Multifunctional inorganic carbon sequestration coating as well as preparation method and coating of multifunctional inorganic carbon sequestration coating
By incorporating multiphase minerals and modified silica sols into inorganic carbon-solid coatings, the problem of insufficient wear resistance and scrubbing resistance of gamma-type dicalcium silicate coatings is solved, and the wear resistance and solar radiation of the coating are improved The reflection effect enhances the bonding strength and achieves efficient passive cooling of buildings.
Patent Information
- Application Number
- CN202411032909.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-30
AI Technical Summary
The existing inorganic carbon-solid coatings with gamma-type dicalcium silicate as the main bonding component have poor performance in wear resistance and scrubbing resistance, and the bonding strength is not high, resulting in the coating being easily powdered during long-term use. and fall off.
Carbon-cured composite materials of heterogeneous minerals are prepared by incorporating calcium, silicon, aluminum and titanium raw materials, and combined with modified silicon sol and organic emulsion to form a multifunctional inorganic carbon-solid coating, using heterogeneous minerals Improve the wear resistance and solar radiation reflection effect of the coating, and introduce modified silicon sols and organic emulsions to enhance the cohesion and bonding strength of the coating.
It significantly improves the wear resistance, scrubbing resistance and solar radiation reflection effect of the inorganic carbon solid coating, enhances the bonding strength, extends the service life of the coating, and realizes the passive cooling effect of the building.
Smart Images

Figure CN118994946A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, and in particular to a multifunctional inorganic carbon-fixing coating and a preparation method and coating thereof. Background Art
[0002] Water-based inorganic coatings are environmentally friendly coatings. Compared with traditional organic coatings, they have the advantages of low VOC content, low flammability, and environmental friendliness. However, the water-based inorganic coatings currently on the market still have defects in some performance aspects, which limits their widespread application. Specifically, coatings with silicate (mainly sodium silicate and lithium silicate) aqueous solution as inorganic film-forming material have poor water resistance. This is because the silicate aqueous solution is easy to redissolve in an environment with moisture, resulting in the degradation of the coating. At the same time, this also leads to the phenomenon that the coating is easy to wipe off after drying, thereby reducing the adhesion and wear resistance of the coating. On the other hand, inorganic coatings with silica sol as the main film-forming material perform better in water resistance, which is attributed to the cross-linked network structure formed by silica sol particles during the curing process, which can effectively block the penetration of moisture. However, the curing process of this coating is accompanied by significant volume shrinkage, which is easy to cause cracking of the coating. Finally, the above two coatings need to be cured by contact with CO in the air. 2 Reaction occurs, so there is a problem of long curing time.
[0003] Among the calcium silicate mineral phases, γ-type dicalcium silicate is considered to be a major bonding component of a new type of water-based inorganic coating due to its high carbonization activity and high mechanical strength after curing. 2 During the curing process, amorphous silica gel (binder) with high polymerization degree and insoluble calcium carbonate are generated in situ. There is a certain amount of system expansion during the curing process, so the porosity gradually decreases, which can effectively reduce water penetration. Therefore, the inorganic coating with γ-type dicalcium silicate as the main component has more obvious advantages than the two inorganic coatings mentioned above.
[0004] At present, patents CN202110166883.3 and CN202210323347.4 both use γ-type dicalcium silicate as the main bonding component of the coating, and pressurized CO at a gas pressure of 0.1 to 0.6 MPa 2Carbonization was carried out under the environment to obtain different functionalized coatings. However, due to the presence of a large amount of calcium carbonate and a low content of silica gel in the cured product, the coating has the problem of poor wear resistance and scrubbing resistance. Under long-term service conditions, the above coating will inevitably lose powder and fall off. At the same time, CN202210323347.4 uses a solar radiation reflector with high solar radiation reflection ability to improve the radiation cooling effect of the coating, but the solar radiation reflector needs to be modified in the preparation process, and the adhesion between the interfaces of each phase in the coating is low, and the final adhesion strength of the coating is relatively low. Therefore, improving the functional effect of the inorganic carbon-fixing coating by adding functional materials will inevitably cause the problem of decreased cohesion of the coating. Summary of the invention
[0005] The purpose of the present invention is to overcome the above technical deficiencies, provide a multifunctional inorganic carbon-fixing coating and its preparation method and coating, and solve the technical problems in the prior art that the inorganic carbon-fixing coating with γ-type dicalcium silicate as the main bonding component has poor wear resistance and scrubbing resistance and low bonding strength.
[0006] In order to achieve the above technical purpose, the technical solution provided by the present invention is: In a first aspect, the present invention provides a multifunctional inorganic carbon-fixing coating, wherein the raw materials include 70 to 140 parts by weight of a carbon-cured composite material, 14 to 100 parts by weight of deionized water, 10 to 70 parts by weight of a modified silica sol, and 1 to 14 parts by weight of an organic emulsion; wherein the carbon-cured composite material is obtained by mixing a calcium raw material, a silicon raw material, an aluminum raw material, and a titanium raw material and subjecting the mixture to a calcination treatment.
[0007] In a second aspect, the present invention provides a method for preparing a multifunctional inorganic carbon-fixing coating, comprising the following steps: uniformly mixing deionized water and an organic emulsion by ultrasonic mixing, during which time modified silica sol is slowly added dropwise to obtain a mixed solution; and then adding a carbon-cured composite material to the mixed solution, and mixing uniformly to obtain an inorganic carbon-fixing coating.
[0008] In a third aspect, the present invention provides a multifunctional inorganic carbon-fixing coating, wherein the inorganic carbon-fixing coating is coated on the surface of a substrate and then placed in a CO 2 Formed by maintenance in the environment.
[0009] Compared with the prior art, the beneficial effects of the present invention include: The present invention prepares γ-C by adding calcium raw materials, silicon raw materials, aluminum raw materials and titanium raw materials. 2 S and other multiphase mineral carbon-cured composite materials, and then with modified silica sol and organic emulsion to make inorganic carbon-fixing coatings. The multiphase minerals in the carbon-cured composite materials are conducive to improving wear resistance and effectively improving the single γ-C 2The problem of poor wear resistance and scrub resistance of S mineral carbonized coating is solved; at the same time, the multiphase mineral has a high bandgap width and a high refractive index, so that the obtained inorganic carbon-fixing coating has excellent visible light radiation reflection effect and long-wave mid-infrared transparent window emission effect; the introduced modified silica sol and the organic emulsion that can produce an organic cross-linked network fully play the role of the cross-linked network, synergistically improve the cohesion of the coating, and enhance the scrub resistance and bonding strength of the coating; therefore, the inorganic carbon-fixing coating prepared by the coating of the present invention has excellent wear resistance, scrub resistance and solar radiation reflection effect, and high bonding strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figure 1 is a backscattered image of the inorganic carbon-fixing coating prepared in Example 1 of the present invention; Figure 2 This is a backscattered image of the inorganic carbon-fixing coating prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0011] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0012] In order to solve the problem that the inorganic carbon-fixing coating with gamma-type dicalcium silicate as the main bonding component has poor wear resistance and scrubbing resistance, and at the same time give the coating more functional effects, the present invention provides a multifunctional inorganic carbon-fixing coating that can be quickly cured and a preparation method thereof, wherein a gamma-type dicalcium silicate (γ-C 2 S) as the main component of the carbon-solidified composite material, and by adding different coating additives, an inorganic carbon-fixing coating with multiple functionalities is finally obtained.
[0013] In a first aspect, the present invention provides a multifunctional inorganic carbon-fixing coating, wherein the raw materials include 70 to 140 parts of carbon-cured composite material, 14 to 100 parts of deionized water, 10 to 70 parts of modified silica sol, and 1 to 14 parts of organic emulsion, by weight; The carbon-solidified composite material is obtained by mixing calcium raw materials, silicon raw materials, aluminum raw materials and titanium raw materials and then calcining them.
[0014] Preferably, the preparation method of the carbon-solidified composite material specifically comprises: wet mixing a calcium raw material, a silicon raw material, an aluminum raw material and a titanium raw material in proportion for 0.5 to 2 hours and then drying, placing the raw material in a high-temperature furnace for calcination after drying, and placing the calcined clinker in a high-energy ball mill for dry grinding for 0.5 hours to 1 hour to finally obtain a carbon-solidified composite material containing multiphase minerals, wherein the multiphase minerals include γ-C 2 S, Ca 2 Al2 SiO 7 , Ca 2 Ti 1-x Si x O 4 and CaTiO 3 . During the wet mixing process, the mass ratio of powder to water is 1: (1.1-1.3), and more preferably 1: 1.2. The purpose of wet mixing is to mix the phases evenly and reduce the distance between particles, which is convenient for subsequent firing. Direct dry mixing cannot reduce the distance between particles. The dry grinding step mainly grinds the carbon-cured composite material obtained by firing to a particle size range of 0.4μm to 70μm. Within this particle size range, the coating prepared from the carbon-cured composite material has the maximum degree of carbon curing.
[0015] Preferably, the calcium raw material comprises Ca(OH) 2 Siliceous raw materials include SiO 2 , aluminum raw materials include Al 2 O 3 , titanium raw materials include TiO 2 .
[0016] Preferably, the purity of the calcium raw material is above 92%, the purity of the silicon raw material is above 95%, and the remaining impurities include MgO, BaO, SrO, ZrO 2 , Li 2 O、Na 2 O.K 2 O.B 2 O 3 、ZnO、Cs 2 O.P 2 O 5 ; The purity of aluminum raw materials and titanium raw materials is above 99%; The particle sizes of calcium raw materials, silicon raw materials, aluminum raw materials and titanium raw materials are all between 0.1μm and 500μm. Aluminum raw materials and titanium raw materials are used to provide functionalization.
[0017] Preferably, in the carbon-cured composite material, the calcium raw material, silicon raw material, aluminum raw material and titanium raw material are prepared in the following molar ratio: Ca / Si=3.3-1.2, Al / Si<2, Ti / Si<1. Among them, too much or too little calcium-silicon ratio will lead to the γ-C 2 If the S content is low and the aluminum-silicon ratio and titanium-silicon ratio are not within the range, other aluminum- and titanium-containing silicate mineral phases will be generated.
[0018] More preferably, Ca / Si=3.3-2.0, Al / Si=0.07-0.95, and Ti / Si=0.03-0.82.
[0019] Preferably, the calcination treatment method is: calcining the raw materials in a box furnace, with the calcination temperature being 1250 - 1400 °C and the calcination time being 30 - 180 min. Among them, too low a calcination temperature and too short a calcination time will result in too high free calcium oxide in the carbon solidified composite material, while too high a temperature or too long a calcination time will lead to a decrease in the γ-C 2 S content.
[0020] Preferably, the finally obtained carbon solidified composite material contains multiphase minerals. By mass percentage, the multiphase minerals include 30 - 55 wt% of γ-C 2 S, and the rest is Ca 2 Al 2 SiO 7 、Ca 2 Ti 1-x Si x O 4 and the sum of CaTiO 3 Preferably, the multiphase minerals include 30 - 55 wt% of γ-C 2 S, 2 - 45% of Ca 2 Al 2 SiO 7 、6 - 35% of Ca 2 Ti 1-x Si x O 4 and 2 - 20% of CaTiO 3 , where 0 < x < 1; and the ratio of the content of Ca 2 Al 2 SiO 7 to the content of Ca 2 Ti 1-x Si x O 4 +CaTiO 3 is in the range of 0.03 - 5.5. Specifically, under the same other conditions, the relative contents of Ca 2 Al 2 SiO 7 、Ca 2 Ti 1-x Si x O 4 and CaTiO 3 are determined according to the requirements of the multifunctional inorganic carbon fixation coating. Ca 2 Al 2 SiO 7 is more conducive to improving the scrub resistance, and Ca 2 Ti 1-x Si x O 4 +CaTiO 3It is more conducive to synergistically improving the reflectivity. The present invention controls the mineral phase composition through the raw material ratio and the firing system. For the coating with the main demand of high brush resistance, Ca 2 Al 2 SiO 7 The content of Ca 2 Ti 1-x Si x O 4 +CaTiO 3 The content ratio is between 5.5 and 1. For coatings that mainly require high solar radiation 4 reflection ability, Ca 2 Al 2 SiO 7 The content of Ca 2 Ti 1-x Si x O 4 +CaTiO 3 The content ratio is between 0.03 and 1.
[0021] It should be noted here that Ca 2 Ti 1-x Si x O 4 Probably due to Ca 2 Ti 0.24 Si 0.76 O 4 , Ca 2 Ti 0.1 Si 0.9 O 4 , Ca 2 Ti 0.06 Si 0.94 O 4 A mixture of multiple crystals. These crystals cannot be clearly distinguished by XRD and have little difference in actual properties, so they are abbreviated as Ca 2 Ti 1-x Si x O 4 , 0 <x<1。
[0022] Preferably, the preparation steps of the modified silica sol include: dissolving chitosan in an acetic acid solution with a mass concentration of 1% to obtain a chitosan solution; then adding the chitosan solution to the silica sol, adjusting the pH value to 8.5-9.5, stirring evenly and aging for more than 24 hours to obtain a modified silica sol; wherein the mass ratio of the acetic acid solution to chitosan is 100: (4-6), and the mass ratio of the silica sol to the chitosan solution is 100: (8-12). The modified silica sol of the present invention is modified by organic hybridization, so that it can protect the inorganic silica sol under alkaline conditions and inhibit agglomeration.
[0023] Preferably, the solid content of the modified silica sol is 33±5%.
[0024] Preferably, the organic emulsion includes a mixture of one or more of acrylate emulsion, styrene-acrylic emulsion, pure acrylic emulsion, epoxy resin emulsion, EVA emulsion and silicone-acrylic emulsion in any proportion; the solid content of the organic emulsion is 40-50%.
[0025] Further preferably, the solid content of the organic emulsion is 45%.
[0026] In a second aspect, the present invention provides a method for preparing a multifunctional inorganic carbon-fixing coating, comprising the following steps: The deionized water and the organic emulsion are uniformly mixed by ultrasonication, and the modified silica sol is slowly added dropwise during the process to obtain a mixed solution; Then the carbon-solidified composite material is added into the mixed solution and mixed evenly to obtain the inorganic carbon-solidified coating.
[0027] Preferably, the deionized water and the organic emulsion are uniformly mixed by ultrasonication for 15 to 25 minutes; the carbon-cured composite material is added to the mixed solution and dispersed at a speed of 2500 to 3500 r / min for 0.5 to 1.5 hours to be uniformly mixed.
[0028] In a third aspect, the present invention provides a multifunctional inorganic carbon-fixing coating, which is an inorganic carbon-fixing coating applied to the surface of a substrate and then placed in a CO-rich 2 The coating is cured in an organic carbon-fixing environment to form a multifunctional inorganic carbon-fixing coating.
[0029] Preferably, the substrate comprises a concrete building base or a steel structure after surface silanization treatment.
[0030] Preferably, the coating is carried out by spraying, rolling or pressing; the coating thickness is 0.3 to 3 mm.
[0031] Preferably, the maintenance system is: CO 2 The concentration is 5% to 100%, CO 2 The partial pressure is 0.01MPa to 7.4MPa, and the carbonization time is 0.1 to 72h. In the present invention, the curing method can be CO 2 Jet curing can also be film-coated aeration curing. For prefabricated components, pressurized curing can be carried out in the reaction tank, and others can be cured at normal pressure.
[0032] The main mechanism of action and advantages of the present invention are: (1) The present invention prepares γ-C by sintering 2 S process, a certain mass percentage of Al is added 2 O 3 and TiO 2Functional raw materials such as γ-C 2 The S content is low, and too little addition will result in the carbon-cured composite material not being able to achieve the best functional effect. By optimizing the firing system, gamma-type dicalcium silicate (γ-C 2 S) as the main component, and also contains Ca 2 Al 2 SiO 7 , Ca 2 Ti 1-x Si x O 4 and CaTiO 3 Carbon-solidified composite materials of minerals such as Ca 2 Al 2 SiO 7 Mohs hardness is 6.5, CaTiO 3 Mohs hardness is 6, compared to γ-C 2 S (Mohs hardness is 5) and its carburization product CaCO 3 (Mohs hardness is 3) has higher wear resistance. By using this multiphase mineral to prepare an inorganic carbon-fixing coating, the single γ-C 2 The problem of poor wear resistance and scrubbing resistance of S mineral carbide coating; (2) The present invention incorporates Al 2 O 3 or TiO 2 , so that the final carbon-cured composite material contains a part of Ca 2 Al 2 SiO 7 , Ca 2 Ti 1-x Si x O 4 and CaTiO 3 These substances and the carbonization product CaCO 3 They all have a high bandgap and a high refractive index. This makes the inorganic carbon-fixing coating prepared using this multiphase mineral have excellent visible light radiation reflection effect and long-wave mid-infrared transparent window emission effect. The coating is applied to concrete buildings and steel structures with high radiation cooling efficiency; (3) The present invention adopts the method of 2 During the preparation of S, different functionalized mineral phases are added, and the firing system is optimized. Finally, a variety of functionalized carbon-solidified composite materials can be obtained only by firing. Secondly, by adding coating additives and appropriate coating preparation processes, multifunctional inorganic carbon-fixing coatings can be obtained. 2S mineral carbon-fixing coating and carbon-fixing coating obtained by mechanical mixing have better carbonization reaction activity and system compatibility.
[0033] In order to make the purpose, technology / solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0034] To avoid redundancy, the main raw materials are described here. Among the raw materials of carbon-cured composite materials, the calcium raw material is Ca(OH) 2 , the siliceous raw material is SiO 2 , aluminum raw material is Al 2 O 3 , titanium raw material is TiO 2 ; Among the raw materials of the inorganic carbon-fixing coating, the silica sol uses S309 from Shanghai Xinshou Additive Co., Ltd.; the modified silica sol is an organic hybrid modified silica sol with a solid content of 33%. The specific preparation steps of the organic hybrid modified silica sol include: dissolving chitosan powder in a 1% acetic acid solution, stirring continuously at a speed of 300 rpm / s for 20 minutes to prepare a 5% concentration chitosan solution, and then slowly adding a 10% chitosan solution to the silica sol, during which the pH value of the mixed system is adjusted to about 9 with ammonia water, and stirring continuously at a speed of 300 rpm / s for 1 hour to fully mix the two, and then aging for 1 day; The solid content of the organic emulsions is 45%.
[0035] In each embodiment and comparative example, the preparation method of the inorganic carbon fixing coating includes the following steps: ultrasonically mixing deionized water and an organic emulsion for 20 minutes, during which the modified silica sol is slowly added; then the carbon-cured composite material is added to the mixed solution three times, and after the previous portion of the carbon-cured composite material is added, stirring is continued for 5 minutes before adding the next portion, and high-speed dispersion is performed at a speed of 3000 r / min for 1 hour to finally prepare the inorganic carbon fixing coating.
[0036] Example 1 The inorganic carbon-fixing coating composition of this embodiment includes: 85 parts of carbon-cured composite material, 14 parts of deionized water, 35 parts of modified silica sol and 7 parts of organic emulsion (styrene-acrylic emulsion).
[0037] The proportion of ingredients in the process of preparing raw materials for carbon-cured composite materials is Ca / Si=2.1, Al / Si=0.72, Ti / Si=0.08, respectively. After wet mixing for 2 hours, it is dried and calcined. The calcination temperature is 1400℃, the calcination time is 3 hours, and then dry-grinded for 0.5 hours to obtain a carbon-cured composite material. The mineral composition (by mass percentage) tested by XRD is: 51% γ-C 2 S, 33% Ca 2 Al 2 SiO 7 、10%Ca 2 Ti 1-x Si x O 4 and 6%CaTiO 3 .
[0038] The inorganic carbon-fixing coating was sprayed on the concrete substrate with a coating thickness of 0.3 mm. 100% concentration of CO 2 Gas, after carbonization and curing for 20 minutes under normal pressure, a multifunctional inorganic carbon-fixing coating was obtained.
[0039] Example 2 The inorganic carbon-fixing coating composition of this embodiment includes: 100 parts of carbon-cured composite material, 28 parts of deionized water, 48 parts of modified silica sol and 10 parts of organic emulsion; the organic emulsion is a combination of epoxy resin emulsion (solid content of 45%) and acrylate emulsion (solid content of 45%), with a mass ratio of 1:2.
[0040] The proportion of ingredients in the process of preparing raw materials for carbon-cured composite materials is Ca / Si=2.4, Al / Si=0.58, Ti / Si=0.28, respectively. After wet mixing for 2 hours, it is dried and calcined. The calcination temperature is 1350℃, the calcination time is 3 hours, and then dry-grinded for 1 hour to obtain a carbon-cured composite material. The mineral composition of the composite material is 45% γ-C tested by XRD. 2 S, 23% Ca 2 Al 2 SiO 7 , 20%Ca 2 Ti 1-x Si x O 4 and 12%CaTiO 3 .
[0041] The inorganic carbon-fixing coating was sprayed on the concrete substrate with a coating thickness of 1 mm. A 60% concentration of CO 2 Gas, after carbonization and curing for 2 hours under normal pressure, a multifunctional inorganic carbon-fixing coating is obtained.
[0042] Example 3 The inorganic carbon-fixing coating composition of this embodiment includes: 70 parts of carbon-cured composite material, 35 parts of deionized water, 40 parts of modified silica sol and 4 parts of organic emulsion; the organic emulsion is a combination of styrene-acrylic emulsion and acrylate emulsion (both with a solid content of 45%), with a mass ratio of 2:3.
[0043] The proportion of ingredients in the process of preparing raw materials for carbon-cured composite materials is Ca / Si=2.2, Al / Si=0.95, Ti / Si=0.16 respectively. After wet mixing for 1 hour, it is dried and calcined. The calcination temperature is 1325℃, the calcination time is 2 hours, and then dry-grinded for 1 hour to obtain a carbon-cured composite material. The mineral composition of the composite material is as follows: 40% γ-C 2 S, 45% Ca 2 Al 2 SiO 7 、15%Ca 2 Ti 1-x Si x O 4 and 10%CaTiO 3 .
[0044] The inorganic carbon-fixing coating was sprayed on the concrete substrate with a coating thickness of 0.5 mm. 20% concentration of CO 2 Gas, after carbonization and curing for 24 hours under normal pressure, a multifunctional inorganic carbon-fixing coating is obtained.
[0045] Example 4 The inorganic carbon-fixing coating composition of this embodiment includes: 97 parts of carbon-cured composite material, 38 parts of deionized water, 70 parts of modified silica sol and 12 parts of organic emulsion; the organic emulsion is a combination of pure acrylic emulsion and epoxy resin emulsion (both with a solid content of 45%), with a mass ratio of 1:1.
[0046] The proportion of ingredients in the process of preparing raw materials for carbon-cured composite materials is Ca / Si=2.2, Al / Si=0.24, Ti / Si=0.21 respectively. After wet mixing for 1 hour, it is dried and calcined. The calcination temperature is 1350℃, the calcination time is 3 hours, and then dry-grinded for 0.5 hours to obtain a carbon-cured composite material. The mineral composition of the XRD test is: 42% γ-C 2 S, 10% Ca 2 Al 2 SiO 7 , 33%Ca 2 Ti 1-x Si x O 4 and 15%CaTiO 3 .
[0047] The inorganic carbon-fixing coating was sprayed on the concrete substrate with a coating thickness of 0.5 mm. 100% concentration of CO 2 Gas, after carbonization and curing for 12 hours under normal pressure, a multifunctional inorganic carbon-fixing coating was obtained.
[0048] Example 5 The inorganic carbon-fixing coating composition of this embodiment includes: 88 parts of carbon-cured composite material, 63 parts of deionized water, 39 parts of modified silica sol and 8 parts of organic emulsion; the organic emulsion is a combination of styrene-acrylic emulsion and pure acrylic emulsion (both with a solid content of 45%), with a mass ratio of 1:1.
[0049] The proportion of ingredients in the process of preparing raw materials for carbon-cured composite materials is Ca / Si=2.0, Al / Si=0.87, Ti / Si=0.03 respectively. After wet mixing for 2 hours, it is dried and calcined. The calcination temperature is 1400℃, the calcination time is 2 hours, and then dry-grinded for 1 hour to obtain a carbon-cured composite material. The mineral composition of the composite material is as follows: 50% γ-C 2 S, 42% Ca 2 Al 2 SiO 7 , 6%Ca 2 Ti 1-x Si x O 4 and 2%CaTiO 3 .
[0050] The inorganic carbon-fixing coating was sprayed on the concrete substrate with a coating thickness of 0.4 mm. 100% concentration of CO 2 After carbonization and curing for 8 hours under a 0.1MPa environment, a multifunctional inorganic carbon-fixing coating was obtained.
[0051] Example 6 The inorganic carbon-fixing coating composition of this embodiment includes: 120 parts of carbon-cured composite material, 40 parts of deionized water, 58 parts of modified silica sol and 14 parts of organic emulsion; the organic emulsion is a combination of epoxy resin emulsion and EVA emulsion (both with a solid content of 45%), with a mass ratio of 2:1.
[0052] The proportion of ingredients in the process of preparing raw materials for carbon-cured composite materials is Ca / Si=2.6, Al / Si=0.58, Ti / Si=0.39, respectively. After wet mixing for 2 hours, it is dried and calcined. The calcination temperature is 1400℃, the calcination time is 2 hours, and then dry-grinded for 1 hour to obtain a carbon-cured composite material. The mineral composition of the XRD test is: 41% γ-C 2 S, 21% Ca 2 Al 2 SiO 7 , 22%Ca2 Ti 1-x Si x O 4 and 16%CaTiO 3 .
[0053] The inorganic carbon-fixing coating was sprayed on the silanized steel structure substrate with a coating thickness of 1.5 mm. 100% concentration of CO was introduced. 2 Gas, after carbonization and curing for 24 hours under normal pressure, a multifunctional inorganic carbon-fixing coating is obtained.
[0054] Example 7 The inorganic carbon-fixing coating composition of this embodiment includes: 105 parts of carbon-cured composite material, 50 parts of deionized water, 26 parts of modified silica sol and 7 parts of organic emulsion; the organic emulsion is epoxy resin emulsion, and the solid content is 45%.
[0055] The proportion of ingredients in the process of preparing raw materials for carbon-cured composite materials is Ca / Si=3.3, Al / Si=0.07, Ti / Si=0.82 respectively. After wet mixing for 1 hour, it is dried and calcined. The calcination temperature is 1350℃, the calcination time is 3 hours, and then dry-grinded for 0.5 hours to obtain a carbon-cured composite material. The mineral composition of the composite material is 43% γ-C tested by XRD. 2 S, 2% Ca 2 Al 2 SiO 7 , 35%Ca 2 Ti 1-x Si x O 4 and 20%CaTiO 3 .
[0056] The inorganic carbon-fixing coating was sprayed on the silanized steel structure substrate with a coating thickness of 1.8 mm. 100% concentration of CO was introduced. 2 Gas, after carbonization and curing for 24 hours in a 0.1MPa environment, a multifunctional inorganic carbon-fixing coating was obtained.
[0057] Comparative Example 1 An inorganic carbon-fixing coating, which differs from Example 1 only in that the carbon-fixing composite material is obtained by mechanical mixing, and the other steps and conditions are the same as those of Example 1; the difference is that: The raw material ratio of carbon-cured composite materials is based on a molar ratio of Ca / Si=2.0. After wet mixing for 2 hours, it is dried and calcined at a temperature of 1400°C for 3 hours. After that, Ca is added according to calculation. 2 Al 2 SiO 7 、CaTiO 3 and Ca2 Ti 1-x Si x O 4 After mechanical mixing for 2 hours and dry grinding for 0.5 hours, the final product, calculated by mass percentage, includes: 51% γ-C 2 S, 33% Ca 2 Al 2 SiO 7 、10%Ca 2 Ti 1-x Si x O 4 and 6%CaTiO 3 .
[0058] Comparative Example 2 An inorganic carbon-fixing coating, which differs from Example 1 only in that the carbon-fixing composite material is replaced with the same amount of γ-C 2 S, other steps and conditions are the same as in Example 1.
[0059] Comparative Example 3 An inorganic carbon-fixing coating, which differs from Example 1 only in that the inorganic carbon-fixing coating comprises: 85 parts of carbon-cured composite material and 14 parts of deionized water; other steps and conditions are the same as those in Example 1.
[0060] Comparative Example 4 An inorganic carbon-fixing coating, which differs from Example 1 only in that when preparing the carbon-fixing composite material, the Al 2 O 3 , other steps and conditions are the same as in Example 1.
[0061] Comparative Example 5 An inorganic carbon-fixing coating, which differs from Example 1 only in that when preparing the carbon-fixing composite material, the TiO 2 , other steps and conditions are the same as in Example 1.
[0062] Evaluation Test The above embodiments and comparative examples are dispersed in the same system according to the corresponding proportions, and applied to the corresponding plates, and carbonization curing is carried out at room temperature for the corresponding time and system according to the corresponding carbonization curing system. After the curing, the scrub resistance test is carried out according to the GB / T 9266 standard; the solar reflectance, near-infrared reflectance and thermal insulation temperature difference with the reference blackboard are carried out according to the GB / T 25261-2018 and JG / T 235-2014 standards; the bonding strength test is carried out according to the GB / T 9779-2015 standard; and finally, the carbonization degree is measured by the heat loss method, and the results are shown in Table 1 below.
[0063] Table 1 Test results of Examples 1-7 and Comparative Examples 1-5
[0064] As can be seen from Table 1, the present invention has excellent scrubbing resistance and solar radiation reflection effect. The scrubbing resistance of Examples 1 to 7 is all above 5000 times, and the thermal insulation temperature difference with the reference blackboard can reach up to 32°C. Specifically, the scrubbing resistance of the inorganic carbon-fixing coating obtained by the present invention can reach 5011 to 5421 times, the solar light reflectance can reach 0.9 to 0.96, the near-infrared reflectance can reach 0.89 to 0.93, the thermal insulation temperature difference with the reference blackboard is 25 to 32°C, and the bonding strength is 3.37 to 8.41 MPa.
[0065] By comparing Example 1 with Comparative Example 1, it can be seen that the carbon-cured composite material prepared by sintering in the present invention has higher carbonization activity and higher bonding strength than the multiphase mineral obtained by mechanical mixing. This is because the interfacial bonding strength of each phase of the carbon-cured composite material prepared by sintering is higher after carbonization, thereby improving its scrubbing resistance.
[0066] By comparing Example 1 with Comparative Example 2, it can be seen that the carbon-solidified composite material used in the present invention contains multiphase minerals. 2 S content 100%), of which γ-C 2 The S content is reduced. It is found that the carbonization activity of the carbon-solidified composite material with the multiphase minerals of the present invention is higher. Figure 1 (Example 1) and Figure 2 (Comparative Example 2) also shows that γ-C 2 When the S content is relatively low, more carbonization products will be produced (the gray part in the figure), which will then fill the voids in the coating (the black part in the figure). Figure 1 The gap is significantly less than Figure 2 This greatly improves the density of the coating.
[0067] Since the silica gel network generated during the carbonization process is relatively small and cannot fully play the role of a cross-linked network, it is necessary to introduce modified silica sol and an organic emulsion that can generate an organic cross-linked network to synergistically improve the cohesion of the coating. It can be seen from Example 1 and Comparative Example 3 that after removing the modified silica sol and the organic emulsion, the various properties of the coating are reduced.
[0068] It can be seen from Example 1 and Comparative Examples 4-5 that removing the aluminum raw material and the titanium raw material of the carbon-solidified composite material will affect the performance of the obtained inorganic carbon-fixing coating.
[0069] The present invention discloses a multifunctional inorganic carbon-fixing coating, the coating formed by the coating has both high scrub resistance and high solar radiation reflection effect. 2S is the main bonding component, and other mineral phases play different functional effects. Through the overall solar reflectance and near-infrared reflectance of the coating, the coating can be radiated and cooled through the long-wave mid-infrared transparent window, thereby achieving passive cooling inside the building. 2 The maintenance method is to absorb CO 2 The coating is cured in a low-carbon and environmentally friendly way. In addition, the coating has better resistance to weathering and UV aging and has a longer service life.
[0070] The specific implementation of the present invention described above does not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A multifunctional inorganic carbon-fixing coating, wherein the raw materials include 70 to 140 parts of carbon-cured composite material, 14 to 100 parts of deionized water, 10 to 70 parts of modified silica sol, and 1 to 14 parts of organic emulsion in parts by weight; in, The carbon-solidified composite material is obtained by mixing calcium raw materials, silicon raw materials, aluminum raw materials and titanium raw materials and then subjecting the mixture to calcination treatment.
2. The multifunctional inorganic carbon-fixing coating according to claim 1, It is characterized in that The calcium raw material, silicon raw material, aluminum raw material and titanium raw material are prepared according to the following molar ratio: Ca / Si=3.3-1.2, Al / Si<2, Ti / Si<1.
3. The multifunctional inorganic carbon-fixing coating according to claim 1, It is characterized in that The calcium raw material includes Ca(OH) 2 The silicon raw material includes SiO 2 The aluminum raw material includes Al 2 O 3 The titanium raw material includes TiO 2 The particle sizes of the calcium raw material, silicon raw material, aluminum raw material and titanium raw material are all between 0.1 μm and 500 μm.
4. The multifunctional inorganic carbon-fixing coating according to claim 1, It is characterized in that The calcium raw material, silicon raw material, aluminum raw material and titanium raw material are wet-mixed and then dried, followed by calcination treatment and dry grinding to obtain a carbon solidified composite material containing multiphase minerals; the multiphase minerals include 30-55% of γ-C 2 S, and the rest is Ca 2 Al 2 SiO 7 , Ca 2 Ti 1-x Si x O 4 and CaTiO 3 , where 0 < x < 1; the particle size of the carbon solidified composite material is between 0.4 μm and 70 μm.
5. The multifunctional inorganic carbon-fixing coating according to claim 1, It is characterized in that During the calcination treatment, the temperature is 1250-1400° C. and the time is 30-180 min.
6. The multifunctional inorganic carbon-fixing coating according to claim 1, It is characterized in that The preparation steps of the modified silica sol include: dissolving chitosan in an acetic acid solution with a mass concentration of 1% to obtain a chitosan solution; then adding the chitosan solution to the silica sol, adjusting the pH value to 8.5-9.5, stirring evenly and aging for more than 24 hours to obtain the modified silica sol; wherein the mass ratio of the acetic acid solution to chitosan is 100:(4-6), and the mass ratio of the silica sol to the chitosan solution is 100:(8-12); The solid content of the modified silica sol is 28-38%.
7. The multifunctional inorganic carbon-fixing coating according to claim 1, It is characterized in that The organic emulsion comprises one or more mixtures of acrylate emulsion, styrene-acrylic emulsion, pure acrylic emulsion, epoxy resin emulsion, EVA emulsion and silicone-acrylic emulsion in any proportion; the solid content of the organic emulsion is 40-50%.
8. A method for preparing a multifunctional inorganic carbon-fixing coating according to any one of claims 1 to 7, It is characterized in that The following steps are involved: The deionized water and the organic emulsion are uniformly mixed by ultrasonication, and the modified silica sol is slowly added dropwise to obtain a mixed solution; Then the carbon-solidified composite material is added into the mixed solution and mixed evenly to obtain the inorganic carbon-solidified coating.
9. The method for preparing the multifunctional inorganic carbon-fixing coating according to claim 8, It is characterized in that The deionized water and the organic emulsion are uniformly mixed by ultrasonication for 15 to 25 minutes; the carbon-cured composite material is added into the mixed solution, dispersed at a speed of 2500 to 3500 r / min for 0.5 to 1.5 hours and mixed uniformly.
10. An inorganic carbon-fixing coating, It is characterized in that The inorganic carbon-fixing coating is a coating of the inorganic carbon-fixing coating on the surface of the substrate, and then placed in CO 2 The inorganic carbon-fixing coating is formed by curing in an environment; the inorganic carbon-fixing coating is the inorganic carbon-fixing coating according to any one of claims 1 to 7.
Citation Information
Patent Citations
Low-carbon inorganic radiation refrigeration coating and preparation method thereof
CN114804745A
Carbon curing cementing material, preparation method and application
CN115650609A
Carbon-sequestration early-strength clinker-free low-carbon cementing material and use method thereof
CN116354625A
Colored low-calcium carbon sequestration cementing material and preparation method thereof
CN117534351A