Preparation method of boron-containing polyethylene shielding material

By preparing B4C/HDPE shielding masterbatches in boron-containing polyethylene materials and mixing them with ultra-high molecular weight polyethylene, the problem of poor dispersion uniformity of boron carbide particles is solved, the mechanical properties and shielding efficiency of the material are improved, and high density and Good radiation resistance.

CN118994764APending Publication Date: 2024-11-22XIAN RARE METAL MATERIALS RES INST CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411328774.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The dispersion uniformity between boron carbide particles and ultra-high molecular weight polyethylene in the existing boron-containing polyethylene materials is poor, resulting in low shielding efficiency, making it difficult to achieve high-density sintered bodies and good mechanical properties.

Method used

The ethanol dispersion solution using coupling agent was sprayed onto the surface of boron carbide particles and mixed with high-density polyethylene and maleic anhydride grafted polyethylene to prepare B4C/HDPE shielded masterbatch, and mixed with ultra-high molecular weight polyethylene, and then extruded. The molding process obtains uniformly distributed boron carbide particles, improving the mechanical properties and shielding efficiency of the material.

Benefits of technology

By pre-preparing B4C/HDPE shielding masterbatch, the uniform distribution of boron carbide particles in the material is achieved, the mechanical properties and surface quality of boron-containing polyethylene shielding materials are improved, and the problems of particle agglomeration and low production efficiency are solved. Excellent radiation resistance and corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994764A_ABST
    Figure CN118994764A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a boron-containing polyethylene shielding material. The method comprises the following steps: 1, dispersing a coupling agent on the surfaces of boron carbide particles to obtain surface-modified boron carbide particles; 2, uniformly mixing the surface-modified boron carbide particles with high-density polyethylene and maleic anhydride grafted polyethylene to obtain a mixture; 3, granulating the mixture to obtain a B4C / HDPE shielding master batch; and 4, mixing and molding the B4C / HDPE shielding master batch, ultra-high molecular weight polyethylene, an antioxidant, an ultraviolet absorbent and a nucleating agent to obtain the boron-containing polyethylene shielding material. According to the invention, the B4C / HDPE shielding master batch with good boron nitride particle dispersity and density similar to that of the ultra-high molecular weight polyethylene is prepared firstly, and is easy to disperse when being mixed with the ultra-high molecular weight polyethylene to prepare the shielding material, so that the distribution uniformity of the boron carbide particles in the shielding material is improved; the boron-containing polyethylene shielding material is suitable for the field of neutron radiation shielding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of boron-containing polyethylene material processing, and in particular relates to a method for preparing a boron-containing polyethylene shielding material. Background Art

[0002] In the core components of nuclear reactors, neutron absorbing materials are important structural and functional materials second only to nuclear fuel elements. Boron carbide, as a ceramic material with strong covalent bonds, has a high neutron capture cross section, no secondary radiation pollution, and high thermal stability. At the same time, boron carbide is abundant in source and easy to handle waste. It is widely used as a neutron absorber in nuclear reactor control. However, boron carbide ceramics directly sintered with boron carbide raw materials have two fatal weaknesses: one is that the fracture toughness of the ceramics is very low, and the other is that it is difficult to obtain a high-density sintered body. Selecting radiation-resistant polyethylene materials as carriers to prepare boron-containing polyethylene composite materials is a better technical means. Compared with traditional metals and concrete, boron-containing polyethylene has the characteristics of low density, corrosion resistance, good attenuation curve, low cost, and excellent processing performance, which can meet the needs of radiation shielding occasions of different energy levels.

[0003] However, the density and particle size differences between the thermal neutron shielding components and polyethylene in the existing boron-containing polyethylene materials are large, and the binding energy between them is weak, making it difficult to disperse evenly. There are always shielding component enrichment areas at the microscopic scale, which in turn affects the comprehensive shielding performance of the material. Chinese patent publication number CN110358177A discloses a boron-containing polyethylene rod and its preparation process, and the corresponding raw and auxiliary materials are mixed at the same time and then extruded to prepare the boron-containing polyethylene rod; Chinese patent publication number CN112143066A discloses a boron-containing polyethylene composite shielding rod and its preparation method, and elaborates on the types of raw materials and auxiliary materials in the boron-containing polyethylene formula; Chinese patent publication number CN114672086A discloses a neutron poison storage material and its preparation method, a neutron poison storage tank, and a neutron poison storage tank is prepared by a molding process. The above three patents all adopt a mixing method of directly mixing polyethylene and boron carbide particles, or adding polyethylene wax premix and then adding boron carbide powder. Due to the density of boron carbide (2.52g / cm 3 ) and ultra-high molecular weight polyethylene density (0.920~0.964g / cm 3 ) differences, the problem of dispersion uniformity has not been effectively solved. Among them, the Chinese patent CN114672086A mentioned that the maximum value of component uniformity (the difference between the maximum and minimum values ​​of boron content) is 1.7%, and the minimum value is 0.9%. The uneven distribution of boron carbide content in different parts will seriously affect the shielding performance of the composite material, resulting in poor shielding efficiency. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a method for preparing a boron-containing polyethylene shielding material in view of the above-mentioned deficiencies of the prior art. The method first prepares B nitride particles with good dispersibility and a density similar to that of ultra-high molecular weight polyethylene. 4 C / HDPE shielding masterbatch is easy to disperse when mixed with ultra-high molecular weight polyethylene to prepare shielding materials, further improving the distribution uniformity of boron carbide particles in the shielding material, effectively improving the mechanical properties and shielding efficiency of the shielding material, and solving the problem of reduced shielding efficiency of boron carbide in ultra-high molecular weight polyethylene due to poor dispersion uniformity.

[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a boron-containing polyethylene shielding material, characterized in that the method comprises the following steps: Step 1: spray the ethanol dispersion solution of the coupling agent evenly onto the surface of the boron carbide particles, stir evenly and dry to obtain surface-modified boron carbide particles; Step 2: uniformly mixing the surface-modified boron carbide particles obtained in step 1 with high-density polyethylene and maleic anhydride grafted polyethylene to obtain a mixture; Step 3: Melt the mixture and extrude it into granules to prepare B 4 C / HDPE shielding masterbatch; Step 4: B obtained in step 3 4 C / HDPE shielding masterbatch is mixed with ultra-high molecular weight polyethylene, antioxidant, ultraviolet absorber and nucleating agent, and the boron-containing polyethylene shielding material is prepared by extrusion molding or compression molding.

[0006] The present invention sprays the ethanol dispersion solution of the coupling agent evenly onto the surface of the boron carbide particles, stirs evenly, and then leaves the mixture to completely volatilize the solvent component to obtain surface-modified boron carbide particles, and then mixes the mixture with high-density polyethylene and maleic anhydride grafted polyethylene and puts the mixture into a parallel twin-screw extruder for melt extrusion and granulation to obtain B 4 The C / HDPE shielding masterbatch is then mixed with ultra-high molecular weight polyethylene, antioxidant, UV absorber and nucleating agent, and is extruded by a single screw extruder to obtain a shielding rod of a target size, or is molded by a hot press to obtain a shielding sheet of a target size.

[0007] In the preparation process of the present invention, high-density polyethylene (HDPE) is used as a matrix and boron carbide particles are used as fillers to prepare B with neutron shielding performance. 4 C / HDPE shielding masterbatch, using the good melt fluidity and high thermal neutron attenuation coefficient of high-density polyethylene, makes its molten state fully wrap the boron carbide particles. At the same time, maleic anhydride is grafted onto polyethylene to improve the compatibility of boron carbide particles with HDPE matrix, so as to achieve effective dispersion of boron carbide particles. 4C / HDPE shielding masterbatch is mixed with ultra-high molecular weight polyethylene and then molded. Since HDPE and ultra-high molecular weight polyethylene are different polymers of the same polyethylene type, according to the similar compatibility principle of polymer materials, B 4 After adding C / HDPE shielding masterbatch to ultra-high molecular weight polyethylene, the compatibility of the two is improved, and HDPE can be used as a lubricant in the processing of ultra-high molecular weight polyethylene. More importantly, compared with directly adding boron carbide particles to ultra-high molecular weight polyethylene, B 4 The density of C / HDPE shielding masterbatch is similar to that of ultra-high molecular weight polyethylene, making it easier to achieve uniform mixing. 4 C / HDPE shielding masterbatch achieves uniform distribution of boron carbide particles in the shielding material system, improves the mechanical properties and surface quality of boron-containing polyethylene shielding materials, and solves the problems of particle agglomeration and low production efficiency caused by directly adding boron carbide to ultra-high molecular weight polyethylene.

[0008] The above-mentioned method for preparing a boron-containing polyethylene shielding material is characterized in that the molecular weight of the high-density polyethylene described in step 2 is 50,000 to 200,000, the melt index is 4g / 10min to 25g / 10min, the grafting rate of maleic anhydride in the maleic anhydride grafted polyethylene is 0.5% to 1.2%, and the uniform mixing time is 5min to 30min; the viscosity-average molecular weight of the ultra-high molecular weight polyethylene described in step 4 is 3 million to 8 million.

[0009] The present invention selects HDPE resin as the matrix resin of the shielding masterbatch because HDPE has the highest thermal neutron attenuation coefficient among the three polyethylene raw materials of HDPE, LDPE and LLDPE. In addition, by screening the molecular weight and melt index of high-density polyethylene, the processability of the shielding masterbatch is further improved. By controlling the grafting rate of maleic anhydride in maleic anhydride grafted polyethylene, it is avoided that the grafting rate is too low, resulting in a reduction in the binding sites between the boron carbide particles and the HDPE matrix, and the inability to achieve uniform dispersion, and the grafting rate is too high, resulting in self-aggregation between maleic anhydride molecules, and the dispersion effect of the boron carbide particles is not significantly improved; at the same time, by controlling the viscosity average molecular weight of the ultra-high molecular weight polyethylene to be 3 million to 8 million, it is avoided that the mechanical properties of the boron-containing polyethylene shielding material prepared by molding due to the low viscosity average molecular weight and the neutron shielding performance after the irradiation aging test cannot meet the requirements, and the viscosity average molecular weight is too high, resulting in processing and molding difficulties.

[0010] The above-mentioned method for preparing a boron-containing polyethylene shielding material is characterized in that in step three, a parallel twin-screw extruder is used to melt-extrude the mixture into granules, and the extrusion temperature is 150°C~230°C, the screw speed is 5r / min~20r / min, and the granules are air-cooled.

[0011] The above-mentioned method for preparing a boron-containing polyethylene shielding material is characterized in that the B 4 C / HDPE shielding masterbatch includes, by mass percentage: boron carbide particles 40%~65%, high-density polyethylene 28.5%~55.3%, maleic anhydride grafted polyethylene 3%~10%, coupling agent KH570 1%~2%.

[0012] The above-mentioned method for preparing a boron-containing polyethylene shielding material is characterized in that the B 4 The average particle size of C / HDPE shielding masterbatch is 2mm~4mm. 4 The particle size of C / HDPE shielding masterbatch enables it to be mixed more fully with ultra-high molecular weight polyethylene.

[0013] The above-mentioned method for preparing a boron-containing polyethylene shielding material is characterized in that the boron carbide particles in step one are nuclear-grade boron carbide particles, and the average particle size of the boron carbide particles is 5μm~20μm, and the maximum particle size is 15μm~48μm.

[0014] The above-mentioned method for preparing a boron-containing polyethylene shielding material is characterized in that the B 4 The mass ratio of C / HDPE shielding masterbatch to ultra-high molecular weight polyethylene is 1:1~1:10. 4 C / HDPE shielding masterbatch can be fully dispersed in ultra-high molecular weight polyethylene to ensure B 4 C concentration, thereby obtaining a boron-containing polyethylene shielding material with good mechanical properties.

[0015] The above-mentioned method for preparing a boron-containing polyethylene shielding material is characterized in that the mass ratio of the high-density polyethylene in the shielding masterbatch to the added ultra-high molecular weight polyethylene in step 4 is 1:1 to 1:32. When the mass ratio is lower than this, the mechanical properties of the boron-containing polyethylene shielding material deteriorate, and when the mass ratio is higher than this, the mechanical properties of the boron-containing polyethylene shielding material deteriorate. 4 C / HDPE shielding masterbatch cannot be fully dispersed in UHMWPE to obtain the specified concentration.

[0016] The above-mentioned method for preparing a boron-containing polyethylene shielding material is characterized in that the antioxidant in step 4 is selected from Irganox 1010, Irganox 1076, Irgafos 168 and DLTP, the ultraviolet absorber is selected from one or more of UV-944, UV-1130 and UV-329, and the nucleating agent is selected from one or more of nano silicon dioxide, zinc stearate and calcium stearate; the extrusion molding adopts a single screw extruder, and the process parameters are: feeding section 130℃~220℃, plasticizing and melting section 180℃~290℃, head molding temperature 220℃~270℃, extrusion speed 50mm / h~120mm / h, screw speed 6Hz~10Hz, and after extrusion molding, it is machined to obtain the boron-containing polyethylene shielding material; the process parameters of the compression molding in step 4 are: molding temperature 160℃~260℃, molding pressure 30MPa~120MPa, pressure cooling after cooling, and the boron-containing polyethylene shielding material is obtained after machining.

[0017] The above-mentioned method for preparing a boron-containing polyethylene shielding material is characterized in that the boron-containing polyethylene shielding material in step 4 comprises, by mass percentage, 50% to 90% of ultra-high molecular weight polyethylene, B 4 C / HDPE shielding masterbatch 9%~48%, antioxidant 0.1%~2%, UV absorber 0.1%~1%, nucleating agent 0.8%~3%.

[0018] Compared with the prior art, the present invention has the following advantages: 1. The present invention uses high-density polyethylene as a matrix and boron carbide particles as an inorganic filler to prepare B with neutron shielding performance 4 C / HDPE shielding masterbatch, the boron nitride particles in the masterbatch have good dispersibility, and the masterbatch density is similar to that of ultra-high molecular weight polyethylene. It is easy to disperse when mixed with ultra-high molecular weight polyethylene to prepare shielding materials, further improving the distribution uniformity of boron carbide particles in the shielding material, effectively improving the mechanical properties and shielding efficiency of the shielding material, and has excellent radiation resistance and corrosion resistance.

[0019] 2. The present invention prepares B 4 C / HDPE shielding masterbatch is added to ultra-high molecular weight polyethylene, and the good processability of high-density polyethylene in the masterbatch and its good compatibility with ultra-high molecular weight polyethylene are utilized to play a role of lubricant, thereby improving the problems of ultra-high molecular weight polyethylene such as difficult extrusion process due to the addition of fillers and defects inside the rods, thereby preparing large-diameter rods or high-thickness and long-sized boron-containing polyethylene sheets filled with high-content boron carbide particles, without internal defects and with good apparent quality.

[0020] 3. The deviation of the mass content of boron carbide in the boron-containing polyethylene shielding material prepared by the present invention is less than 0.45%. The tensile strength of the boron-containing polyethylene shielding material is greater than 21.5 MPa, the elongation at break is greater than 183%, the bending strength is greater than 22.0 MPa, and the boron-containing polyethylene shielding material is irradiated by 4.5×10 6 After the irradiation aging test with a Gy dose, the change rate of the ion shielding performance is no more than 0.6%. After immersion for one month at 60°C and 4 mol / L nitric acid, the change rate of the ion shielding performance is no more than 0.7%. Therefore, the boron-containing polyethylene shielding material not only has excellent radiation resistance and corrosion resistance, but also has good mechanical properties and processability.

[0021] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a physical picture of the test device for immersion at 60°C and 4 mol / L nitric acid in the present invention.

[0023] Figure 2 The bar graph is a graph showing the tensile strength, flexural strength and elongation at break of the boron-containing polyethylene shielding material profiles prepared in Examples 1 to 5 of the present invention and Comparative Examples 1, 3, 5 and 7.

[0024] Figure 3 B prepared in Example 1 of the present invention 4 Scanning electron microscopy image of the distribution state of boron carbide particles in C / HDPE shielding masterbatch.

[0025] Figure 4 This is a scanning electron micrograph of the distribution state of boron carbide particles in the boron-containing polyethylene shielding material rod prepared in Example 1 of the present invention.

[0026] Figure 5 This is a scanning electron micrograph of the distribution state of boron carbide particles in the boron-containing polyethylene shielding material rod prepared in Comparative Example 7 of the present invention. DETAILED DESCRIPTION

[0027] The manufacturer of the maleic anhydride grafted polyethylene used in Examples 1 to 5 and Comparative Examples 1 to 10 of the present invention is Ningbo Nengzhiguang New Material Technology Co., Ltd.

[0028] Example 1 This embodiment includes the following steps: Step 1: Spray 325 mL of 3 mol / L KH570 ethanol dispersion solution evenly onto the surface of 7.2 kg of boron carbide particles with an average particle size of 20 μm and a maximum particle size of 48 μm, stir evenly and dry until the liquid component is completely volatilized to obtain surface-modified boron carbide particles; Step 2: Put the surface-modified boron carbide particles obtained in step 1, 9.958 kg of high-density polyethylene with a molecular weight of 50,000 and a melt index of 25 g / 10 min, and 0.6 kg of maleic anhydride grafted polyethylene with a grafting rate of 0.5% into a high-speed mixer and mix them evenly for 10 minutes to obtain a mixture; Step 3: The mixed material obtained in step 2 is put into a parallel twin-screw extruder for melt extrusion granulation, and the extrusion temperature is 150°C, the screw speed is 20r / min, and air-cooled granulation is performed to prepare B 4 C / HDPE shielding masterbatch; 4 C / HDPE shielding masterbatch includes, by mass percentage: 40% boron carbide particles, 55.3% high-density polyethylene, 3.3% maleic anhydride grafted polyethylene, 1.3% coupling agent KH570, and the B 4 The particle size of C / HDPE shielding masterbatch is 2.4mm±0.2mm; Step 4: 10 kg of B obtained in step 3 4 C / HDPE shielding masterbatch was mixed with 10.58kg ultra-high molecular weight polyethylene with a viscosity average molecular weight of 3 million, 70g antioxidant Irganox 1010, 70g ultraviolet absorber UV-329 and 280g nucleating agent calcium stearate, and extruded by a single screw extruder. The process parameters were as follows: feeding section 130°C, plasticizing and melting section 210°C, die head molding temperature 220°C, extrusion speed 50mm / h, screw speed 6Hz, and the boron-containing polyethylene shielding material rod was obtained by machining; the boron-containing polyethylene shielding material rod included, by mass percentage: ultra-high molecular weight polyethylene 50.38%, B 4 C / HDPE shielding masterbatch 47.62%, antioxidant Irganox 1010 0.33%, UV absorber UV-329 0.33%, nucleating agent calcium stearate 1.3%.

[0029] After testing, the deviation value of the mass content of boron carbide in the boron-containing polyethylene shielding material rod prepared in this embodiment is 0.42%, the tensile strength of the boron-containing polyethylene shielding material rod is 26.89MPa, the elongation at break is 205.46%, the bending strength is 24.10MPa, and the gamma-ray 4.5×10 6 After the irradiation aging test with a dose of Gy, the change rate of the neutron shielding performance was 0.5%. Figure 1 The device shown in the figure has a 0.4% change in ion shielding performance after being immersed in 4 mol / L nitric acid at 60°C for one month.

[0030] The antioxidant of this embodiment can also be selected from one or more of Irganox 1010, Irganox 1076, Irgafos 168 and DLTP other than Irganox 1010; the ultraviolet absorber can also be selected from one or more of UV-944, UV-1130 and UV-329 other than UV-329; the nucleating agent can also be selected from one or more of nano-silicon dioxide, zinc stearate and calcium stearate other than calcium stearate.

[0031] Example 2 This embodiment includes the following steps: Step 1: Spray 240 mL of 2 mol / L KH570 ethanol dispersion solution evenly onto the surface of 6.5 kg of boron carbide particles with an average particle size of 10 μm and a maximum particle size of 27 μm, stir evenly and dry until the liquid component is completely volatilized to obtain surface-modified boron carbide particles; Step 2: The surface-modified boron carbide particles obtained in step 1, 3.08 kg of high-density polyethylene with a molecular weight of 200,000 and a melt index of 4.3 g / 10 min, and 0.3 kg of maleic anhydride grafted polyethylene with a grafting rate of 1.2% are put into a high-speed mixer and uniformly mixed for 25 minutes to obtain a mixture; Step 3: The mixed material obtained in step 2 is put into a parallel twin-screw extruder for melt extrusion granulation, and the extrusion temperature is 230°C, the screw speed is 15r / min, and air-cooled granulation is performed to prepare B 4 C / HDPE shielding masterbatch; 4 C / HDPE shielding masterbatch includes, by mass percentage: 65% boron carbide particles, 30.8% high-density polyethylene, 3% maleic anhydride grafted polyethylene, 1.2% coupling agent KH570, and the B 4 The particle size of C / HDPE shielding masterbatch is 3.5mm±0.5mm; Step 4: 2 kg of B obtained in step 3 4 C / HDPE shielding masterbatch was mixed with 19.61kg ultra-high molecular weight polyethylene with a viscosity average molecular weight of 3 million, 48g antioxidant Irganox 168, 96g ultraviolet absorber UV-944 and 250g nucleating agent nano-silica, and extruded by a single screw extruder. The process parameters were as follows: feeding section 130°C, plasticizing and melting section 290°C, die head molding temperature 270°C, extrusion speed 120mm / h, screw speed 10Hz, and machined to obtain boron-containing polyethylene shielding material rods; the boron-containing polyethylene shielding material rods included, by mass percentage, 89.14% ultra-high molecular weight polyethylene, B 4C / HDPE shielding masterbatch 9.1%, antioxidant Irganox 168 0.22%, UV absorber UV-944 0.44%, nucleating agent nano-silica 1.14%.

[0032] After testing, the deviation value of the mass content of boron carbide in the boron-containing polyethylene shielding material rod prepared in this embodiment is 0.20%, the tensile strength of the boron-containing polyethylene shielding material rod is 29.32MPa, the elongation at break is 210.64%, the bending strength is 22.4MPa, and the gamma-ray 4.5×10 6 After the aging test with a dose of Gy, the change rate of the ion shielding performance was 0.4%. Figure 1 The device shown has a neutron shielding performance change rate of 0.5% after being immersed in 4 mol / L nitric acid at 60°C for one month.

[0033] Example 3 This embodiment includes the following steps: Step 1: Spray 240 mL of 2 mol / L KH570 ethanol dispersion solution evenly onto the surface of 3 kg of boron carbide particles with an average particle size of 5 μm and a maximum particle size of 15 μm, stir evenly and dry until the liquid component is completely volatilized to obtain surface-modified boron carbide particles; Step 2: The surface-modified boron carbide particles obtained in step 1, 2.58 kg of high-density polyethylene with a molecular weight of 125,000 and a melt index of 14 g / 10 min, and 0.3 kg of maleic anhydride grafted polyethylene with a grafting rate of 1.2% are put into a high-speed mixer and uniformly mixed for 10 minutes to obtain a mixture; Step 3: The mixed material obtained in step 2 is put into a parallel twin-screw extruder for melt extrusion granulation, and the extrusion temperature is 190°C, the screw speed is 15r / min, and air-cooled pelletizing is performed to prepare B 4 C / HDPE shielding masterbatch; 4 C / HDPE shielding masterbatch includes, by mass percentage: 50% boron carbide particles, 43% high-density polyethylene, 5% maleic anhydride grafted polyethylene, 1.9% coupling agent KH570, and the B 4 The particle size of C / HDPE shielding masterbatch is 3.0mm±0.5mm; Step 4: 3 kg of B obtained in step 3 4C / HDPE shielding masterbatch was mixed with 11.736kg ultra-high molecular weight polyethylene with a viscosity average molecular weight of 8 million, 48g antioxidant Irganox 168, 96g ultraviolet absorber UV-329 and 120g nucleating agent zinc stearate, and extruded by a single screw extruder. The process parameters were as follows: feeding section 190°C, plasticizing and melting section 290°C, die head molding temperature 245°C, extrusion speed 80mm / h, screw speed 10Hz, and machined to obtain boron-containing polyethylene shielding material rods; the boron-containing polyethylene shielding material rods included, by mass percentage: ultra-high molecular weight polyethylene 78.24%, B 4 C / HDPE shielding masterbatch 20%, antioxidant Irganox 168 0.32%, UV absorber UV-329 0.64%, nucleating agent zinc stearate 0.8%.

[0034] After testing, the deviation value of the mass content of boron carbide in the boron-containing polyethylene shielding material rod prepared in this embodiment is 0.30%, the tensile strength of the boron-containing polyethylene shielding material rod is 27.92MPa, the elongation at break is 190.08%, the bending strength is 23.84MPa, and the gamma-ray 4.5×10 6 After the aging test with a dose of Gy, the change rate of the neutron shielding performance was 0.6%. Figure 1 The device shown in the figure has a 0.4% change in ion shielding performance after being immersed in 4 mol / L nitric acid at 60°C for one month.

[0035] Example 4 This embodiment includes the following steps: Step 1: Spray 240 mL of 2 mol / L KH570 ethanol dispersion solution evenly onto the surface of 6.5 kg of nuclear grade boron carbide particles with an average particle size of 10 μm and a maximum particle size of 27 μm, stir evenly and dry until the liquid component is completely volatilized to obtain surface-modified boron carbide particles; Step 2: Put the surface-modified boron carbide particles obtained in step 1, 3.08 kg of high-density polyethylene with a molecular weight of 200,000 and a melt index of 4.3 g / 10 min, and 0.3 kg of maleic anhydride grafted polyethylene with a grafting rate of 1.2% into a high-speed mixer and mix them evenly for 25 minutes to obtain a mixture; Step 3: The mixed material obtained in step 2 is put into a parallel twin-screw extruder for melt extrusion granulation, and the extrusion temperature is 230°C, the screw speed is 15r / min, and air-cooled granulation is performed to prepare B 4 C / HDPE shielding masterbatch; 4C / HDPE shielding masterbatch includes, by mass percentage: 65% boron carbide particles, 30.8% high-density polyethylene, 3% maleic anhydride grafted polyethylene, 1.2% coupling agent KH570, and the B 4 The particle size of C / HDPE shielding masterbatch is 3.5mm±0.5mm; Step 4: 4 kg of B obtained in step 3 4 C / HDPE shielding masterbatch is mixed with 4.61kg ultra-high molecular weight polyethylene with a viscosity average molecular weight of 3 million, 48g antioxidant Irganox 168, 96g ultraviolet absorber UV-944 and 250g nucleating agent calcium stearate, and produced by compression molding process. The process parameters of compression molding are: molding temperature 260°C, molding pressure 100MPa, cooling under pressure after cooling, and machining to obtain boron-containing polyethylene shielding material sheet; the boron-containing polyethylene shielding material sheet includes, by mass percentage: ultra-high molecular weight polyethylene 51.20%, B 4 C / HDPE shielding masterbatch 44.42%, antioxidant Irganox 168 0.53%, UV absorber UV-944 1.07%, nucleating agent calcium stearate 2.78%.

[0036] After testing, the deviation value of the mass content of boron carbide in the boron-containing polyethylene shielding material sheet prepared in this embodiment is 0.43%, the tensile strength of the boron-containing polyethylene shielding material sheet is 21.67MPa, the elongation at break is 183.45%, the bending strength is 27.95MPa, and the gamma-ray 4.5×10 6 After the aging test with a dose of Gy, the change rate of the ion shielding performance was 0.4%. Figure 1 The device shown has a neutron shielding performance change rate of 0.6% after being immersed in 4 mol / L nitric acid at 60°C for one month.

[0037] Example 5 This embodiment includes the following steps: Step 1: Spray 150 mL of 2 mol / L KH570 ethanol dispersion solution evenly onto the surface of 3 kg of boron carbide particles with an average particle size of 15 μm and a maximum particle size of 34 μm, stir evenly and dry until the liquid component is completely volatilized to obtain surface-modified boron carbide particles; Step 2: Put the surface-modified boron carbide particles obtained in step 1, 1.43 kg of high-density polyethylene with a molecular weight of 50,000 and a melt index of 25 g / 10 min, and 0.5 kg of maleic anhydride grafted polyethylene with a grafting rate of 0.8% into a high-speed mixer and mix them evenly for 10 minutes to obtain a mixture; Step 3: The mixed material obtained in step 2 is put into a parallel twin-screw extruder for melt extrusion granulation, and the extrusion temperature is 200°C, the screw speed is 15r / min, and air-cooled granulation is performed to prepare B 4 C / HDPE shielding masterbatch; 4 C / HDPE shielding masterbatch includes, by mass percentage: 60% boron carbide particles, 28.5% high-density polyethylene, 10% maleic anhydride grafted polyethylene, 1.5% coupling agent KH570, and the B 4 The particle size of C / HDPE shielding masterbatch is 3.0mm±0.5mm; Step 4: 3 kg of B obtained in step 3 4 C / HDPE shielding masterbatch is mixed with 14.61kg ultra-high molecular weight polyethylene with a viscosity average molecular weight of 8 million, 120g antioxidant Irganox 168, 120g ultraviolet absorber UV-944 and 530g nucleating agent nano-silicon dioxide, and produced by a compression molding process. The process parameters of the compression molding are: molding temperature 240°C, molding pressure 60MPa, pressure-maintaining cooling after cooling, and machining to obtain a boron-containing polyethylene shielding material sheet; the boron-containing polyethylene shielding material sheet includes, by mass percentage: ultra-high molecular weight polyethylene 79.49%, B 4 C / HDPE shielding masterbatch 16.32%, antioxidant Irganox 168 0.65%, UV absorber UV-944 0.65%, nucleating agent nano-silica 2.88%.

[0038] After testing, the deviation value of the mass content of boron carbide in the boron-containing polyethylene shielding material sheet prepared in this embodiment is 0.26%, the tensile strength of the boron-containing polyethylene shielding material sheet is 26.84MPa, the elongation at break is 194.73%, the bending strength is 22.04MPa, and the gamma-ray 4.5×10 6 After the aging test with a dose of Gy, the change rate of the neutron shielding performance was 0.5%. Figure 1 The device shown has a neutron shielding performance change rate of 0.7% after being immersed in 4 mol / L nitric acid at 60°C for one month.

[0039] Comparative Example 1 The difference between this comparative example and Example 1 is that the boron carbide particles are not subjected to surface treatment and masterbatch preparation process, and 4 kg of boron carbide particles with an average particle size of 20 μm and a maximum particle size of 48 μm, 5.53 kg of high-density polyethylene with a molecular weight of 50,000 and a melt index of 25 g / 10 min, 0.33 kg of maleic anhydride grafted polyethylene with a grafting rate of 0.5%, 10.58 kg of ultra-high molecular weight polyethylene with a viscosity-average molecular weight of 3 million, 70 g of antioxidant Irganox 1010, 70 g of ultraviolet absorber UV-329 and 280 g of nucleating agent calcium stearate are directly selected and mixed, and a single-screw extruder is used for extrusion molding, and the process parameters are: 130° C. for the feeding section, 210° C. for the plasticizing and melting section, 220° C. for the die molding temperature, 50 mm / h for the extrusion speed, and 6 Hz for the screw speed. The boron-containing polyethylene shielding material rod is obtained by machining.

[0040] Comparative Example 2 The difference between this comparative example and Example 1 is that in step 4, high-density polyethylene with a molecular weight of 125,000 and a melt index of 10 g / 10 min is used to replace ultra-high molecular weight polyethylene with a viscosity-average molecular weight of 4 million to prepare boron-containing polyethylene shielding material rods.

[0041] Comparative Example 3 The difference between this comparative example and Example 1 is that in step 4, 5 kg of B obtained in step 3 is added 4 C / HDPE shielding masterbatch was mixed with 10.58kg ultra-high molecular weight polyethylene with a viscosity average molecular weight of 3 million, 70g antioxidant Irganox 1010, 70g ultraviolet absorber UV-9329 and 280g nucleating agent calcium stearate, and extruded by a single screw extruder. The process parameters were as follows: feeding section 130°C, plasticizing and melting section 210°C, die head molding temperature 220°C, extrusion speed 50mm / h, screw speed 6Hz, and the boron-containing polyethylene shielding material rod was obtained by machining; the boron-containing polyethylene shielding material rod included, by mass percentage: ultra-high molecular weight polyethylene 66.13%, B 4 C / HDPE shielding masterbatch 31.25%, antioxidant Irganox 1010 0.44%, UV absorber UV-329 0.44%, nucleating agent calcium stearate 1.75%.

[0042] Comparative Example 4 The difference between this comparative example and Example 1 is that the high-density polyethylene used in step 2 has a molecular weight of 10,000 and a melt index of 40 g / 10 min, and the viscosity-average molecular weight of the ultra-high molecular weight polyethylene used in step 4 is 1.5 million.

[0043] Comparative Example 5 The difference between this comparative example and Example 1 is that the high-density polyethylene used in step 2 has a molecular weight of 500,000 and a melt index of 2.4 g / 10 min, and the viscosity-average molecular weight of the ultra-high molecular weight polyethylene used in step 4 is 10 million.

[0044] Comparative Example 6 The difference between this comparative example and Example 1 is that the molecular weight of the high-density polyethylene used in step 2 is 125,000 and the melt index is 14 g / 10 min, and the viscosity-average molecular weight of the ultra-high molecular weight polyethylene used in step 4 is 10 million.

[0045] Comparative Example 7 This comparative example comprises the following steps: Step 1: Spray 175 mL of 3 mol / L KH570 ethanol dispersion solution evenly onto the surface of 4 kg of boron carbide particles with an average particle size of 20 μm and a maximum particle size of 48 μm, stir evenly and dry until the liquid component is completely volatilized to obtain surface-modified boron carbide particles; Step 2: The surface-modified boron carbide particles obtained in step 1 are mixed evenly with 5.53 kg of high-density polyethylene with a molecular weight of 50,000 and a melt index of 25 g / 10 min, 0.33 kg of maleic anhydride grafted polyethylene with a grafting rate of 0.5%, 10.58 kg of ultra-high molecular weight polyethylene with a viscosity-average molecular weight of 3 million, 70 g of antioxidant Irganox 1010, 70 g of ultraviolet absorber UV-329 and 280 g of nucleating agent calcium stearate, and extruded by a single-screw extruder. The process parameters are: 130°C for the feeding section, 210°C for the plasticizing and melting section, 220°C for the die molding temperature, 50 mm / h for the extrusion speed, and 6 Hz for the screw speed. The boron-containing polyethylene shielding rod is obtained by machining.

[0046] Comparative Example 8 The difference between this comparative example and Example 1 is that maleic anhydride grafted polyethylene is omitted in step 2.

[0047] Comparative Example 9 The difference between this comparative example and Example 1 is that the grafting rate of maleic anhydride grafted polyethylene in step 2 is 0.2%.

[0048] Comparative Example 10 The difference between this comparative example and Example 1 is that the grafting rate of maleic anhydride grafted polyethylene in step 2 is 2.0%.

[0049] The boron carbide content deviation, mechanical properties including tensile strength, elongation at break, bending strength and neutron shielding performance of the boron-containing polyethylene shielding material profiles prepared in Examples 1 to 5 of the present invention and Comparative Examples 1 to 10 were tested. The test results are shown in Tables 1 and 2 below. Figure 2As shown, the mechanical properties test is carried out in accordance with GB / T 1040.2 "Determination of tensile properties of plastics Part 2 Test conditions for molded and extruded plastics" and GB / T 9341 "Test method for bending properties of plastics". The boron carbide content deviation and neutron shielding performance test methods are as follows: (1) Boron carbide content deviation test: Randomly select 7 to 9 positions on the surface of the boron-containing polyethylene shielding material per unit area (10 cm × 10 cm) and take samples. Then, refer to the method specified in EJ / T 20077-2014 "Specification for Lead Boron Polyethylene Sheet" to test the boron carbide content. The difference between the maximum and minimum boron carbide content detected per unit area is taken as the boron carbide content deviation.

[0050] (2) Neutron shielding performance test: Take a 20 mm thick disc at any position of the boron-containing polyethylene shielding material rod, and then test the neutron shielding performance according to the method specified in the corporate standard Q / CYSXY0009-2022 "Determination of Attenuation Performance of Neutron Radiation Shielding Materials" of Beijing Radiation Application Research Center Co., Ltd.

[0051]

[0052] As shown in Table 1, by comparing Example 1 with Comparative Examples 1, 4, 5, 6, and 7, it can be seen that the HDPE raw material with a specified molecular weight and the modified B 4 Preparation of B with C granules 4 C / HDPE shielding masterbatch can effectively improve B 4 The uniformity of the dispersion of C particles in the ultra-high molecular weight polyethylene matrix reduces the 4 C content deviation (wherein the maximum deviation of boron carbide content in comparative example 7 is 1.58%), and improves the mechanical properties of boron-containing polyethylene shielding materials.

[0053] By comparing Example 1 with Comparative Examples 1, 2, and 7, it can be seen that B 4 C particles were surface modified and prepared by 4 C / HDPE shielding masterbatch can achieve good dispersion effect in ultra-high molecular weight polyethylene materials, such as Figure 3 , 4 As shown, the dispersion effect of comparative example 7 without preparing shielding masterbatch and directly blending boron carbide modified is as follows Figure 5 As shown, from Figure 5 It can be seen that the particles are agglomerated and unevenly distributed. Therefore, the preparation method of the present invention can further reduce the B 4 C content deviation, while ensuring the excellent mechanical properties of the boron-containing polyethylene shielding material.

[0054] By comparing Example 1 with Comparative Examples 2, 4, 5, and 6, it can be seen that the present invention achieves B by controlling the molecular weight of high-density polyethylene to be 50,000 to 200,000 and the viscosity-average molecular weight of ultra-high molecular weight polyethylene to be 3 million to 8 million. 4 The uniform dispersion of C particles makes the mechanical properties of the boron-containing polyethylene shielding material reach the best.

[0055] By comparing Example 1 with Comparative Examples 8, 9, and 10, it can be seen that the present invention prepares B 4 The addition of maleic anhydride grafted polyethylene with a specific grafting rate in the process of C / HDPE shielding masterbatch can improve B 4 The dispersion of C particles in the matrix reduces B 4 Therefore, the grafting rate of maleic anhydride in the maleic anhydride grafted polyethylene is adjusted to 0.5% to 1.2% to obtain B 4 C effective dispersion and optimal mechanical properties.

[0056]

[0057] As can be seen from Table 2, by comparing Example 1 with Comparative Examples 1, 3, and 7, it can be seen that the neutron shielding performance of the boron-containing polyethylene shielding material prepared in Example 1 before aging is significantly higher than that of the materials prepared in Comparative Examples 1, 3, and 7. The main reason is that the neutron shielding performance of the boron-containing polyethylene shielding material prepared in Example 1 before aging is significantly higher than that of the materials prepared in Comparative Examples 1, 3, and 7. 4 Preparation of C / HDPE shielding masterbatch significantly improves B 4 The uniformity of the dispersion of C particles in the ultra-high molecular weight polyethylene matrix reduces the B 4 The deviation of C content effectively improves the neutron shielding efficiency of the material. 4 The deviation of C content will also significantly affect the change rate of the neutron shielding performance of the material before and after aging.

[0058] At the same time, it can be seen from Examples 1 to 5 that as the B 4 With the increase of C particle content, the neutron shielding efficiency of the material before aging gradually improves, and the change rate of neutron shielding performance after γ-ray irradiation aging and nitric acid immersion is lower than the relevant neutron shielding performance change rate data of the control example, which can meet the performance indicators and application requirements of neutron poison materials in the field of spent fuel reprocessing.

[0059] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a boron-containing polyethylene shielding material, characterized in that: The method comprises the following steps: Step 1, spraying the ethanol dispersion solution of the coupling agent evenly onto the surface of the boron carbide particles, stirring evenly and drying to obtain surface-modified boron carbide particles; Step 2: uniformly mixing the surface-modified boron carbide particles obtained in step 1 with high-density polyethylene and maleic anhydride grafted polyethylene to obtain a mixture; Step 3, melt-extrude the mixture into granules to prepare B4C / HDPE shielding masterbatch; Step 4: Mix the B4C / HDPE shielding masterbatch obtained in step 3 with ultra-high molecular weight polyethylene, an antioxidant, an ultraviolet absorber and a nucleating agent, and prepare a boron-containing polyethylene shielding material by extrusion molding or compression molding.

2. The method for preparing a boron-containing polyethylene shielding material according to claim 1, characterized in that: The molecular weight of the high-density polyethylene described in step 2 is 50,000 to 200,000, the melt index is 4g / 10min to 25g / 10min, the grafting rate of maleic anhydride in the maleic anhydride grafted polyethylene is 0.5% to 1.2%, and the uniform mixing time is 5min to 30min; the viscosity-average molecular weight of the ultra-high molecular weight polyethylene described in step 4 is 3 million to 8 million.

3. The method for preparing a boron-containing polyethylene shielding material according to claim 1, characterized in that: In step three, a parallel twin-screw extruder is used to melt-extrude the mixed material into pellets, and the extrusion temperature is 150° C. to 230° C., the screw speed is 5 r / min to 20 r / min, and the pellets are air-cooled.

4. The method for preparing a boron-containing polyethylene shielding material according to claim 1, characterized in that: The B4C / HDPE shielding masterbatch described in step 3 includes, by mass percentage, 40% to 65% of boron carbide particles, 28.5% to 55.3% of high-density polyethylene, 3% to 10% of maleic anhydride grafted polyethylene, and 1% to 2% of coupling agent KH570.

5. The method for preparing a boron-containing polyethylene shielding material according to claim 1, characterized in that: The average particle size of the B4C / HDPE shielding masterbatch described in step 3 is 2 mm to 4 mm.

6. The method for preparing a boron-containing polyethylene shielding material according to claim 1, characterized in that: The boron carbide particles in step 1 are nuclear grade boron carbide particles, and the average particle size of the boron carbide particles is 5 μm to 20 μm, and the maximum particle size is 15 μm to 48 μm.

7. The method for preparing a boron-containing polyethylene shielding material according to claim 1, characterized in that: The mass ratio of the B4C / HDPE shielding masterbatch to the ultra-high molecular weight polyethylene in step 4 is 1:1 to 1:

10.

8. The method for preparing a boron-containing polyethylene shielding material according to claim 1, characterized in that: The mass ratio of the high-density polyethylene in the shielding masterbatch to the added ultra-high molecular weight polyethylene is 1:1 to 1:

32.

9. The method for preparing a boron-containing polyethylene shielding material according to claim 1, characterized in that: The antioxidant in step 4 is selected from one or more of Irganox 1010, Irganox 1076, Irgafos 168 and DLTP, the ultraviolet absorber is selected from one or more of UV-944, UV-1130 and UV-329, and the nucleating agent is selected from one or more of nano-silicon dioxide, zinc stearate and calcium stearate; the extrusion molding adopts a single screw extruder, and the process parameters are: feeding section 130°C~220°C, plasticizing and melting section 180°C~290°C, head molding temperature 220°C~270°C, extrusion speed 50mm / h~120mm / h, screw speed 6Hz~10Hz, and after extrusion molding, the boron-containing polyethylene shielding material is obtained by machining; the process parameters of the compression molding in step 4 are: molding temperature 160°C~260°C, molding pressure 30MPa~120MPa, pressure cooling after cooling, and the boron-containing polyethylene shielding material is obtained after machining.

10. The method for preparing a boron-containing polyethylene shielding material according to claim 1, characterized in that: The boron-containing polyethylene shielding material in step 4 includes, by mass percentage, 50% to 90% ultra-high molecular weight polyethylene, 9% to 48% B4C / HDPE shielding masterbatch, 0.1% to 2% antioxidant, 0.1% to 1% UV absorber, and 0.8% to 3% nucleating agent.

Citation Information

Cited By

  • Neutron shielding equipment and SER test system

    CN120748793A

  • Medical cyclotron radiation shielding performance detection method and device

    CN121633135A