Metal organic acid complex as well as purification method and application thereof

Through mechanical crushing and benign ester solvent washing, the problem of impurities in metal organic acid complexes was solved, and a high-purity complex with a unique coordination method and low impurities was obtained, which improved its stability in nanomaterial synthesis Sex and application effects.

CN118993877APending Publication Date: 2024-11-22XIAN SUPERMAG BIO NANOTECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411073231.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-22

Smart Images

  • Figure CN118993877A_ABST
    Figure CN118993877A_ABST
Patent Text Reader

Abstract

The invention discloses a purification method of a metal organic acid complex. The purification method comprises the following steps: putting the metal organic acid complex to be purified into a poor solvent; mechanically crushing the metal organic acid complex in the poor solvent to obtain a mechanically crushed mixed solution; carrying out solid-liquid separation on the mixed solution, detecting the conductivity of the separated solution part, if a preset conductivity condition is not met, repeating the steps, and if the preset conductivity condition is met, executing the following steps; stirring and washing the separated solid in a benign solvent of ester, and then carrying out vacuum drying to obtain a dried solid; and transferring the dried solid into a dry inert atmosphere, and storing to obtain the purified metal organic acid complex. According to the purification method disclosed by the invention, the metal organic acid complex with a unique coordination mode and extremely low content of ester impurities and free carboxylic acid can be obtained, and the obtained metal organic acid complex can keep stable and unchanged properties even if being stored for a long time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal organic acid complexes, and specifically relates to a metal organic acid complex and a purification method and application thereof. Background Art

[0002] Metal organic acid complexes, as common precursors for thermal decomposition, show unique advantages. However, the current synthesis methods of such complexes often use metal salts as reactants and ethanol or methanol as solvents, which results in the synthesis of such complexes mixed with a large number of impurities such as esters and inorganic salts. For example, in the synthesis of precursors such as iron oleate and iron erucate, erucic acid and methanol solvent will generate byproduct methyl erucate under the action of iron ions, and will also produce inorganic salts such as sodium chloride and sodium sulfate. In addition, the synthesized metal organic acid complexes often contain impurities such as different coordination modes, unreacted free carboxylic acids, and residual solvents. The presence of these impurities causes the composition of the complex to change easily, and the stability of the coordination mode of the complex is poor, which in turn affects its application in the subsequent synthesis of nanomaterials.

[0003] There have been many studies on the purification of such complexes. For example, Hyeon et al. successfully removed inorganic salt impurities from iron oleate by washing iron oleate in n-hexane solution with water. Bronstein et al. removed free carboxylic acid by washing iron oleate complexes with ethanol and acetone. Kirkpatrick et al. crushed iron oleate with a disperser and washed with water to remove sodium chloride impurities, and then dried at 70°C to obtain powdered iron oleate, and this treatment method improved the stability of iron oleate. Dirk et al. invented a method for synthesizing iron oleate, which obtained single-coordination iron oleate with less free carboxylic acid content through a complex synthetic route. Zhang et al. removed free carboxylic acid and inorganic salt impurities from erucic acid iron by washing it with water and methanol.

[0004] However, there is no purification method that can obtain metal organic acid complexes with a unique coordination mode and extremely low ester impurities and free carboxylic acid content. Studies have shown that the presence of inorganic salts, free carboxylic acids and ester impurities in metal organic acid complexes makes the coordination mode of metal organic acid complexes complex and the composition unclear, which seriously affects its stability and has a negative impact on subsequent applications.

[0005] For example, the infrared spectrum of the iron erucate complex changes with time as follows Figure 1 As shown. Its -1 There are three absorption peaks between them, representing three different coordinations ( Figure 1 b), 1700~1750cm -1The absorption represents the ratio of ester impurities to free carboxylic acid. As time goes by, the ratio of the three coordination modes changes, and the content of ester impurities and free carboxylic acid continues to increase, indicating that the stability of this erucic acid iron is poor, and ultimately the size of the synthesized ferrite increases over time, but its monodispersity decreases. Figure 2 shown.

[0006] Therefore, developing effective purification methods to remove impurities, especially ester impurities, from the complexes is crucial to improving the quality and stability of metal-organic acid complexes. Summary of the invention

[0007] In order to solve the above problems existing in the prior art, the present invention provides a metal organic acid complex and a purification method and application thereof, which can effectively reduce the impurity content in the metal organic acid complex. Thanks to the removal of impurities, the purified metal complex has the following characteristics: (1) clear composition and unique coordination mode; (2) ester impurities, free carboxylic acid, inorganic salt, water, methanol and other impurities content is less than 2%; (3) can be stored stably for a long time; (4) the prepared nanoparticles are stable in size and have good monodispersity.

[0008] The technical problem to be solved by the present invention is achieved through the following technical solutions:

[0009] One aspect of the present invention provides a method for purifying a metal organic acid complex, comprising:

[0010] S1: placing the metal organic acid complex to be purified in a poor solvent;

[0011] S2: mechanically crushing the metal organic acid complex placed in the poor solvent to obtain a mixed solution after mechanical crushing, wherein the poor solvent includes a mixture of one or more of water, lower alcohol, acetone, acetonitrile, and dimethyl sulfoxide, and the ratio of the mass of the metal organic acid complex to the volume of the poor solvent is 1g:(10-50)mL;

[0012] S3: after solid-liquid separation of the mechanically pulverized mixed solution, the conductivity of the separated solution is detected, if the conductivity does not meet the preset conductivity condition, steps S1 to S3 are repeated, if the conductivity meets the preset conductivity condition, step S4 is executed;

[0013] S4: stirring and washing the separated solid in a benign ester solvent and performing solid-liquid separation, adding water to the separated liquid and observing whether the solution after adding water is transparent and colorless, if it is opaque or colored, continuing to stir and wash the solid with the benign ester solvent until the liquid after solid-liquid separation is transparent and colorless after adding water, and then vacuum drying to obtain a dried solid; the benign ester solvent is a mixture of one or more of acetone, acetonitrile, and tetrahydrofuran;

[0014] S5: transferring the dried solid matter into a dry inert atmosphere for storage to obtain a metal organic acid complex with a unique coordination mode and low ester impurities and free carboxylic acid content.

[0015] In one embodiment of the present invention, the metal in the metal-organic acid complex is a combination of one or more transition metals and rare earth metal elements.

[0016] In one embodiment of the present invention, the organic acid in the metal-organic acid complex is a combination of one or more saturated carboxylic acids or unsaturated carboxylic acids having 15 to 25 carbon chains.

[0017] In one embodiment of the present invention, the S2 includes:

[0018] The metal organic acid complex placed in the poor solvent is mechanically crushed by a homogenizer, the rotation speed of the homogenizer is 3000-12000 rpm, and the mesh number of the metal organic acid complex solid after crushing is greater than 80 meshes.

[0019] In one embodiment of the present invention, in step S3, when water is used as a poor solvent, the conductivity of the separated solution is detected after solid-liquid separation. When the conductivity is not greater than 20 μS / cm, the finally separated solid is obtained and step S4 is performed; when a mixed solvent of water and one or more of lower alcohols, acetone, acetonitrile, and dimethyl sulfoxide is used as a poor solvent, the conductivity of the solution after two adjacent mechanical crushing and solid-liquid separation is recorded. When the difference between the two conductivities is not greater than 5 μS / cm, it is considered that the conductivity of the solution is stable, the finally separated solid is obtained, and step S4 is performed.

[0020] In one embodiment of the present invention, the S4 includes:

[0021] The solid that meets the requirements of step S3 is added to a benign solvent of ester for stirring and washing. After solid-liquid separation, water is added to the separated liquid, and it is observed whether the solution after adding water is transparent and colorless. If it is opaque or colored, continue to stir and wash the solid with a benign solvent of ester until the liquid after solid-liquid separation is transparent and colorless after adding water; then the separated solid is vacuum dried below 50°C.

[0022] Another aspect of the present invention provides a metal organic acid complex obtained by the purification method described in any one of the above embodiments.

[0023] Another aspect of the present invention provides an application of a metal organic acid complex in preparing nanoparticles by high temperature pyrolysis.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1. The present invention provides a method for purifying a metal organic acid complex. Through the set washing and drying process, a high-purity metal organic acid complex (with a unique coordination mode and a free carboxylic acid and ester impurity content of less than 2%) can be obtained. Thanks to the extremely low impurity content, the composition of the metal organic acid complex is stable and can be stored for a long time without changing its properties, so that it has better reproducibility as a precursor in the subsequent synthesis of nanoparticles and other applications. In addition, the purification method of the present invention is simple and easy to implement, and can be applied to industrial production by simply amplifying the system.

[0026] 2. The purification method of the present invention can be used to purify various metal organic acid complexes, wherein the metal in the metal organic acid complex comprises one or more combinations of transition metals and rare earth metal elements, and the organic acid comprises one or more combinations of long-chain carboxylic acids with 15 to 25 carbon chains. Since the purified metal organic acid complex has the characteristics of low impurity content and stable composition, it has a better effect in synthesizing ultra-small ferrites. This metal organic acid complex with a unique coordination mode can be used in synthesizing small-sized nanoparticles.

[0027] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The infrared spectrum of an existing iron erucate changes with time;

[0029] Figure 2 is to use Figure 1 The change of size of ultra-small ferrite nanoparticles with time using iron erucate as a precursor;

[0030] Figure 3 This is a flow chart of a method for purifying a metal organic acid complex provided by an embodiment of the present invention;

[0031] Figure 4 It is an infrared spectrum of iron oleate obtained by using a traditional method and a purification method provided by an embodiment of the present invention;

[0032] Figure 5It is a comparison chart of MALDI-TOFMS mass spectra of iron oleate obtained by the traditional method and the purification method provided by the embodiment of the present invention;

[0033] Figure 6 The thermogravimetric diagram of iron oleate obtained by the traditional method and the purification method provided by the embodiment of the present invention;

[0034] Figure 7 It is a comparison chart of ethyl oleate content in iron oleate obtained by the traditional method and the purification method provided by the embodiment of the present invention;

[0035] Figure 8 It is a transmission electron microscope image of ultra-small ferrite synthesized by iron oleate obtained by using the traditional method and the purification method provided by the embodiment of the present invention;

[0036] Fig. 9 is a comparison chart of the nuclear magnetic resonance hydrogen spectra of ferric erucate obtained by the traditional method and the purification method of the embodiment of the present invention;

[0037] Fig.10 is a stability comparison chart of purified ferric erucate obtained by the purification method of an embodiment of the present invention;

[0038] Fig.11 This is a consistency comparison diagram of ultra-small ferrite synthesized at different times by the purified iron erucate obtained by the purification method of the embodiment of the present invention;

[0039] Fig.12 This is a comparison chart of infrared spectra of iron stearate obtained by a traditional method and a purification method according to an embodiment of the present invention;

[0040] Fig.13 This is a perspective electron microscope image of manganese ferrite synthesized from purified iron stearate obtained by the purification method of an embodiment of the present invention;

[0041] Fig.14 It is a comparison chart of infrared spectra of ferromanganese erucate obtained by the traditional method and the purification method of the embodiment of the present invention. DETAILED DESCRIPTION

[0042] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, a purification method of a metal organic acid complex proposed by the present invention is described in detail below in conjunction with the accompanying drawings and specific implementation methods.

[0043] The above and other technical contents, features and effects of the present invention are clearly presented in the following detailed description of the specific implementation modes in conjunction with the accompanying drawings. Through the description of the specific implementation modes, the technical means and effects adopted by the present invention to achieve the predetermined purpose can be more deeply and specifically understood. However, the attached drawings are only for reference and explanation purposes and are not used to limit the technical solutions of the present invention.

[0044] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants are intended to cover non-exclusive inclusion, so that an article or device including a series of elements includes not only those elements, but also other elements that are not explicitly listed. In the absence of more restrictions, the elements defined by the statement "including one..." do not exclude the existence of other identical elements in the article or device including the elements.

[0045] Embodiment 1

[0046] See also Figure 3 , Figure 3 1 is a flow chart of a method for purifying a metal organic acid complex provided by an embodiment of the present invention. The purification method specifically comprises the following steps:

[0047] S1: placing the original metal organic acid complex to be purified in a poor solvent.

[0048] The metal organic acid complex to be purified refers to the initial product of the metal organic acid complex synthesized in the previous steps. The initial product of the metal organic acid complex usually has a variety of different coordination modes and is accompanied by impurities such as esters, free carboxylic acids, inorganic salts, organic solvents, water, etc.

[0049] The metal in the metal organic acid complex is a combination of one or more transition metals and rare earth metal elements, and the organic acid in the metal organic acid complex is a combination of one or more saturated carboxylic acids or unsaturated carboxylic acids containing 15 to 25 carbon chains.

[0050] Specifically, the original metal organic acid complex (solid) to be purified is placed in a poor solvent, wherein the ratio of the mass (g) of the metal organic acid complex to the volume (mL) of the poor solvent is 1:(10-50), preferably 1:20, which has a better cleaning effect on impurities in the metal organic acid complex. In other words, 20 mL of the poor solvent is required for every 1 g of the metal organic acid complex.

[0051] The poor solvent used includes, but is not limited to, a mixture of one or more of water, lower alcohols, acetone, acetonitrile, and DMSO (dimethyl sulfoxide), preferably a mixture of water and lower alcohols or acetonitrile. Lower alcohols and acetonitrile have a certain solubility for ester impurities and free acids, and can remove some ester impurities and free carboxylic acid impurities in the metal organic acid complex. Water can effectively remove inorganic salt impurities in the complex.

[0052] S2: Mechanically crushing the metal organic acid complex placed in a poor solvent to obtain a mixed solution after mechanical crushing; the poor solvent includes a mixture of one or more of water, lower alcohol, acetone, acetonitrile, and dimethyl sulfoxide.

[0053] Specifically, a homogenizer is used to mechanically crush the metal organic acid complex placed in a poor solvent to crush the metal organic acid complex solid, and the speed of the homogenizer is 3000 to 12000 rpm. Preferably, the speed of the homogenizer is 8000 rpm, which can achieve a better crushing effect, and the mesh number of the crushed solid is greater than 80 meshes. In other embodiments, other appropriate methods or devices can also be used to achieve mechanical crushing of the metal organic acid complex, which is not limited here.

[0054] S3: After solid-liquid separation of the mechanically crushed mixed solution, the conductivity of the separated solution is detected. If the solution conductivity does not meet the preset conductivity condition, steps S1 to S3 are repeated. If the solution conductivity meets the preset conductivity condition, step S4 is executed.

[0055] In this embodiment, solid-liquid separation is performed by filtering or suction filtration. The preset conductivity conditions are: when water is used as a poor solvent, the detected liquid conductivity is less than or equal to 20μS / cm; when a mixed solvent of water and one or more of lower alcohols, acetone, acetonitrile, and dimethyl sulfoxide is used as a poor solvent, the difference between the detected liquid conductivity and the last detected liquid conductivity is less than or equal to 5μS / cm.

[0056] Specifically, when water is used as a poor solvent, the liquid conductivity is detected after solid-liquid separation. If the currently detected liquid conductivity is greater than 20 μS / cm, the separated solid is placed in a new poor solvent for mechanical crushing, and then solid-liquid separation is performed and the liquid conductivity is detected until the detected liquid conductivity is less than or equal to 20 μS / cm, and the finally separated solid is obtained and step S4 is performed;

[0057] When a mixed solvent of water and one or more of lower alcohols, acetone, acetonitrile, and dimethyl sulfoxide is used as a poor solvent, the liquid conductivity is detected after solid-liquid separation. If the difference between the currently detected liquid conductivity and the last detected liquid conductivity is greater than 5 μS / cm, the separated solid is placed in a new poor solvent for mechanical crushing, and then solid-liquid separation is performed and the liquid conductivity is detected until the difference between the currently detected liquid conductivity and the last detected liquid conductivity is less than or equal to 5 μS / cm, to obtain the finally separated solid and execute step S4.

[0058] In this step, the inorganic salt impurities and some ester impurities can be fully removed by mechanically crushing the metal organic acid complex in a poor solvent, and the removal effect of the inorganic salt can be judged by conductivity detection. The separated liquid contains inorganic salt impurities washed out of the metal organic acid complex. The residual amount of inorganic salt impurities in the solid can be determined by detecting the liquid conductivity. When the liquid conductivity reaches a specified value, it means that the inorganic salt impurities in the solid are basically washed out.

[0059] S4: After the separated solid is stirred and washed in a benign solvent of ester, vacuum drying is performed to remove ester impurities to obtain a dried solid; the benign solvent is a mixture of one or more of acetone, acetonitrile and tetrahydrofuran.

[0060] Specifically, the solid that meets the requirements of step S3 is added to the benign solvent of ester for stirring and washing. After solid-liquid separation, water is added to the separated liquid, and the solution after adding water is observed to be transparent and colorless. If it is not transparent or has color, the solid is continued to be stirred and washed with the benign solvent of ester until the solid-liquid separation solution is transparent and colorless after adding water. Then the separated solid is vacuum dried below 50°C to obtain a dried solid, which can be ground into a solid powder. It is worth noting that a similar effect can also be achieved in this step by eluting with the same benign solvent.

[0061] This step can remove free carboxylic acid, ester impurities and poor solvents remaining in the metal organic acid complex by washing, so that the coordination mode is changed to a unique bidentate coordination. The final vacuum drying removes the organic solvent used in this step.

[0062] The good solvent used in the present embodiment is a mixture of one or more of acetone, acetonitrile and tetrahydrofuran, preferably acetonitrile and acetone. These solvents have good solubility for ester impurities, and will not dissolve metal organic acid complexes at the same time, and the intermolecular force with the complex is small, and it is easy to remove by vacuum drying. The temperature of vacuum drying does not exceed 50°C, preferably 30°C. Too high a temperature will cause the metal organic acid complexes to react with the residual solvent during the drying process, and too low a temperature is not conducive to the volatilization of the organic solvent. Therefore, 30°C is a good choice when vacuum drying.

[0063] S5: The dried solid or solid powder is transferred to a strictly dried inert atmosphere for storage to obtain a purified metal organic acid complex. Storage in an inert atmosphere can prevent moisture from affecting the coordination mode of the purified metal organic acid complex.

[0064] The metal organic acid complex obtained by the method has a lower impurity content and a unique coordination mode, and can be synthesized into nanoparticles with a size less than 5nm by a dynamic synchronous thermal decomposition method.

[0065] Specifically, taking the synthesis of ultra-small manganese ferrite as an example, the preparation process includes:

[0066] 1 mmol of erucic acid iron (or oleic acid iron), 1 mmol of manganese oleate, 0.57 g of oleic acid and 1.61 g of oleyl alcohol are dissolved in 10 g of benzyl ether at room temperature to react and obtain a reaction mixture; the reaction mixture is heated to 110° C. and maintained for 30 minutes by passing argon gas into a three-necked flask accompanied by magnetic stirring to discharge impurities such as oxygen and water in the reaction mixture; then the reaction system is heated to 265° C. (if the raw material is oleic acid iron, the heating rate is 10° C. / min) at a heating rate of 5° C. / min (if the raw material is oleic acid iron, the heating rate is 10° C. / min), maintained for 30 minutes, and then rapidly cooled to room temperature, and centrifuged and washed using n-hexane as a dispersant and anhydrous ethanol as a precipitant to obtain final manganese ferrite nanoparticles.

[0067] Example 2: Iron Oleate

[0068] On the basis of Example 1, this example provides a specific method for purifying a metal organic acid complex, ferric oleate, and compares its performance with that of ferric oleate obtained by a traditional method.

[0069] There are two common ways to synthesize iron oleate. One is to add hot alkali metal oleate and inorganic iron salt to a mixture of n-hexane, ethanol and water, and the other is to react oleic acid with inorganic iron salt in methanol. The traditional purification method is to wash the n-hexane solution containing the initial product of iron oleate with water or directly wash it with a polar solvent. The obtained iron oleate is a complex mixture with multiple coordination modes, and often contains a large amount of free carboxylic acid and ester impurities. The iron oleate obtained by the purification method of the embodiment of the present invention is significantly different from the iron oleate obtained by the traditional method in terms of coordination mode, impurity content, properties, and application. The beneficial effects of the purification method proposed by the present invention will be described below through comparative experiments.

[0070] In this example, iron oleate 1 was obtained by a conventional purification method, and iron oleate 2 was obtained by the purification method proposed in this example. Figure 4 , Figure 4 The infrared spectra of iron oleate obtained by the traditional method and the purification method of the present invention are shown in Figure 1, wherein the horizontal axis represents the wave number and the vertical axis represents the transmittance. Iron oleate 1 is an iron oleate precursor obtained by the traditional method, and its infrared spectrum is shown in Figure 2. Figure 4 (a) 3300cm -1 、1710cm -1 The absorption at 1743 cm indicates that iron oleate 1 contains a large amount of free oleic acid. -1 、1170cm -1 The peak at 1590 cm-1 indicates that there are esters and free carboxylic acid impurities in iron oleate 1. -1 、1550cm -1 、1533cm -1 The absorption at indicates that there are three different coordination modes of iron oleate 1. These three coordination modes have different proportions and are impurities of each other, affecting the properties of iron oleate 1.

[0071] Iron oleate 2 is an iron oleate precursor obtained by the purification method of this embodiment. The specific purification process is as follows: 10g of the initial iron oleate product is placed in a mixture of 150mL of water and 50mL of methanol, and then mechanically crushed in a homogenizer at a speed of 8000rpm. After filtering and removing the upper layer of liquid, the liquid conductivity is detected. After repeating three times, the liquid conductivity is reduced to 19.6μS / cm. Then 50mL of acetonitrile is used to rinse the solid. After four times of washing, no white turbidity is precipitated after the washed acetonitrile is mixed with water; the obtained iron oleate complex is dried in a vacuum for 6h, and finally the iron oleate product is transferred to a dry vacuum desiccator for storage.

[0072] The infrared spectrum of iron oleate 2 is as follows Figure 4 (b) 1500-1750cm -1 Only 1531cm -1There is an absorption peak at , indicating that the oleate iron 2 has only one coordination mode and there is no impurity of free oleic acid and ethyl oleate.

[0073] See also Figure 5 , Figure 5 : is a comparison chart of the MALDI-TOF MS mass spectra of iron oleate obtained by the traditional method and the purification method of the present invention, wherein the abscissa represents the mass-to-charge ratio of the mass spectrum in Daltons, and the ordinate represents the relative intensity of the signal. Figure 5 It can be seen that the iron oleate 2 purified by the purification method of this embodiment has a unique component (such as Figure 5 The iron oleate 1 obtained by the traditional method is a complex mixture (such as Figure 5 shown by the red line).

[0074] For further information, see Figure 6 , Figure 6 The thermogravimetric diagram of iron oleate obtained by the traditional method and the purification method of the embodiment of the present invention is shown in FIG. 1 , wherein the abscissa represents the temperature and the ordinate represents the weight loss percentage. It can be seen that the thermal decomposition temperatures of the two iron oleates are very different. Benefiting from the unique coordination mode and the removal of impurities, the thermal decomposition temperature of iron oleate 2 is significantly higher than that of iron oleate 1, and the decomposition range is more concentrated.

[0075] See also Figure 7 , Figure 7 1 is a comparison chart of the ethyl oleate content in iron oleate obtained by the traditional method and the purification method of the embodiment of the present invention (obtained by gas chromatography detection), wherein the abscissa represents the retention time and the ordinate represents the relative signal intensity. It can be seen that the purification method of the embodiment of the present invention reduces the content of ethyl oleate impurity in iron oleate from 6.2% to 1.3%.

[0076] In addition, this example also uses the purified iron oleate 2 to synthesize ultra-small manganese ferrite nanoparticles. Figure 8 , Figure 8 The transmission electron microscope images of ultra-small manganese ferrite synthesized by iron oleate obtained by the traditional method and the purification method of the embodiment of the present invention are shown in FIG. As can be seen from the figure, the iron oleate 2( Figure 8 (b) The size uniformity and monodispersity of the synthesized ferrite nanoparticles are better than those of iron oleate 1( Figure 8 (a)), where d represents the average size of the nanoparticles and x represents the standard deviation.

[0077] Example 3: Ferric erucate

[0078] On the basis of Example 1, this example provides a method for purifying ferric erucate, and compares the performance of ferric erucate obtained by the traditional method with that of ferric erucate obtained by the traditional method.

[0079] Figure 1 This is the infrared spectrum change diagram of erucate purified by traditional methods and stored in an inert atmosphere. After 60 days of storage, the infrared spectrum of erucate treated by traditional methods has changed significantly. Figure 2 Ferrite nanoparticles obtained by storing erucate purified by traditional methods in an inert atmosphere for different periods of time have obvious changes in size and morphology, indicating that the erucate obtained by traditional treatment methods is not stable enough.

[0080] The method for purifying ferric erucate in this embodiment comprises the following steps: placing 100 g of ferric erucate 1 or untreated ferric erucate primary product in 2 L of water for mechanical crushing, the speed of the homogenizer used for mechanical crushing is 8000 rpm, followed by suction filtration, detecting the conductivity of the filtered liquid, repeating the crushing and washing until the liquid conductivity is reduced to below 20 μS / cm, then crushing and washing in 1 L of acetone, suction filtration and separation, repeating three times, the filtered acetone is mixed with water and becomes clear and colorless. Finally, drying for 3 h under vacuum conditions of 30° C. and 0.8 MPa to remove acetone, and transferring the product to a dry, oxygen-free environment for storage, and obtaining ferric erucate 2 through the above steps.

[0081] See also Fig. 9 , Fig. 9 The figure is a comparison of the hydrogen nuclear magnetic resonance spectra of erucate obtained by the traditional method and the purification method of the embodiment of the present invention. The hydrogen nuclear magnetic resonance spectrum shows that erucate 2 has lower impurities (lower peak area at 3.6 ppm).

[0082] See also Fig.10 , Fig.10 : This is a stability comparison diagram of purified iron erucate 2 obtained by the purification method of the embodiment of the present invention. It can be seen that the infrared spectrum of iron erucate 2 has hardly changed over time, proving that the composition of the iron erucate precursor treated by the purification method of the embodiment of the present invention has very good stability.

[0083] In addition, in order to illustrate the stability of the properties of the iron erucate obtained in the embodiment of the present invention, the present invention uses iron erucate 2 at different time points (the time is calculated from the first day after the synthesis of iron erucate) to synthesize ultra-small manganese ferrite. The size of the obtained manganese ferrite is characterized by transmission electron microscopy as follows: Fig.11 As shown, the ultrasmall ferrites synthesized at four different time points have high consistency, indicating that the purified erucate iron has high stability and reliability.

[0084] Example 4: Iron stearate

[0085] On the basis of Example 1, this example provides a method for purifying iron stearate, and compares the performance of iron stearate obtained by traditional methods.

[0086] The iron stearate obtained by the traditional method is called iron stearate 1. The process of the traditional method is roughly as follows: after the synthesis of iron stearate, it is washed with water and then vacuum dried. The drying temperature is generally 70 degrees Celsius (different synthesis processes vary).

[0087] The iron stearate obtained by the purification method of the embodiment of the present invention is called iron stearate 2, and the purification method of iron stearate 2 comprises the following steps:

[0088] 10 g of the initial product of iron stearate was placed in a mixture of 100 mL of methanol and 100 mL of water, and then mechanically crushed in a homogenizer at a speed of 8000 rpm, filtered and rinsed with acetonitrile, and finally vacuum dried at 40°C to obtain iron stearate 2.

[0089] See also Fig.12 , Fig.12 FIG. 2 is a comparison of the infrared spectra of iron stearate obtained by the traditional method and the purification method of the present invention. Fig.12 (a) 1500-1700cm -1 Only 1530cm -1 There is a strong absorption peak at , indicating that the iron stearate 2 exists in the form of a unique bidentate coordination. The infrared spectrum of iron stearate 1 is shown in Fig.12 (b) 1706cm -1 The absorption at 1573 cm indicates that there is free stearic acid in the iron stearate. -1 The strong absorption peak at indicates that the iron stearate is mainly coordinated by bridging, which is completely different from the 2-coordination mode of iron stearate.

[0090] Furthermore, the purified iron stearate obtained by the purification method of the embodiment of the present invention realizes the synthesis of ultra-small ferrite nanoparticles, and its transmission electron microscopy characterization is as follows: Fig.13 As shown, it can be seen that the size of the synthesized ultra-small manganese ferrite is 3.0±0.5nm and the morphology is good. This uniform and extremely small size manganese ferrite is difficult to synthesize using iron stearate obtained by traditional methods.

[0091] Example 5: Iron-manganese erucate complex

[0092] The purification method of the present invention is also applicable to the purification of multi-metal organic acid complexes, taking the iron-manganese erucate complex as an example, in which erucic acid coordinates with both iron and manganese. Fig.14 , Fig.14This is a comparison of the infrared spectra of erucic acid iron-manganese obtained by the traditional method and the purification method of the present invention. As shown in the figure, using the same purification method as erucic acid iron, the erucic acid iron-manganese obtained has only one coordination mode (erucic acid iron-manganese-2), such as Fig.14 As shown in the middle right figure; the iron manganese erucate 1 obtained by the traditional treatment method has three different coordination modes, such as Fig.14 Shown in the middle left picture.

[0093] In summary, the present invention provides a method for purifying a metal organic acid complex. Through the set washing and drying process, a high-purity metal organic acid complex with a unique coordination mode and a free carboxylic acid and ester impurity content of less than 2% can be obtained. Thanks to the extremely low impurity content, the composition of the metal organic acid complex is stable, and the properties can be stored for a long time without changing, so that it has better reproducibility as a precursor in the subsequent synthesis of nanoparticles and other applications. In addition, the purification method of the present invention is simple and easy, and can be applied to industrial production by simply amplifying the system.

[0094] The purification method of the present invention can be used to purify various metal organic acid complexes, wherein the metal in the metal organic acid complex comprises a combination of one or more transition metals and rare earth metal elements, and the organic acid comprises a combination of one or more long-chain carboxylic acids with 15 to 25 carbon chains. Since the purified metal organic acid complex has the characteristics of a unique coordination mode and a low impurity content, it has a better effect in synthesizing ultra-small ferrites, and the metal organic acid complex with a unique coordination mode can be applied in synthesizing small-sized nanoparticles.

[0095] In the several embodiments provided by the present invention, it should be understood that the apparatus and method disclosed by the present invention can be implemented in other ways. For example, the apparatus embodiments described above are only illustrative, for example, the division of the modules is only a logical function division, and there may be other division methods in actual implementation, for example, multiple modules or components can be combined or integrated into another system, or some features can be ignored or not executed.

[0096] In addition, each functional module in each embodiment of the present invention may be integrated into one processing module, or each module may exist physically separately, or two or more modules may be integrated into one module. The above-mentioned integrated module may be implemented in the form of hardware or in the form of hardware plus software functional modules.

[0097] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.

Claims

1. A method for purifying a metal organic acid complex, characterized in that: include: S1: placing the metal organic acid complex to be purified in a poor solvent; S2: mechanically crushing the metal organic acid complex placed in the poor solvent to obtain a mixed solution after mechanical crushing, wherein the poor solvent includes a mixture of one or more of water, lower alcohol, acetone, acetonitrile, and dimethyl sulfoxide, and the ratio of the mass of the metal organic acid complex to the volume of the poor solvent is 1g:(10-50)mL; S3: after solid-liquid separation of the mechanically pulverized mixed solution, the conductivity of the separated solution is detected, if the conductivity does not meet the preset conductivity condition, steps S1 to S3 are repeated, if the conductivity meets the preset conductivity condition, step S4 is executed; S4: stirring and washing the separated solid in a benign ester solvent and performing solid-liquid separation, adding water to the separated liquid and observing whether the solution after adding water is transparent and colorless, if it is opaque or colored, continuing to stir and wash the solid with the benign ester solvent until the liquid after solid-liquid separation is transparent and colorless after adding water, and then vacuum drying to obtain a dried solid; the benign ester solvent is a mixture of one or more of acetone, acetonitrile, and tetrahydrofuran; S5: transferring the dried solid matter into a dry inert atmosphere for storage to obtain a metal organic acid complex with a unique coordination mode and low ester impurities and free carboxylic acid content.

2. The method for purifying a metal organic acid complex according to claim 1, characterized in that: The metal in the metal-organic acid complex is a combination of one or more transition metals and rare earth metal elements.

3. The method for purifying a metal organic acid complex according to claim 1, characterized in that: The organic acid in the metal organic acid complex is a combination of one or more saturated carboxylic acids or unsaturated carboxylic acids containing 15 to 25 carbon chains.

4. The method for purifying a metal organic acid complex according to claim 1, characterized in that: The S2 includes: The metal organic acid complex placed in the poor solvent is mechanically crushed by a homogenizer, the rotation speed of the homogenizer is 3000-12000 rpm, and the mesh number of the metal organic acid complex solid after crushing is greater than 80 meshes.

5. The method for purifying a metal organic acid complex according to claim 1, characterized in that: In step S3, when water is used as the poor solvent, the conductivity of the separated solution is detected after solid-liquid separation. When the conductivity is not greater than 20 μS / cm, the solid after final separation is obtained and step S4 is performed; when a mixed solvent of water and one or more of lower alcohols, acetone, acetonitrile, and dimethyl sulfoxide is used as the poor solvent, the conductivity of the solution after two adjacent mechanical crushing and solid-liquid separation is recorded. When the difference between the two conductivities is not greater than 5 μS / cm, the conductivity of the solution is considered to be stable, the solid after final separation is obtained, and step S4 is performed.

6. The method for purifying a metal organic acid complex according to claim 1, characterized in that: The S4 includes: The solid that meets the requirements of step S3 is added to a benign solvent of ester for stirring and washing. After solid-liquid separation, water is added to the separated liquid, and it is observed whether the solution after adding water is transparent and colorless. If it is opaque or colored, continue to stir and wash the solid with a benign solvent of ester until the liquid after solid-liquid separation is transparent and colorless after adding water; then the separated solid is vacuum dried below 50°C.

7. A metal organic acid complex, characterized in that: Obtained by the purification method according to any one of claims 1 to 6.

8. Use of the metal organic acid complex according to claim 7 in preparing nanoparticles by high temperature pyrolysis.