2 portions of 100ml OD 680nm =1.2 The above algae liquid was centrifuged and concentrated as fresh algae liquid for standby use. Weigh 35 mg of dry weight, 9-10 mm active and freeze-dried Aspergillus niger particles, respectively, and then add the above microalgae-active Aspergillus niger particle combination and microalgae-freeze-dried Aspergillus niger particle combination to 100 mL of HAuCl4 solution with an initial pH of 2 and an initial concentration of 80 mg / L, respectively, and shake at 250 rpm in an orbital shaker at room temperature of 25±2°C for 6 hours. Samples were taken at 60, 120, 180, 240, 300, and 360 minutes, and the samples were centrifuged at 8000 rpm for 5 minutes. The supernatant was taken and the gold ion concentration was determined by atomic absorption spectrometer. The results are as follows Figure 2 shown.

[0161] Comparative Example 2

[0162] Same as Example 1, except that the initial pH of the solution is 4. The initial concentration is 7.2×10 3 Spores / mL Aspergillus niger spore suspension was cultured in potato dextrose liquid medium (PDB) at pH 4 and shaken in an orbital shaker at 28°C and 120rpm. After 4-5 days of culture, fungal mycelium balls with a particle size of 9-10mm were formed. They were thoroughly rinsed with sterile deionized water, and one portion was used as active fungal particles for later use; another portion of active fungal particles was freeze-dried and stored in a freeze dryer and used as freeze-dried fungal particles for later use. The freshwater microalgae Tetradesmus obliquus concentrated by centrifugation was diluted with sterile deionized water to an absorbance of 1.2 at 680nm, and 2 portions of 100ml OD 680nm=1.2 The above algae liquid was centrifuged and concentrated as fresh algae liquid for standby use. Weigh 35 mg of dry weight, 9-10 mm active and freeze-dried Aspergillus niger particles, respectively, and then add the above microalgae-active Aspergillus niger particle combination and microalgae-freeze-dried Aspergillus niger particle combination to 100 mL of HAuCl4 solution with an initial pH of 4 and an initial concentration of 80 mg / L, respectively, and shake at 250 rpm in an orbital shaker at room temperature of 25±2°C for 6 hours. Samples were taken at 60, 120, 180, 240, 300, and 360 minutes, and the samples were centrifuged at 8000 rpm for 5 minutes. The supernatant was taken and the gold ion concentration was determined by atomic absorption spectrometer. The results are as follows Figure 2 shown.

[0163] Comparative Example 3

[0164] Same as Example 1, except that the initial pH of the solution is 5. The initial concentration is 7.2×10 3 Spores / mL Aspergillus niger spore suspension was cultured in potato dextrose liquid medium (PDB) at pH 4 and shaken in an orbital shaker at 28°C and 120rpm. After 4-5 days of culture, fungal mycelium balls with a particle size of 9-10mm were formed. They were thoroughly rinsed with sterile deionized water, and one portion was used as active fungal particles for later use; another portion of active fungal particles was freeze-dried and stored in a freeze dryer and used as freeze-dried fungal particles for later use. The freshwater microalgae Tetradesmus obliquus concentrated by centrifugation was diluted with sterile deionized water to an absorbance of 1.2 at 680nm, and 2 portions of 100ml OD 680nm =1.2 The above algae liquid was centrifuged and concentrated and used as fresh algae liquid. Weigh 35 mg of dry weight, active and freeze-dried Aspergillus niger particles with a particle size of 9-10 mm, respectively, and then add the above microalgae-active Aspergillus niger particle combination and microalgae-freeze-dried Aspergillus niger particle combination to 100 mL of HAuCl4 solution with an initial pH of 5 and an initial concentration of 80 mg / L, respectively, and shake at 250 rpm in an orbital shaker at room temperature of 25±2°C for 6 hours. Samples were taken at 60, 120, 180, 240, 300, and 360 minutes, and the samples were centrifuged at 8000 rpm for 5 minutes. The supernatant was taken and the gold ion concentration was determined by atomic absorption spectrometer. The results are as follows Figure 2 shown.

[0165] Experimental results: By comparing the results of Example 1 and Comparative Examples 1, 2, and 3, it can be seen that the coexistence of fungal mycelium balls and microalgae under appropriate pH conditions is very important for efficient adsorption of gold ions and flocculation of microalgae. The flocculation effect is best when the initial pH is 3.5, and the combination of microalgae-active Aspergillus niger particles is better than the combination of microalgae-freeze-dried Aspergillus niger particles. More than 95% of microalgae cells can be fixed on active mycelium balls within 3 hours (Example 1); when the initial pH is 2, only about 80% of microalgae cells are fixed on active mycelium balls within 3 hours (Comparative Example 1); when the initial pH is 4, only about 73% of microalgae cells are fixed on active mycelium balls within 3 hours (Comparative Example 2); when the initial pH is 5, only 64% of microalgae cells are fixed on active mycelium balls within 3 hours (Comparative Example 3). On the other hand, the pH variation in the range of 2-5 has little effect on the adsorption of gold ions. Therefore, when the optimal pH is 3.5, the microalgae-Aspergillus niger particle combination has the best adsorption effect on gold ions, and the bioflocculation effect of the microalgae is also the best.

[0166] Example 2

[0167] The initial concentration was 7.2×10 3 Spores / mL Aspergillus niger spore suspension was cultured in potato dextrose liquid medium (PDB) at pH 4 and shaken in an orbital shaker at 28°C and 120rpm. After 4-5 days of culture, fungal mycelium balls with a particle size of 9-10mm were formed. They were thoroughly rinsed with sterile deionized water, and one portion was used as active fungal particles for later use; another portion of active fungal particles was freeze-dried and stored in a freeze dryer and used as freeze-dried fungal particles for later use. The freshwater microalgae Tetradesmus obliquus concentrated by centrifugation was diluted with sterile deionized water to an absorbance of 1.2 at 680nm, and 2 portions of 100ml OD 680nm =1.2 The above algae liquid was centrifuged and concentrated and used as fresh algae liquid. Weigh 35 mg of dry weight, active and freeze-dried Aspergillus niger particles with a particle size of 9-10 mm, respectively, and then add the above microalgae-active Aspergillus niger particle combination and microalgae-freeze-dried Aspergillus niger particle combination to 100 mL of HAuCl4 solution with an initial pH of 3.5 and an initial concentration of 100 mg / L, respectively, and shake at 250 rpm in an orbital shaker at room temperature of 25±2°C for 6 hours. Sampling was performed at 5, 15, 30, 60, 120, 180, 240, 300, and 360 minutes. The samples were centrifuged at 8000 rpm for 5 minutes, the supernatant was taken, and the gold ion concentration was determined by atomic absorption spectrometer. The results are as follows Figure 3 As shown in the figure, its adsorption kinetic constant (k2) and its adsorption capacity (q e ) as shown in Table 2.

[0168] The Lagergren pseudo-second-order reaction model is a commonly used tool for analyzing adsorption kinetics, and its linear equation can be expressed as:

[0169]

[0170] q t is the amount of gold ions adsorbed per unit adsorbent mass at time t (mg / g), q e is the amount of gold ions adsorbed per unit mass of adsorbent at equilibrium (mg / g), and k2 is the second-order adsorption rate constant (g / (mg·min)).

[0171] Comparative Example 4

[0172] Same as Example 2, except that no microalgae was added. The initial concentration was 7.2×10 3 Spores / mL Aspergillus niger spore suspension was cultured in potato dextrose liquid medium (PDB) at pH 4 and shaken in an orbital shaker at 28°C and 120rpm. After 4-5 days of culture, fungal mycelium balls with a particle size of 9-10mm were formed, which were thoroughly rinsed with sterile deionized water, and one portion was used as active fungal particles for standby; another portion of active fungal particles was freeze-dried and stored using a freeze dryer as freeze-dried fungal particles for standby. Weigh the adsorbent with the same dry weight as in Example 2, and add the active and freeze-dried fungal particles to 100mL of HAuCl4 solution with an initial pH of 3.5 and an initial concentration of 100mg / L, respectively, and shaken in an orbital shaker at 250rpm for 6h at room temperature 25±2°C. Samples were taken at 5, 15, 30, 60, 120, 180, 240, 300, and 360 min, and the samples were centrifuged at 8000 rpm for 5 min. The supernatant was taken and the gold ion concentration was measured by atomic absorption spectrometry. The results are as follows: Figure 3 shown.

[0173] Comparative Example 5

[0174] The same as in Example 2, except that Aspergillus niger was not added. Weigh the same dry weight of adsorbent as in Example 2, and calculate the absorbance corresponding to 0.1 g dry weight of microalgae using formula (2) to be 1.43. Dilute the centrifuged and concentrated freshwater microalgae Tetradesmus obliquus with sterile deionized water until the absorbance of the algae solution at 680 nm is 1.43, and prepare 2 100 ml OD 680nm=1.43 The above algae liquid, one portion is centrifuged and concentrated as fresh algae liquid for standby use, and the other portion is dried into algae powder by freeze drying machine for standby use. The above fresh algae liquid and freeze-dried algae powder are added to 100mL of HAuCl4 solution with initial pH=3.5 and initial concentration of 100mg / L, respectively, and shaken at 250rpm in an orbital shaker for 6h at room temperature 25±2℃. Samples are taken at 5, 15, 30, 60, 120, 180, 240, 300, and 360min, and the samples are centrifuged at 8000rpm for 5 minutes. The supernatant is taken and the gold ion concentration is measured by atomic absorption spectrometer. The results are as follows Figure 3 shown.

[0175] Dry weight (g / L) = 1.363 × OD 680nm -0.9467,R 2 =0.974 (2)

[0176] Comparative Example 6

[0177] The initial concentration was 7.2×10 3 Spores / mL Aspergillus niger spore suspension was cultured in a potato dextrose liquid medium (PDB) at pH 4, and shaken in an orbital shaker at 28°C and 120rpm. After culturing for 4 to 5 days, fungal mycelium balls with a particle size of 9 to 10 mm were formed, which were thoroughly rinsed with sterile deionized water. Then the fungal mycelium balls were added to the culture solution of microalgae Tetradesmus obliquus with a pH of 5.0 and a bacteria-algae ratio of 1:2, and shaken on an orbital shaker at 200rpm at 25±2°C for 3h, and the algae-bacteria symbiotic particles formed were thoroughly rinsed with deionized water and used as active algae-bacteria symbiotic particles for standby use; some algae-bacteria symbiotic particles were freeze-dried and stored using a freeze dryer, and used as freeze-dried algae-bacteria symbiotic particles for standby use. Weigh the adsorbent of the same dry weight as in Example 2, add the active and freeze-dried algae-bacteria symbiotic particles with a particle size of 9 to 10 mm to 100 mL of the optimal initial pH = 3.5 (active algae-bacteria symbiotic particles) and the optimal initial pH = 2.0 (freeze-dried algae-bacteria symbiotic particles), respectively, and the initial concentration is 100 mg / L HAuCl4 solution, and shake at 250 rpm in an orbital shaker at room temperature 25±2°C for 6 hours. Samples were taken at 5, 15, 30, 60, 120, 180, 240, 300, and 360 minutes, and the samples were centrifuged at 8000 rpm for 5 minutes. The supernatant was taken and the gold ion concentration was determined by atomic absorption spectrometer, and its adsorption kinetic constant (k2) and the adsorption capacity (q2) when the adsorption reached equilibrium were measured. e ) as shown in Table 2.

[0178] Table 2 Adsorption kinetic constants of algae-bacteria symbiotic particles and microalgae-mycelium pellets

[0179]

[0180] *Including the time for preparing the algae-bacteria symbiotic particles and the time for adsorption to reach equilibrium

[0181] Experimental results: By comparing the results of Example 2 with those of Comparative Examples 4 and 5, it can be seen that in terms of gold ion adsorption efficiency, the microalgae-active fungal granule combination (Example 2, 99%) > microalgae-freeze-dried fungal granule combination (Example 2, 95%) > active / freeze-dried fungal granules (Comparative Example 4, 83%-85%) > active / freeze-dried microalgae (Comparative Example 5, 80%-81%), and within 3 to 6 hours, almost 100% of the microalgae cells were fixed on the active or freeze-dried fungal particles. Compared with the adsorption of gold ions by microalgae or fungi alone, the microalgae-fungal mycelium ball combination not only improves the adsorption performance of gold ions, but also the microalgae cells are stably fixed on the fungal mycelium balls to form algae-fungus symbiotic particles with larger particle size (9 to 10 mm) in situ, and solid-liquid separation is quickly achieved through simple sedimentation.

[0182] R 2 The closer the value is to 1, the better the model fits the data. In Example 2 and Comparative Example 6, the behavior of gold ion adsorption is very consistent with the Lagergren pseudo-second-order reaction model. Compared with the method of preparing microalgae and mycelial balls into algae-bacteria symbiotic particles in advance in Comparative Example 6, the method of combining microalgae-mycelial balls to adsorb gold ions and synchronize microalgae flocculation in Example 2 has more advantages in adsorption capacity, reaction rate and operation time. In Example 2, the adsorption capacity (100 mg / g) and adsorption rate (0.0028 g / (mg·min)) of the microalgae-active Aspergillus niger granules combination are higher than those of the microalgae-freeze-dried Aspergillus niger granules combination (96.15 mg / g, 0.0007 g / (mg·min)); in Comparative Example 6, the adsorption capacity (94.34 mg / g) and adsorption rate (0.0007 g / (mg·min)) of the freeze-dried algae-bacteria symbiotic particles are higher than those of the active algae-bacteria symbiotic particles (80 mg / g, 0.0003 g / (mg·min)). Compared with the method of preparing algae-bacteria symbiotic particles in advance with microalgae and mycelium balls, the method of using a microalgae-mycelium ball combination to adsorb gold ions and synchronously flocculate microalgae cells not only improves the adsorption performance of gold ions, but also combines the adsorption and flocculation processes, and does not require additional time and space to prepare and preserve algae-bacteria symbiotic particles, which is more advantageous in its large-scale production and application.

[0183] Example 3

[0184] The microalgae-active Aspergillus niger granules combination and the microalgae-freeze-dried Aspergillus niger granules combination in Example 1 were added to 100 mL of HAuCl4 solution with an initial pH of 3.5 and an initial concentration of 80, 100, 120, 150, and 200 mg / L, respectively, and shaken at 250 rpm in an orbital shaker at room temperature of 25±2°C for 6 h. Samples were taken when the adsorption reached stability at 360 min, and the gold ion concentration was determined by atomic absorption spectrometry. The isothermal constants (b) and the maximum adsorption capacities (q) of the two combined adsorbents were m ) as shown in Table 3. Langmuir isotherm is one of the models describing the adsorption process, and its linear equation can be expressed as:

[0185]

[0186] Ce is the concentration of gold ions in the solution at equilibrium (mg / L), q e is the amount of gold ions adsorbed per unit adsorbent mass at equilibrium (mg / g), q m is the maximum adsorption capacity of the adsorbent (mg / g), and b is a constant related to the adsorption energy (L / mg).

[0187] Table 3 Langmuir adsorption isotherm constants

[0188]

[0189] Experimental results: R 2 The closer the value is to 1, the better the model fits the data. In Example 3, the behavior of the microalgae-fungal mycelium ball combination in adsorbing gold ions is very consistent with the Langmuir model. The maximum adsorption capacity of the microalgae-active fungal granules combination is significantly higher than that of the microalgae-freeze-dried fungal granules combination (163.93 mg / g), and its maximum adsorption capacity within 6 hours at room temperature and pressure is 196.08 mg / g. In reference 4, the maximum adsorption capacity of the preformed algae-bacteria symbiotic particles freeze-dried within 6 hours at room temperature and pressure (112 mg / g) is higher than that of the active preformed algae-bacteria symbiotic particles (104 mg / g). Compared with the method of preparing microalgae and mycelium balls into algae-bacteria symbiotic particles in advance in reference 4, the method of adsorbing gold ions by the microalgae-mycelium ball combination and synchronous microalgae flocculation in Example 3 increases the maximum adsorption capacity of gold ions by 75%.

[0190] Compared with other reported biosorbents, the adsorption performance of the combination of microalgae and fungal mycelium balls in Example 3 for gold ions is significantly improved by 2 to 9 times. Reference 1 uses a manganese oxide-producing bacterium Lysinibaeillus sp.M14 to adsorb trivalent gold ions in water, and its adsorption capacity is only 21 mg / g within 1 hour at room temperature and pressure; Reference 2 uses modified mangosteen residue (particles below 40 mesh) to adsorb gold ions in wastewater, and its adsorption capacity is 100 mg / g within 24 hours at room temperature and pressure. In addition, the water-soluble adsorption material (reference document 3) and micron-sized particles (reference document 2) or bacterial cells (reference document 1) reported in the report are difficult to separate from the solution, while in Examples 1 and 2, after 3 to 6 hours of adsorption, almost 100% of the microalgae cells are stably fixed on the fungal mycelium balls, forming large algae-bacteria symbiotic particles with a particle size of 9 to 10 mm in situ, which can settle to the bottom of the container within a few seconds, and quickly achieve solid-liquid separation.

[0191] Example 4

[0192] like Figure 4 As shown, in a tower upflow reactor with a height-to-diameter ratio H / D=5.9 (inner diameter 6cm, liquid effective height 35.4cm), 1L of simulated printed circuit board (PCB) wastewater with an initial pH of 3.5 (wherein the gold ion concentration is 30mg / L) was added, and fresh algae solution Tetradesmus obliquus (1L of the algae solution has an absorbance of 1.2 at 680nm) after centrifugation and concentration, and 0.35g of dry weight, 9-10mm active fungus Aspergillus niger particles were added, and the dry weight ratio of fungi to microalgae was 1:2. The reactor was operated at room temperature of 25±2℃, and an air compressor was used for aeration at the bottom of the reactor. The concentrations of the components in the wastewater before and after adsorption are shown in Table 4.

[0193] After 3 h of adsorption, the samples were extracted from the heights of 1 / 4, 1 / 2 and 3 / 4 from the bottom of the reactor. Subsequently, the algae-bacteria symbiotic particles formed quickly settled at the bottom without aeration, and the treated wastewater was discharged from the bottom. Finally, the algae-bacteria symbiotic particles loaded with gold ions were thoroughly washed in situ with deionized water, 500 mL of 1 M thiourea was added as a desorption solution, and the pH was adjusted to 0.7 with HNO3 / NaOH. The concentrations of each component in the wastewater were determined by inductively coupled plasma mass spectrometry.

[0194] Table 4 Components and concentrations in PCB wastewater before and after adsorption (pH = 3.5, 25 ± 2 ° C)

[0195]

[0196] Experimental results: In Example 4, the adsorption rate of gold ions by the microalgae-active fungi granules combination reached 98.8% within 3 hours. The competitive adsorption results showed that although there were some coexisting heavy metal ions, such as Ni and Co, the microalgae-active fungi granules combination only removed 9.49% of Ni and 9.52% of Co, respectively, but still had strong selective adsorption for gold ions. In addition, 354.4 mg / LK in PCB wastewater + The concentration is almost 12 times that of 30 mg / L gold ions, but it has no effect on the adsorption of gold ions. After 3 hours of adsorption, nearly 80% of the microalgae cells were fixed on the active fungal particles, and the in situ algae-bacteria symbiotic particles could quickly settle to the bottom of the reactor within a few seconds, without the need for other high-energy separation methods such as centrifugation, filtration and flotation. Finally, 1M acidic thiourea (pH = 0.7) can strip 92.12% of the gold ions from the algae-bacteria symbiotic particles within 30 minutes and concentrate them in 500mL of solution, greatly reducing the cost and energy consumption of electrolysis in the next stage.

[0197] It should be noted that, although the technical solution of the present invention is introduced with specific examples, those skilled in the art will appreciate that the present invention should not be limited thereto.

[0198] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and variations will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or technical improvements in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.

Claims

1. A method for recovering precious metals from aqueous samples by adsorption, wherein: The method comprises: The step of adding an adsorbent to the aqueous sample, wherein the adsorbent comprises microalgae and mycelium pellets, and before the adsorbent is added to the aqueous sample, the microalgae and mycelium pellets in the adsorbent do not flocculate and do not form symbiotic particles; a step of adsorbing precious metals in an aqueous sample, using the adsorbent to adsorb precious metals in the aqueous sample; Preferably, the precious metal includes gold, cobalt and nickel; more preferably, the precious metal is gold; Preferably, in the step of adsorbing precious metals in the aqueous sample, while the adsorbent adsorbs the precious metals in the aqueous sample, the microalgae and mycelial balls in the adsorbent flocculate to form symbiotic particles.

2. The method according to claim 1, wherein: Before the step of adding the adsorbent to the aqueous sample, the method further comprises a step of adjusting the pH, wherein the pH value of the aqueous sample is adjusted to 2-5, preferably 2-4.

3. The method according to claim 1 or 2, wherein: Based on dry weight, the mass ratio of the mycelial pellet to the microalgae is 1:1-10, preferably 1:1-5.

4. The method according to any one of claims 1 to 3, wherein: The particle size of the mycelium ball is 5 to 15 mm, preferably 8 to 12 mm; Optionally, the mycelial pellet is an active mycelial pellet or a freeze-dried mycelial pellet.

5. The method according to any one of claims 1 to 4, wherein: The microalgae are present in the form of a suspension; Preferably, the absorbance of the microalgae suspension at 680 nm is 0.5 to 2, preferably 0.8 to 1.

5.

6. The method according to any one of claims 1 to 5, wherein: The mycelial ball is a mycelial ball formed from fungi or bacteria; Optionally, the fungus is selected from at least one of filamentous fungi and yeast; Optionally, the bacteria are selected from at least one of actinomycetes, iron bacteria and sulfur bacteria; Preferably, the fungus is selected from at least one of Aspergillus niger, Aspergillus oryzae, Rhizopus oryzae, Cladosporium cladosporoides and Aspergillus nidulans; More preferably, the fungus comprises Aspergillus niger; and / or, The microalgae is selected from at least one of freshwater microalgae, red algae and brown algae; Preferably, the microalgae is selected from at least one of Tetradesmus obliquus, Chlorella vulgaris, Chlorococcum ellipsoideum, and Phaeodactylum tricornutum; More preferably, the microalgae comprises Tetradesmus obliquus.

7. The method according to any one of claims 1 to 6, wherein: The aqueous sample is a water sample; Optionally, the water sample is selected from at least one of water samples from a water environment, industrial wastewater, mining and mineral processing wastewater, domestic water, solid digestion solution and eluent.

8. The method according to any one of claims 1 to 7, wherein: After the step of adsorbing the precious metals in the aqueous sample, the method further includes a step of recovering the precious metals, wherein: A desorption liquid is added to the adsorbent obtained in the step of adsorbing the precious metals in the aqueous sample to desorb the precious metals from the adsorbent.

9. An adsorbent, wherein The adsorbent comprises microalgae and mycelium pellets; Optionally, based on dry weight, the mass ratio of the mycelial pellet to the microalgae is 1:1 to 10, preferably 1:1 to 5; Optionally, the particle size of the mycelium pellet is 5 to 15 mm, preferably 8 to 12 mm; Optionally, the mycelial pellet is an active mycelial pellet or a freeze-dried mycelial pellet; Optionally, the microalgae is in the form of a suspension; preferably, the absorbance of the microalgae suspension at 680 nm is 0.5 to 2, preferably 0.8 to 1.5; Preferably, before using the adsorbent, the microalgae and mycelial balls in the adsorbent have not been flocculated and have not formed symbiotic particles.

10. The adsorbent according to claim 9, wherein in, The mycelial ball is a mycelial ball formed from fungi or bacteria; Optionally, the fungus is selected from at least one of filamentous fungi and yeast; Optionally, the bacteria are selected from at least one of actinomycetes, iron bacteria and sulfur bacteria; Preferably, the fungus is selected from at least one of Aspergillus niger, Aspergillus oryzae, Rhizopus oryzae, Cladosporium cladosporoides and Aspergillus nidulans; More preferably, the fungus comprises Aspergillus niger; and / or, The microalgae is selected from at least one of freshwater microalgae, red algae and brown algae; Preferably, the microalgae is selected from at least one of Tetradesmus obliquus, Chlorella vulgaris, Chlorococcum ellipsoideum, and Phaeodactylum tricornutum; More preferably, the microalgae comprises Tetradesmus obliquus.

11. A device for adsorbing and recovering precious metals in aqueous samples, wherein: The device comprises the adsorbent according to claim 9 or 10; Preferably, the precious metals include gold, cobalt and nickel; More preferably, the precious metal is gold.

12. Use of the adsorbent according to claim 9 or 10 in adsorbing and recovering precious metals in aqueous samples; Preferably, the precious metals include gold, cobalt and nickel; More preferably, the precious metal is gold.

Citation Information

Patent Citations

  • Adsorption agent for noble metal, method for manufacturing same, and method for recovering noble metal

    CN102366716A

  • Method for adsorbing heavy metal in wastewater by using mold spore

    CN104787902A

  • Macromolecular biochar sphere-immobilized microalgal composite adsorbent and preparation and application thereof

    CN107262039A

  • Bacterial-alga mixture, bacterial-alga symbiotic system and construction method and application of bacterial-alga symbiotic system

    CN114058517A

  • Multi-element bacteria and algae composition for sewage treatment, complexing agent and application of multi-element bacteria and algae composition

    CN115259391A