Method for improving recovery grade and recovery rate of calcium fluoride in fluorine-containing sludge
Through the optimization of ultrasonic flotation process, the problem of insufficient regulation of calcium fluoride recovery grade and recovery rate in fluorinated sludge in the existing technology is solved, and efficient calcium fluoride recovery is achieved, providing theoretical support for resource processing and Data support.
Patent Information
- Application Number
- CN202411018300.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, when extracting calcium fluoride from fluorine-containing sludge, there is a lack of in-depth research on off-site regulation, especially the mechanism and effect of ultrasonic treatment on the recovery grade and recovery rate of calcium fluoride have not been fully explored.
Through the ultrasonic flotation process, the ultrasonic flotation process parameters are designed, including crushing, uniform preparation of ore slurry, adding sodium oleate and acidifying water glass, and ultrasonic treatment to optimize the flotation agent. Adsorption effect improves the recovery grade and recovery rate of calcium fluoride.
It significantly improves the recycling grade and recovery rate of calcium fluoride in fluorine-containing sludge, reduces input costs, and does not need to modify existing production equipment, providing theoretical support and data support for resource processing.
Smart Images

Figure CN118993472A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of resource treatment of fluorine-containing sludge, and in particular to a method for improving the recovery grade and recovery rate of calcium fluoride in fluorine-containing sludge. Background Art
[0002] Fluorine chemical companies, photovoltaic companies and glass manufacturers produce a large amount of fluorine-containing sludge and fluorine-containing wastewater during the production process, which will cause environmental pollution if not properly treated. The main component of fluorine-containing sludge is calcium fluoride, which is a scarce and non-renewable resource in China. Therefore, fluorine-containing sludge has the value of resource recovery. At present, the main methods for extracting calcium fluoride from fluorine-containing sludge are flotation method and step-by-step extraction method.
[0003] However, the above methods all focus on using a variety of flotation agents to improve the recovery grade and recovery rate of calcium fluoride, but there is little in-depth research on off-site regulation to improve the recovery effect of calcium fluoride, especially the mechanism and effect of ultrasonic treatment on the recovery grade and recovery rate of calcium fluoride.
[0004] Many scholars at home and abroad have explored and studied ultrasonic-assisted mineral processing. For example, an article (DOI: 10.1021 / acs.energyfuels.9b01543) records that ultrasonic-assisted coal slime and graphite flotation can significantly improve the flotation concentrate yield; an article (Study on the Effect of Pretreatment on the Flotation Behavior of Scheelite and Calcium-Containing Gangue Minerals) records that when sodium oleate is used as a collector to float scheelite, fluorite, and calcite respectively, the use of ultrasonic treatment can promote the ionization of the reagent molecules; and an article (DOI: 10.1016 / j.mineng.2021.107092) records that the use of ultrasonic treatment of potash ore slurry can improve the recovery rate of potassium chloride.
[0005] Inspired by the above research, the inventors are committed to using ultrasonic treatment to recover calcium fluoride from fluoride-containing sludge, and through detailed experimental verification, reveal the influence mechanism of ultrasonic treatment on fluoride-containing sludge Zeta, the influence mechanism on the adsorption of flotation agents at the active sites of calcium fluoride, and the influence mechanism on the adsorption of flotation agents at the active sites of calcium carbonate and silicon oxide, which are the main impurities in fluoride-containing sludge, to provide detailed data and theoretical support for the improvement of fluoride-containing sludge resource treatment in the future. Summary of the invention
[0006] In order to achieve the above-mentioned purpose, the present invention provides a method for improving the recovery grade and recovery rate of calcium fluoride in fluorine-containing sludge. For the fluorine-containing sludge produced by photovoltaic enterprises, based on an in-depth study of the action mechanism of each component in the slurry by ultrasonic treatment, the recovery grade and recovery rate of calcium fluoride are improved by accurately designing the parameters of the ultrasonic flotation process. The scheme is shown below.
[0007] The present invention discloses a method for improving the recovery grade and recovery rate of calcium fluoride in fluoride-containing sludge, comprising the following steps:
[0008] S1. Collecting fluorine-containing sludge generated from treating fluorine-containing wastewater by calcium salt precipitation method, and determining the components of the fluorine-containing sludge;
[0009] S2, the fluorine-containing sludge is treated by ultrasonic flotation, washed and dried to obtain refined sludge;
[0010] The components of the fluorine-containing sludge in S1 include: CaF2 as a recycled material and CaCO3, SiO2 and other trace impurities as impurities; the mass percentage of each element in the components in the fluorine-containing sludge is:
[0011] F: 22.1-22.2%, Si: 10.8-10.9%, C: 3.4-3.5%, O: 26-26.1%, Al: 1.3-1.4%, S: 0.4-0.5%, P: 0.3-0.4%, the balance is Ca;
[0012] The flotation reagents used in the ultrasonic flotation process in S2 are: sodium oleate as a capture agent and acidified water glass as a depressant;
[0013] The steps and parameters of the ultrasonic flotation process in S2 are defined as follows:
[0014] S2-A1, crushing the fluorine-containing sludge so that the proportion of particles in the fluorine-containing sludge with a particle size range of 25 to 45 μm is ≥ 90%;
[0015] Note: At this particle size, most of the CaF2, CaCO3 and SiO2 have reached monomer dissociation, so flotation at this particle size is conducive to the removal of SiO2;
[0016] S2-A2, mixing the fluorine-containing sludge particles treated in S2-A1 with water to prepare a slurry with a mass concentration of 20%, and adjusting the pH to 9;
[0017] Description: Zeta potential can affect the adsorption of flotation agent on the sludge surface. When the charges of flotation agent and sludge particle surface are opposite, the adsorption efficiency is higher. Since sodium oleate is an anionic collector, when the Zeta potential is low (pH>9), it will generate electrostatic repulsion with the mineral surface, which is not conducive to the adsorption of sodium oleate on the target mineral surface. At the same time, it will reduce the inhibition performance of acidified water glass on SiO2.
[0018] The change of slurry concentration mainly affects the recovery efficiency of CaF2 and secondarily affects the recovery grade of CaF2. Therefore, it is necessary to select the slurry concentration value when the recovery efficiency of CaF2 is the highest.
[0019] S2-A3, adding sodium oleate and acidified water glass to the slurry; the concentration range of sodium oleate in the slurry is 1800-2400 mg / L, and the concentration range of acidified water glass in the slurry is 1300-2000 mg / L;
[0020] Note: When the dosage of sodium oleate increases, the recovery grade of CaF2 tends to decrease with a small gradient, and its recovery rate also increases greatly. However, when it exceeds a certain limit, the recovery grade of CaF2 will decrease rapidly. This is because as the dosage of sodium oleate increases, a certain amount of sodium oleate will be adsorbed on the surface of SiO2 and CaCO3, and the content of SiO2 and CaCO3 in the flotation concentrate will increase accordingly. Therefore, the addition amount of sodium oleate needs to be carefully selected;
[0021] When the amount of acidified water glass increases, the recovery grade of CaF2 has a significant increasing trend, while its recovery rate shows a trend of increasing first and then decreasing; this is because acidified water glass has a significant inhibitory effect on SiO2 and CaCO3, but with the increase in the amount of acidified water glass, water glass also has a certain inhibitory effect on CaF2, which leads to a decrease in the recovery rate of CaF2, so the addition amount of sodium oleate needs to be carefully selected;
[0022] S2-A4, ultrasonic treatment of the slurry in S2-A3, the ultrasonic parameters are: ultrasonic power of 80-200W, ultrasonic frequency of 20-60kHz, and ultrasonic time of 10-60min;
[0023] Description: When pH=8-9, the adsorption strength of Si(OH)4 molecules, the main component of acidified water glass, on the surface of CaF2 is stronger than that on the surface of CaCO3. Ultrasonic treatment will make the desorption of Si(OH)4 molecules from CaF2 more complete, the inhibitory effect of water glass on CaF2 is weakened, and the desorption site will be replaced by sodium oleate, and the floatability of CaF2 is improved. Therefore, more CaF2 is floated out overall, and the recovery rate of CaF2 shows an upward trend.
[0024] Under the action of ultrasound, sodium oleate is desorbed from the surface of SiO2, and the adsorption site is replaced by acidified water glass, which strengthens the inhibition effect of water glass, thus showing a decrease in the overall content of SiO2; the content of SiO2 also has a certain downward trend, which is due to the fact that there are two hydrogen bonds between the hydrogen atoms of Si(OH)4 molecules and the fluorine atoms on the surface of CaF2, and there is only one hydrogen bond between the hydrogen atoms of Si(OH)4 molecules and the oxygen atoms on the surface of CaCO3. The interaction between Si(OH)4 molecules and CaF2 is stronger than that of calcite, and the adsorption amount is also greater; therefore, ultrasonic treatment can more significantly improve the floatability of CaF2, that is, it can more significantly improve the recovery grade and recovery efficiency of CaF2;
[0025] When the ultrasonic flotation process in S2 meets the constraints in S2-A1 to S2-A4, the adsorption effect between the flotation reagent and CaF2, CaCO3 and SiO2 changes as follows:
[0026] The adsorption amount of sodium oleate on the active sites of CaF2, before ultrasonic treatment: after ultrasonic treatment = 1: 1.34;
[0027] The adsorption amount of acidified water glass on the active sites of CaF2, before ultrasonic treatment: after ultrasonic treatment = 1: 0.61;
[0028] The adsorption amount of sodium oleate on the active sites of CaCO3, before ultrasonic treatment: after ultrasonic treatment = 1: 1.24;
[0029] The adsorption amount of acidified water glass on the active sites of CaCO3, before ultrasonic treatment: after ultrasonic treatment = 1: 0.33;
[0030] The adsorption amount of sodium oleate on the active sites of SiO2, before ultrasonic treatment: after ultrasonic treatment = 1:0.5;
[0031] The adsorption amount of acidified water glass on the active sites of SiO2, before ultrasonic treatment: after ultrasonic treatment = 1:0.1;
[0032] It can be seen that the ultrasonic flotation process designed in the present invention can enhance the adsorption of the active sites on CaF2 to sodium oleate and reduce the adsorption of the active sites on CaF2 to acidified water glass when the constraints in S2-A1 to S2-A4 are met.
[0033] Furthermore, the steps of cleaning and drying in S2 are as follows:
[0034] The slurry treated with S2-B1 and S2-A4 was centrifuged to collect the precipitate, which was then washed with pure water;
[0035] S2-B2, drying the precipitate treated by S2-B1 at 80-110°C for 2h, and grinding and crushing the dried product to obtain refined mud.
[0036] Furthermore, the rotation speed of the centrifugal treatment in S2-B1 is 3000-3500 r / min.
[0037] Furthermore, the particle size range of the refined mud obtained after crushing in S2-B2 is 40 to 45 μm.
[0038] Further, the preparation steps of acidified water glass are as follows:
[0039] S2-C1, mixing the water glass stock solution and water in a volume ratio of 1:10 and stirring evenly to prepare a water glass prepared solution;
[0040] S2-C2, mix laboratory AR grade concentrated sulfuric acid and water in a volume ratio of 1:10 and stir evenly to prepare sulfuric acid preparation solution;
[0041] S2-C3, the sulfuric acid solution in S2-C2 and the water glass solution in S2-C1 are mixed and stirred evenly in a volume ratio of 1:1 to obtain acidified water glass as an inhibitor.
[0042] Note: Water glass was originally used mainly to inhibit SiO2, but the effect of a single inhibitor is limited, so the water glass is acidified to improve its inhibitory effect on carbonates, that is, to enhance its selective inhibitory effect on CaCO3.
[0043] Furthermore, the present invention designs a method for improving the recovery grade and recovery rate of calcium fluoride in fluorine-containing sludge, which is used for resource-based production of fluorite from fluorine-containing sludge in the photovoltaic industry.
[0044] Compared with the existing method for recovering calcium fluoride from fluoride-containing sludge, the present invention has the following beneficial effects:
[0045] (1) The design scheme of the present invention is aimed at the fluorine-containing sludge produced by photovoltaic enterprises. Based on the in-depth study of the mechanism of action of each component in the pulp by ultrasonic treatment, the parameters of the ultrasonic flotation process are precisely designed to effectively improve the recovery grade and recovery rate of CaF2 in the fluorine-containing sludge. Furthermore, the calcium fluoride extracted from the fluorine-containing sludge produced by photovoltaic enterprises can be used as a substitute for fluorite, with high added value and large market demand. These advantages significantly enhance the market competitiveness of the method of the present invention.
[0046] (2) The design scheme of the present invention does not require any changes to the production and processing equipment of existing photovoltaic enterprises. It only requires the addition of an ultrasonic flotation process after the tail sludge to effectively improve the recovery grade and recovery rate of CaF2 in the fluorine-containing sludge, with low investment cost.
[0047] (3) The pH of the original pulp is greater than 9, while the favorable pH of sludge flotation is between 8 and 9. The design of the present invention adds an ultrasonic treatment process, and the ultrasonic wave acts on water to produce H2O2, which makes H in the pulp + The concentration increases and the pH decreases. This has the following benefits: reducing the amount of acid added when adjusting the pH of the slurry, which is conducive to the selective adsorption of hydrophilic Si(OH)4 molecules on the surface of CaF2, while inhibiting SiO2 and reducing Ca 2+ Activation of SiO2. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 It is a flow chart of the steps of the design method of the present invention;
[0049] Figure 21 is a graph showing the effect of ultrasonic treatment on the adsorption of reagents on the CaF2 surface in the experimental example, wherein: (a) is a graph showing the variation of the adsorption of sodium oleate on the CaF2 surface with the ultrasonic power, (b) is a graph showing the variation of the adsorption of sodium oleate on the CaF2 surface with the ultrasonic time, (c) is a graph showing the variation of the adsorption of acidified water glass on the CaF2 surface with the ultrasonic power, and (d) is a graph showing the variation of the adsorption of acidified water glass on the CaF2 surface with the ultrasonic time;
[0050] Figure 3 1 is the effect of ultrasonic treatment on the adsorption of reagents on the CaCO3 surface in the experimental example, wherein: (a) is a curve diagram showing the variation of the adsorption of sodium oleate on the CaCO3 surface with the ultrasonic power, (b) is a curve diagram showing the variation of the adsorption of sodium oleate on the CaCO3 surface with the ultrasonic time, (c) is a curve diagram showing the variation of the adsorption of acidified water glass on the CaCO3 surface with the ultrasonic power, and (d) is a curve diagram showing the variation of the adsorption of acidified water glass on the CaCO3 surface with the ultrasonic time;
[0051] Figure 4 It is the effect of ultrasonic treatment on the adsorption of drugs on the SiO2 surface in the experimental example, where: (a) is a graph showing the variation of the adsorption of sodium oleate on the SiO2 surface with ultrasonic power, (b) is a graph showing the variation of the adsorption of sodium oleate on the SiO2 surface with ultrasonic time, (c) is a graph showing the variation of the adsorption of acidified water glass on the SiO2 surface with ultrasonic power, and (d) is a graph showing the variation of the adsorption of acidified water glass on the SiO2 surface with ultrasonic time. DETAILED DESCRIPTION
[0052] In order to further illustrate the method adopted by the present invention and the effect achieved, the technical solution of the present invention will be clearly and completely described in combination with experiments below.
[0053] Example 1: This example describes a method for improving the recovery grade and recovery rate of calcium fluoride in fluoride-containing sludge.
[0054] S1. Collecting fluorine-containing sludge generated from treating fluorine-containing wastewater by calcium salt precipitation method, and determining the components of the fluorine-containing sludge;
[0055] The components of the fluorine-containing sludge in S1 include: CaF2 as a recycled material and CaCO3, SiO2 and other trace impurities as impurities; the mass percentage of each element in the components in the fluorine-containing sludge is:
[0056] F: 22.1-22.2%, Si: 10.8-10.9%, C: 3.4-3.5%, O: 26-26.1%, Al: 1.3-1.4%, S: 0.4-0.5%, P: 0.3-0.4%, the balance is Ca;
[0057] S2, fluoride-containing sludge is treated by ultrasonic flotation method in turn:
[0058] The flotation reagents used in the ultrasonic flotation process in S2 are: sodium oleate as a capture agent and acidified water glass as a depressant;
[0059] The preparation method of acidified water glass is as follows: mixing water glass stock solution and water in a volume ratio of 1:10 and stirring evenly to prepare water glass preparation liquid; mixing laboratory AR grade concentrated sulfuric acid and water in a volume ratio of 1:10 and stirring evenly to prepare sulfuric acid preparation liquid; mixing sulfuric acid preparation liquid and water glass preparation liquid in a volume ratio of 1:1 and stirring evenly to obtain acidified water glass as an inhibitor;
[0060] The parameters of the ultrasonic flotation process in S2 are defined as follows:
[0061] S2-1. Crushing the fluorine-containing sludge so that the proportion of particles in the fluorine-containing sludge with a particle size range of 25 μm is ≥ 90%;
[0062] S2-2, the fluorine-containing sludge particles treated in S2-1 are mixed with water to prepare a slurry with a mass concentration of 20%, and the pH is adjusted to 9;
[0063] S2-3, adding sodium oleate and acidified water glass to the slurry; the concentration range of sodium oleate in the slurry is 1300 mg / L, and the concentration range of acidified water glass in the slurry is 1300 mg / L;
[0064] S2-4, ultrasonic treatment of the slurry in S2-A3, the ultrasonic parameters are: ultrasonic power of 80W, ultrasonic frequency of 20kHz, and ultrasonic duration of 10min;
[0065] The treated slurry was centrifuged at 3500 r / min, and the precipitate was collected and washed with pure water, and finally dried at 80°C for 2 hours. The dried product was ground and crushed to obtain fine mud with a particle size range of 40 to 45 μm.
[0066] When the ultrasonic flotation process in S2 meets the constraints in S2-1 to S2-4, the adsorption effect between the flotation reagent and CaF2, CaCO3 and SiO2 changes as follows:
[0067] The adsorption amount of sodium oleate on the active sites of CaF2, before ultrasonic treatment: after ultrasonic treatment = 1: 1.34;
[0068] The adsorption amount of acidified water glass on the active sites of CaF2, before ultrasonic treatment: after ultrasonic treatment = 1: 0.61;
[0069] The adsorption amount of sodium oleate on the active sites of CaCO3, before ultrasonic treatment: after ultrasonic treatment = 1: 1.24;
[0070] The adsorption amount of acidified water glass on the active sites of CaCO3, before ultrasonic treatment: after ultrasonic treatment = 1: 0.33;
[0071] The adsorption amount of sodium oleate on the active sites of SiO2, before ultrasonic treatment: after ultrasonic treatment = 1:0.5;
[0072] The adsorption amount of acidified water glass on the active sites of SiO2 before ultrasonic treatment: after ultrasonic treatment = 1:0.1.
[0073] Embodiment 2: The content recorded in this embodiment is a method under another parameter.
[0074] S1. Collecting fluorine-containing sludge generated from treating fluorine-containing wastewater by calcium salt precipitation method, and determining the components of the fluorine-containing sludge;
[0075] The components of the fluorine-containing sludge in S1 include: CaF2 as a recyclate and CaCO3, SiO2 and other trace impurities as impurities; the mass percentage of each element in the components in the fluorine-containing sludge is:
[0076] F: 22.1-22.2%, Si: 10.8-10.9%, C: 3.4-3.5%, O: 26-26.1%, Al: 1.3-1.4%, S: 0.4-0.5%, P: 0.3-0.4%, the balance is Ca;
[0077] S2, fluoride-containing sludge is treated by ultrasonic flotation method in turn:
[0078] The flotation reagents used in the ultrasonic flotation process in S2 are: sodium oleate as a capture agent and acidified water glass as a depressant;
[0079] The preparation method of acidified water glass is as follows: mixing water glass stock solution and water in a volume ratio of 1:10 and stirring evenly to prepare water glass preparation liquid; mixing laboratory AR grade concentrated sulfuric acid and water in a volume ratio of 1:10 and stirring evenly to prepare sulfuric acid preparation liquid; mixing sulfuric acid preparation liquid and water glass preparation liquid in a volume ratio of 1:1 and stirring evenly to obtain acidified water glass as an inhibitor;
[0080] The parameters of the ultrasonic flotation process in S2 are defined as follows:
[0081] S2-1. Crushing the fluorine-containing sludge so that the proportion of particles in the fluorine-containing sludge with a particle size range of 45 μm is ≥ 90%;
[0082] S2-2, the fluorine-containing sludge particles treated in S2-1 are mixed with water to prepare a slurry with a mass concentration of 20%, and the pH is adjusted to 9;
[0083] S2-3, adding sodium oleate and acidified water glass to the slurry; the concentration range of sodium oleate in the slurry is 2400 mg / L, and the concentration range of acidified water glass in the slurry is 2000 mg / L;
[0084] S2-4, ultrasonic treatment of the slurry in S2-A3, the ultrasonic parameters are: ultrasonic power of 200 W, ultrasonic frequency of 60 kHz, and ultrasonic duration of 60 min;
[0085] The ore pulp after S2-4 treatment was centrifuged at a speed of 3000 r / min, and the precipitate was collected and washed with pure water, and finally dried at 110°C for 2 hours. The dried product was ground and crushed to obtain fine mud with a particle size range of 40 to 45 μm;
[0086] When the ultrasonic flotation process in S2 meets the constraints in S2-A1 to S2-A4, the adsorption effect between the flotation reagent and CaF2, CaCO3 and SiO2 changes as follows:
[0087] The adsorption amount of sodium oleate on the active sites of CaF2, before ultrasonic treatment: after ultrasonic treatment = 1: 1.34;
[0088] The adsorption amount of acidified water glass on the active sites of CaF2, before ultrasonic treatment: after ultrasonic treatment = 1: 0.61;
[0089] The adsorption amount of sodium oleate on the active sites of CaCO3, before ultrasonic treatment: after ultrasonic treatment = 1: 1.24;
[0090] The adsorption amount of acidified water glass on the active sites of CaCO3, before ultrasonic treatment: after ultrasonic treatment = 1: 0.33;
[0091] The adsorption amount of sodium oleate on the active sites of SiO2, before ultrasonic treatment: after ultrasonic treatment = 1:0.5;
[0092] The adsorption amount of acidified water glass on the active sites of SiO2 before ultrasonic treatment: after ultrasonic treatment = 1:0.1.
[0093] Experimental example: The description of this experimental example is based on the scheme described in Example 1, and is intended to demonstrate the actual effect of the process design of the present invention.
[0094] 1. Effect of ultrasonic treatment on the adsorption of reagents on CaF2 surface
[0095] This section of the experiment uses laboratory AR grade calcium fluoride, the content of particles less than 45μm is 90%±1%, the pH is 8-9, the flotation agent sodium oleate dosage is 2000mg / L, the inhibitor acidified water glass dosage is 1600mg / L, the mud concentration is 20% of the mixed mud system, and different intensities of ultrasound treatment are used to explore the effect of different intensities of ultrasound on the adsorption of mixed reagents on the surface of calcium fluoride.
[0096] The surface adsorption of reagents on CaF2 before and after ultrasound was measured and analyzed. The surface adsorption measurement is to measure the residual reagents in the mud before and after ultrasound, and then calculate the surface adsorption of the material. The experimental results are as follows: Figure 2 shown.
[0097] Figure 2 (a) shows that in the CaF2 sodium oleate adsorption test, as the ultrasonic power increases, the adsorption amount of sodium oleate increases within 40 minutes, and the adsorption amount is always higher than 20kHz under the condition of 40kHz. This is because the greater the ultrasonic power, the greater the ultrasonic frequency, the stronger the sound intensity, the stronger the cavitation effect, the better the removal effect of impurities on the surface of the sludge components, the more impurities are removed, the more new adsorption sites will be exposed, and the adsorption effect of sodium oleate will naturally be better.
[0098] Figure 2 (b) shows that as the ultrasonic time increases, the adsorption of sodium oleate continues to increase when the power is 150W and the frequency is 20kHz; while when the frequency is 40kHz, the adsorption first increases rapidly and then stabilizes, indicating that the greater the frequency, the better the cavitation effect, the higher the efficiency of promoting sodium oleate adsorption, and the shorter the time required for ultrasonic treatment. Without ultrasonic treatment, the adsorption of sodium oleate on the CaF2 surface is 0.62mg / g, and after 40 minutes, 40kHz frequency, and 150W ultrasonic treatment, the adsorption increased to 1.45mg / g. It can be seen that ultrasonic treatment significantly increases the adsorption of sodium oleate on the CaF2 surface, thereby improving its flotation performance.
[0099] Depend on Figure 2 (c) It can be seen that in the adsorption test of acidified water glass on the CaF2 surface, when the ultrasonic time is 40min, within the test range, with the increase of ultrasonic power, the adsorption amount of acidified water glass on the CaF2 surface continues to decrease, and the reduction effect is more obvious when the ultrasonic frequency is 40kHz. Regardless of the ultrasonic frequency of 20kHz or 40kHz, the trend of the adsorption amount decreases with the increase of power, and the efficiency decreases gradually accelerates, and tends to be stable after exceeding a certain power. It can be seen that the desorption of acidified water glass requires a certain ultrasonic intensity. The increase of ultrasonic intensity is conducive to the detachment of acidified water glass from the CaF2 surface. When the ultrasonic power exceeds 150W, the desorption effect tends to be stable. Therefore, the power of 150W can be selected as the optimal ultrasonic power for ultrasonic optimization of sludge flotation indicators.
[0100] Depend on Figure 2 (d) It can be seen that as the ultrasonic time is extended, the frequency is 20kHz and 40kHz, and the power is 150W, the amount of acidified water glass adsorbed on the CaF2 surface continues to decrease; under the condition of 40kHz, the adsorption amount first decreases and then tends to stabilize, and the adsorption amount under the condition of 40kHz is always lower than the adsorption amount under the condition of 20kHz. It can be seen that the higher the frequency, the faster the dissociation rate of acidified water glass on the CaF2 surface, so the ultrasonic frequency of 40kH is selected as the ideal ultrasonic frequency. The amount of acidified water glass adsorbed on the CaF2 surface is 3.25mg / g without ultrasonic treatment. After ultrasonic treatment with an ultrasonic power of 150W, 40kH, and a time of 40min, the adsorption amount drops to 1.27mg / g.
[0101] 2. Effect of ultrasonic treatment on the adsorption of reagents on CaCO3 surface
[0102] This section of the experiment uses laboratory AR-grade CaCO3, with a content of 90%±1% of particles less than 45μm, a pH of 8-9, a flotation agent sodium oleate dosage of 2000mg / L, an inhibitor acidified water glass dosage of 1600mg / L, and a mixed mud system with a mud concentration of 20%. Ultrasonic treatment methods of different intensities are used to explore the effect of different intensities of ultrasound on the adsorption of mixed reagents on the surface of calcium carbonate, and the adsorption of reagents on the CaCO3 surface before and after ultrasound is measured and analyzed. The surface reagent measurement is to calculate the residual reagent in the mud before and after ultrasound, and then calculate the surface adsorption of the substance. The experimental results are as follows Figure 3 shown.
[0103] Depend on Figure 3 (a) It can be seen that in the CaCO3 sodium oleate adsorption test, it was found that with the increase of ultrasonic power, the time was 40min, and at a frequency of 20kHz, the amount of sodium oleate adsorbed on the CaCO3 surface continued to increase. However, at a frequency of 40kHz, the amount of sodium oleate adsorbed on the CaCO3 surface in the acidified water glass and sodium oleate mixed system showed a trend of first increasing and then decreasing with the increase of power, reaching a maximum value at a power of 150W, with an adsorption amount of 1.26mg / g. This is because the adsorption of sodium oleate on the CaCO3 surface is weaker than that of sodium oleate on CaF2, and the saturated adsorption of CaF2 for sodium oleate is greater than that of CaCO3. Therefore, within the experimental range, when the ultrasound reaches a certain intensity, sodium oleate on the calcium carbonate surface is easier to desorb than CaF2.
[0104] Figure 3(b) shows that when the ultrasonic time is prolonged and the power is 150 W, at frequencies of 20 kHz and 40 kHz, the amount of sodium oleate adsorbed on the surface of CaCO3 first increases and then stabilizes. The amount of sodium oleate adsorbed on the surface of CaCO3 is 0.55 mg / g without ultrasonic treatment. After ultrasonic treatment at 40 kHz frequency, 150 W power, and 40 min, the adsorption amount increases to 1.23 mg / g.
[0105] Figure 3 (c) shows that with the increase of ultrasonic power, when the ultrasonic time is 40 minutes, the amount of acidified water glass adsorbed on the CaCO3 surface first decreases and then stabilizes under the conditions of 20kHz and 40kHz. Under the same conditions, the adsorption amount at 40kHz is always lower than that at 20kHz.
[0106] Figure 3 (d) shows that when the ultrasonic power is 150W, at a frequency of 20kHz, the amount of acidified water glass adsorbed decreases continuously with the increase of ultrasonic time; at a frequency of 40kHz, the amount of acidified water glass adsorbed first decreases rapidly and then stabilizes. Therefore, it can be inferred that at a frequency of 40kHz, the dissociation rate of acidified water glass from the CaCO3 surface is faster. Without ultrasonic treatment, the adsorption amount is 4.12mg / g, which drops to 2.77mg / g after ultrasonic treatment at 40kHz, 150W, and 40min.
[0107] 3. Effect of ultrasonic treatment on the adsorption of drugs on SiO2 surface
[0108] This section of the experiment uses laboratory AR grade silica, with a content of 90% ± 1% of particles less than 45μm, a pH of 8-9, a flotation agent sodium oleate dosage of 2000mg / L, an inhibitor acidified water glass of 1600mg / L, and a mud concentration of 20%. Ultrasonic treatment methods of different intensities are used to explore the effect of different intensities of ultrasound on the adsorption of agents on the surface of silica, and the adsorption of agents on the SiO2 surface before and after ultrasound is measured and analyzed. The surface agent measurement is to measure the residual agent in the mud before and after ultrasound, and then calculate the surface adsorption of the material. The experimental results are as follows Figure 4 shown.
[0109] Depend on Figure 4 (a) It can be seen that in the sodium oleate adsorption test on the SiO2 surface, with the increase of ultrasonic power, the ultrasonic time is 40min, and the frequency is in the range of 40kHz and 20kHz, the adsorption amount of sodium oleate on the SiO2 surface continues to decrease, and the decrease is greater under the 40kHz condition.
[0110] Figure 4(b) shows that when the ultrasonic power is 150W, at 20kHz and 40kHz frequencies, as the ultrasonic time increases, the amount of sodium oleate adsorbed on the SiO2 surface first decreases and then stabilizes. Without ultrasonic treatment, the amount of sodium oleate adsorbed on the SiO2 surface is 0.42mg / g, which drops to 0.21mg / g after ultrasonic treatment. This shows that sodium oleate is not strongly adsorbed on SiO2, and even without ultrasonic treatment, only a small part of sodium oleate is adsorbed on the SiO2 surface.
[0111] Sodium oleate has a strong selectivity between SiO2 and CaF2. After ultrasonic treatment, the adsorption of sodium oleate on the SiO2 surface is still improved, and the adsorption ratio is reduced by 50%. This is due to the impact and stripping effect of ultrasonic cavitation on the sodium oleate on the SiO2 surface.
[0112] Depend on Figure 4 (c) It can be seen that in the adsorption test of acidified water glass on the SiO2 surface, as the ultrasonic power increases, the ultrasonic time is 40 min, and the frequency is in the range of 40 kHz and 20 kHz, the amount of acidified water glass adsorbed on the SiO2 surface gradually increases, and the increasing trend is first slow, then fast, and then tends to be stable. When other conditions are the same, the adsorption amount of acidified water glass on the SiO2 surface under the ultrasonic frequency of 40 kHz is always higher than the adsorption amount under the condition of 20 kHz.
[0113] Depend on Figure 4 (d) It can be seen that with the extension of ultrasonic time, when the power is 150W, under the condition of 20kHz frequency, the amount of acidified water glass adsorbed on the SiO2 surface continues to increase; in contrast, under the frequency of 40kHz, the adsorption amount first increases rapidly and then tends to stabilize, which shows that the increase of ultrasonic intensity can improve the adsorption of acidified water glass on the SiO2 surface. Without ultrasonic treatment, the adsorption amount is 8.92mg / g, and it rises to 9.82mg / g after 40kHz frequency, 150W power, and 40min treatment. From the adsorption amount of acidified water glass on the SiO2 surface, it can be seen that the acidified water glass has a good inhibitory effect on SiO2. Under the condition of no ultrasonic treatment, the adsorption amount of acidified water glass on the SiO2 surface has reached a good level.
Claims
1. A method for improving the recovery grade and recovery rate of calcium fluoride in fluoride-containing sludge, comprising the following steps: S1. Collecting fluorine-containing sludge generated from treating fluorine-containing wastewater by calcium salt precipitation method, and determining the components of the fluorine-containing sludge; S2, the fluorine-containing sludge is treated by ultrasonic flotation, washed and dried to obtain refined sludge; Features: The components of the fluorine-containing sludge in S1 include: CaF2 as a recyclate and CaCO3, SiO2 and other trace impurities as impurities; The mass percentage of each element in the components in the fluorine-containing sludge is: F: 22.1-22.2%, Si: 10.8-10.9%, C: 3.4-3.5%, O: 26-26.1%, Al: 1.3-1.4%, S: 0.4-0.5%, P: 0.3-0.4%, the balance is Ca; The flotation reagents used in the ultrasonic flotation process in S2 are: sodium oleate as a capture agent and acidified water glass as a depressant; The steps and parameters of the ultrasonic flotation process in S2 are defined as follows: S2-A1, crushing the fluorine-containing sludge so that the particles of the fluorine-containing sludge with a particle size range of 25 to 45 μm account for ≥ 90%; S2-A2, mixing the fluorine-containing sludge particles treated in S2-A1 with water to prepare a slurry with a mass concentration of 20%, and adjusting the pH to 9; S2-A3, adding sodium oleate and acidified water glass to the slurry; the concentration range of sodium oleate in the slurry is 1800-2400 mg / L, and the concentration range of acidified water glass in the slurry is 1300-2000 mg / L; S2-A4, ultrasonic treatment of the slurry in S2-A3, the ultrasonic parameters are: ultrasonic power of 80-200 W, ultrasonic frequency of 20-60 kHz, and ultrasonic time of 10-60 min.
2. A method for improving the recovery grade and recovery rate of calcium fluoride in fluoride-containing sludge according to claim 1, characterized in that: The steps of cleaning and drying in S2 are as follows: The slurry treated with S2-B1 and S2-A4 was centrifuged to collect the precipitate, which was then washed with pure water; S2-B2, drying the precipitate treated by S2-B1 at 80-110°C for 2h, and grinding and crushing the dried product to obtain refined mud.
3. A method for improving the recovery grade and recovery rate of calcium fluoride in fluoride-containing sludge according to claim 2, characterized in that: The rotation speed of the centrifugal treatment in S2-B1 is 3000-3500 r / min.
4. A method for improving the recovery grade and recovery rate of calcium fluoride in fluoride-containing sludge according to claim 2, characterized in that: The particle size range of the refined mud obtained after crushing in the S2-B2 is 40 to 45 μm.
5. A method for improving the recovery grade and recovery rate of calcium fluoride in fluoride-containing sludge according to claim 1, characterized in that: The preparation steps of the acidified water glass are as follows: S2-C1, mixing the water glass stock solution and water in a volume ratio of 1:10 and stirring evenly to prepare a water glass prepared solution; S2-C2, mix laboratory AR grade concentrated sulfuric acid and water in a volume ratio of 1:10 and stir evenly to prepare sulfuric acid preparation solution; S2-C3, the sulfuric acid solution in S2-C2 and the water glass solution in S2-C1 are mixed and stirred evenly in a volume ratio of 1:1 to obtain acidified water glass as an inhibitor.
6. A method for improving the recovery grade and recovery rate of calcium fluoride in fluoride-containing sludge according to any one of claims 1 to 5, characterized in that: The method is used for resource recovery of fluorine-containing sludge in the photovoltaic industry to produce fluorite.
Citation Information
Patent Citations
Flotation separation method for low-grade carbonate type fluorite mine
CN114570531A
Pretreatment method of fluorine-containing waste residues and recovery method of calcium fluoride
CN114956146A
Method for obtaining calcium fluoride through flotation of calcium fluoride sludge
CN115634775A
Method for producing potassium chloride from carnallite
CN118268124A
High-value comprehensive utilization method for lithium slag
WO2019141098A1