Colored paint for radiation cooling and preparation method thereof

By using colored paint composed of core-shell structure quantum dot microspheres and high electronic band gap particles, the problem of single appearance of existing radiation-cooled paints is solved, the combination of the aesthetics of colored paints and the cooling effect is achieved, and the radiation cooling technology is expanded. The application range is simple and easy to use, suitable for architectural applications.

CN118994973APending Publication Date: 2024-11-22TIANJIN UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202310566964.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing radiation-cooled coatings have a single appearance due to their ultra-high broadband solar reflectivity, lack of color choice, resulting in aesthetic defects and glare effects, limiting their application in building energy conservation.

Method used

Colored paint consisting of core-shell structure quantum dot microspheres and high electron band gap particles are used to adjust the color through different particle sizes and concentrations, and combined with organic coating matrix solution to form a color layer and a radiation cooling layer, which is used to treat hydrothermal method and ultrasonic treatment. Preparation of such processes.

Benefits of technology

It realizes the combination of the aesthetic effect of colored paint and the radiation cooling effect, enhances the summer cooling effect, expands the application range of radiation cooling technology, and is simple in process and easy to prepare on a large scale, suitable for architectural applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994973A_ABST
    Figure CN118994973A_ABST
Patent Text Reader

Abstract

The invention discloses a colored coating for radiation cooling and a preparation method thereof, and relates to the technical field of radiation refrigeration, the colored coating comprises an upper layer and a lower layer, the upper layer is a colored layer, and the lower layer is a radiation cooling layer; the color layer can make the coating present different colors to meet the requirement of beauty, and the lower radiation cooling layer has high sunlight reflectivity and mid-infrared emissivity, so that the coating has a cooling effect; compared with previous colored coatings, the colored coating for radiation cooling has a comfortable optical attractive effect and can also achieve a cooling effect, and the preparation method is simple, wide in application scene and suitable for large-scale application and popularization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of radiation cooling, and in particular to a color coating for radiation cooling and a preparation method thereof. Background Art

[0002] The energy consumption of buildings using traditional cooling methods accounts for 30% of global primary energy use and 10% of greenhouse gas emissions. Therefore, it is very important to develop a green cooling technology that does not consume energy to achieve building energy conservation. Radiative cooling technology uses an atmospheric window of 8 to 13 um to send the heat of an object to outer space in the form of thermal radiation. It is a passive cooling method that does not consume energy, is pollution-free, simple and reliable. Moreover, radiative cooling materials can be prepared into various forms such as thin films or coatings. In particular, coatings are very suitable for application in building energy conservation and other occasions due to their simple preparation process and convenient operation.

[0003] Due to the ultra-high broadband solar reflectivity that reduces solar absorption, current radiative cooling coatings are usually limited to silver, ultra-bright or white appearance, resulting in aesthetic defects and glare effects. Therefore, the development of a colorful coating that can achieve radiative cooling effects is important and urgent for practical applications in architecture. Colored coatings with radiative cooling can further broaden the application of radiative cooling technology. Summary of the invention

[0004] The object of the present invention is to provide a colored coating for radiation cooling and a preparation method thereof, so as to solve the shortcomings of the existing radiation cooling technology in achieving color.

[0005] The present invention is achieved through the following technical solutions:

[0006] A color coating for radiation cooling, comprising an upper and a lower layer, wherein the upper layer is a color layer and the lower layer is a radiation cooling layer;

[0007] The color layer is composed of core-shell structure quantum dot microspheres and an organic coating matrix solution, wherein the core-shell structure quantum dot microspheres can be one of CdSe / CdS, CuGaS2 / ZnS, CuInS2 / ZnS and CuInSe2 / ZnS, and the organic coating matrix solution can be one of polystyrene, polyacrylate, polyalkyl acrylate, polymethacrylate, polyalkyl methacrylate, polycarbonate, polyacrylic acid, polymethacrylic acid and mixtures thereof and copolymers thereof;

[0008] The radiation cooling layer is composed of high electron band gap particles and an organic coating matrix solution, wherein the high electron band gap particles can be one of MgO particles, CaCO3 particles, Al2O3 particles and BaSO4 particles, and the coating matrix solution can be one of polystyrene, polyacrylate, polyalkyl acrylate, polymethacrylate, polyalkyl methacrylate, polycarbonate, polyacrylic acid, polymethacrylic acid and mixtures thereof and copolymers thereof;

[0009] Wherein, the particle size distributions of the core-shell structure quantum dot microspheres and high electron band gap particles are not uniform.

[0010] As an embodiment of the present invention, the color layer of the color coating for radiation cooling is mainly composed of: 0.8 to 1.5 parts by volume of an organic coating matrix solution, 1 to 3 parts by volume of anhydrous ethanol, 0.8 to 1.5 parts by volume of quantum dot microspheres, a defoamer with a volume fraction of 0.3v% to 0.5v%, a thickener with a volume fraction of 0.3v% to 0.5v%, and a dispersant with a volume fraction of 0.3v% to 0.5v%.

[0011] As an embodiment of the present invention, the radiation cooling layer of the colored coating for radiation cooling is mainly composed of: 0.8 to 1.5 parts by volume of an organic coating matrix solution, 1 to 3 parts by volume of anhydrous ethanol, 0.8 to 1.5 parts by volume of high electron band gap particles, a defoamer with a volume fraction of 0.3v% to 0.5v%, a thickener with a volume fraction of 0.3v% to 0.5v%, and a dispersant with a volume fraction of 0.3v% to 0.5v%.

[0012] As an embodiment of the present invention, the core-shell structure quantum dot microspheres can adjust the color of the color layer by introducing different concentrations of Ga / In and S / Se.

[0013] As an embodiment of the present invention, the organic coating matrix solution of the color layer can be one of polystyrene, polyacrylate, polyalkyl acrylate, polymethacrylate, polyalkyl methacrylate, polycarbonate, polyacrylic acid, polymethacrylic acid and mixtures thereof and copolymers thereof.

[0014] As an embodiment of the present invention, the organic coating matrix solution of the radiation cooling layer can be one of polystyrene, polyacrylate, polyalkyl acrylate, polymethacrylate, polyalkyl methacrylate, polycarbonate, polyacrylic acid, polymethacrylic acid and mixtures thereof and copolymers thereof.

[0015] As an embodiment of the present invention, the diameter of the core-shell structure quantum dot microspheres is 0.25 to 3 um.

[0016] As an embodiment of the present invention, the shell thickness of the core-shell structure quantum dot microspheres is 0.1 to 0.5 um.

[0017] As an embodiment of the present invention, the mass fraction of the solution of the organic coating matrix of the color layer is 5 to 50%.

[0018] As an embodiment of the present invention, the diameter of the high electron band gap particles is 0.25 to 3 um.

[0019] As an embodiment of the present invention, the mass fraction of the solution of the organic coating matrix of the radiation cooling layer is 5 to 50%.

[0020] The present invention also provides a method for preparing a colored coating for radiation cooling, comprising the following steps:

[0021] Step 100, preparing core-shell structure quantum dot microspheres by hydrothermal method;

[0022] Step 200, mixing the core-shell structure quantum dot microspheres with the organic coating matrix solution of the color layer, and adding anhydrous ethanol for dispersion and stirring to obtain a pre-dispersed coating;

[0023] Step 300, ultrasonically treat the pre-dispersed coating of the color layer, and then add a defoamer, a thickener, and a dispersant to obtain a finished coating of the color layer;

[0024] Step 400, mixing the high electron band gap particles with the organic coating matrix solution of the radiation cooling layer, and adding anhydrous ethanol for dispersion and stirring to obtain a pre-dispersed coating;

[0025] Step 500, subjecting the pre-dispersed coating of the radiation cooling layer to ultrasonic treatment, and then adding a defoamer, a thickener, and a dispersant to obtain a finished coating of the radiation cooling layer;

[0026] Step 600: After brushing the radiation cooling layer coating prepared in step 500, the color layer coating prepared in step 300 is directly applied on top of the radiation cooling layer, and the two are combined to form a color coating for radiation cooling.

[0027] As an embodiment of the present invention, in step 100, the preparation of core-shell structure quantum dot microspheres specifically includes:

[0028] 1 to 1.5 parts by volume of a mixed solution of a water-soluble reactant and ethanol, 1 to 1.5 parts by volume of sodium linoleate, and 1 to 1.5 parts by volume of a mixed solution of ethanol and linoleic acid are sequentially added into a hydrothermal kettle, stirred at a first preset temperature for a first preset time, hydrothermally reacted at a second preset temperature for a second preset time, the reactor is taken out and allowed to cool naturally, the powder in the reactor is filtered out and washed with water until neutral, and dried at a third preset temperature to obtain core-shell structure quantum dot microspheres.

[0029] Wherein, the first preset temperature is 20-40°C;

[0030] The first preset time is 0.5 to 2 hours;

[0031] The second preset temperature is 100-300°C;

[0032] The second preset time is 5 to 15 hours;

[0033] The third preset temperature is 60-80°C.

[0034] As an embodiment of the present invention, in step 200, the dispersion stirring is achieved by a high-speed disperser;

[0035] Wherein, the dispersion frequency of the high-speed disperser is 6000r / min-8000r / min, and the dispersion time is 3-5h.

[0036] As an embodiment of the present invention, in step 300, the ultrasonic treatment is achieved by a cell disruptor;

[0037] Among them, the ultrasonic treatment time is 30 to 50 minutes;

[0038] Ultrasonic power is 600-900W;

[0039] The ultrasound interval was set to 2 s.

[0040] As an embodiment of the present invention, in step 400, the dispersion stirring is achieved by a high-speed disperser;

[0041] Wherein, the dispersion frequency of the high-speed disperser is 6000r / min-8000r / min, and the dispersion time is 3-5h.

[0042] As an embodiment of the present invention, in step 500, the ultrasonic treatment is achieved by a cell disruptor;

[0043] Among them, the ultrasonic treatment time is 30 to 50 minutes;

[0044] Ultrasonic power is 600-900W;

[0045] The ultrasound interval was set to 2 s.

[0046] Compared with the prior art, the beneficial effects of the present invention are:

[0047] (1) The present invention uses high electron band gap particles of different particle sizes as the main component of the radiation cooling layer coating. The distribution of high electron band gap particles of different particle sizes has different scattering effects on sunlight in different bands. Different particle size distributions can better reflect the sunlight band and enhance the cooling effect of the coating in summer.

[0048] (2) The present invention uses core-shell structure quantum dot microspheres to realize colored coatings, which is simple in method, convenient in preparation and has low net absorption of sunlight;

[0049] (3) The present invention uses one of polystyrene, polyacrylate, polyalkyl acrylate, polymethacrylate, polyalkyl methacrylate, polycarbonate, polyacrylic acid, polymethacrylic acid and mixtures thereof and copolymers thereof as the organic coating matrix solution for the color layer and the radiation cooling layer, which has high emissivity.

[0050] (4) The colored coating for radiative cooling provided by the present invention has good aesthetic effect, is easy to prepare on a large scale, and has good compatibility with buildings, and has good market application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 It is a structural schematic diagram of the present invention.

[0052] For ordinary technicians in this field, other relevant drawings can be obtained based on the above drawings without any creative work. DETAILED DESCRIPTION

[0053] In order to enable those skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention is further described below in conjunction with specific embodiments.

[0054] Example 1

[0055] like Figure 1 As shown, a color coating for radiation cooling, the color coating comprises two layers, the upper layer is a color layer, and the lower layer is a radiation cooling layer. The color layer is composed of core-shell structure quantum dot microspheres and an organic coating matrix; the lower layer is a radiation cooling layer, which is composed of high electron band gap particles and an organic coating matrix, and can simultaneously achieve a solar light emissivity of more than 95% and an atmospheric window emissivity of more than 95%. Spraying the color layer coating on top of the radiation cooling layer coating can achieve both a color effect and a cooling effect.

[0056] The diameter of the color layer core-shell structure quantum dot microspheres is 0.25-3um. The color of the color layer is adjusted by introducing different concentrations of Ga / In and S / Se.

[0057] The color layer organic coating matrix solution can be one of polystyrene, polyacrylate, polyalkyl acrylate, polymethacrylate, polyalkyl methacrylate, polycarbonate, polyacrylic acid, polymethacrylic acid, mixtures thereof, and copolymers thereof.

[0058] The high electron band gap particles in the radiation cooling layer may be one of MgO particles, CaCO3 particles, Al2O3 particles and BaSO4 particles.

[0059] The organic coating matrix solution of the radiation cooling layer can be one of polystyrene, polyacrylate, polyalkyl acrylate, polymethacrylate, polyalkyl methacrylate, polycarbonate, polyacrylic acid, polymethacrylic acid, mixtures thereof and copolymers thereof.

[0060] Compared with the existing technology, this color coating uses core-shell structure quantum dot microspheres to adjust the color of the coating. This technical means can combine aesthetics with cooling, expanding the application scope of radiation cooling. At the same time, the coating can be well combined with architecture, accelerating the practical application of radiation cooling in architecture.

[0061] Example 2

[0062] A method for preparing a colored coating for radiation cooling is carried out according to the following steps:

[0063] 1-1.5 parts by volume of a mixed solution of a water-soluble reactant and ethanol, 1-1.5 parts by volume of sodium linoleate, and 1-1.5 parts by volume of a mixed solution of ethanol and linoleic acid are sequentially added to a hydrothermal kettle, stirred at 20-40°C for 0.5-2h, hydrothermally reacted at 100-300°C for 5-15h, the reactor is taken out and cooled naturally, the powder in the reactor is filtered out and washed with water until neutral, and dried at 60-80°C to obtain core-shell structure quantum dot microspheres. 0.8-1.5 parts by volume of core-shell structure quantum dot microspheres are mixed with 0.8-1.5 parts by volume of a color layer organic coating matrix solution, and 1-3 parts by volume of anhydrous ethanol are added to disperse and stir in a high-speed disperser at 6000r / min-8000r / min for 3-5h to obtain a pre-dispersed coating. The pre-dispersed coating is placed in a cell disruptor, and a defoamer with a volume fraction of 0.3v% to 0.5v%, a thickener with a volume fraction of 0.3v% to 0.5v%, and a dispersant with a volume fraction of 0.3v% to 0.5v% are added, and ultrasonic treatment is performed for 30 to 50 minutes at an ultrasonic power of 600W to 900W and an ultrasonic interval of 2s to obtain a color layer coating; 0.8 to 1.5 parts by volume of high electron band gap particles are mixed with 0.8 to 1.5 parts by volume of a radiation cooling layer organic coating matrix solution, and 1 to 3 parts by volume of anhydrous ethanol are added to perform dispersion and stirring in a high-speed disperser at 6000r / min to 8000r / min for 3 to 5 hours to obtain a pre-dispersed coating. The pre-dispersed coating is placed in a cell disruptor, and a defoamer with a volume fraction of 0.3v% to 0.5v%, a thickener with a volume fraction of 0.3v% to 0.5v%, and a dispersant with a volume fraction of 0.3v% to 0.5v% are added, and ultrasonic treatment is performed for 30 to 50 minutes at an ultrasonic power of 600W to 900W and an ultrasonic interval of 2s to obtain a radiation cooling layer coating; on the basis of the radiation cooling layer coating, a color layer coating is sprayed to complete the preparation of a color coating with a radiation cooling effect.

[0064] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A color coating for radiation cooling and a preparation method thereof, characterized in that: It consists of two layers, the upper layer is a color layer, and the lower layer is a radiation cooling layer; The color layer is composed of core-shell structure quantum dot microspheres and an organic coating matrix solution, wherein the core-shell structure quantum dot microspheres can be one of CdSe / CdS, CuGaS2 / ZnS, CuInS2 / ZnS and CuInSe2 / ZnS, and the organic coating matrix solution can be one of polystyrene, polyacrylate, polyalkyl acrylate, polymethacrylate, polyalkyl methacrylate, polycarbonate, polyacrylic acid, polymethacrylic acid and mixtures thereof and copolymers thereof; The radiation cooling layer is composed of high electron band gap particles and an organic coating matrix solution, wherein the high electron band gap particles can be one of MgO particles, CaCO3 particles, Al2O3 particles and BaSO4 particles, and the organic coating matrix solution can be one of polystyrene, polyacrylate, polyalkyl acrylate, polymethacrylate, polyalkyl methacrylate, polycarbonate, polyacrylic acid, polymethacrylic acid and mixtures thereof and copolymers thereof; The particle size distributions of the quantum dot microspheres and high electron band gap particles of the core-shell structure are not uniform.

2. A colored coating for radiation cooling according to claim 1, characterized in that: The color layer mainly consists of: 0.8-1.5 volume parts of organic coating matrix solution, 1-3 volume parts of anhydrous ethanol, 0.8-1.5 volume parts of quantum dot microspheres, a defoamer with a volume fraction of 0.3v%-0.5v%, a thickener with a volume fraction of 0.3v%-0.5v%, and a dispersant with a volume fraction of 0.3v%-0.5v%.

3. A colored coating for radiation cooling according to claim 1, characterized in that: The core-shell structure quantum dot microspheres can adjust the color of the color layer by introducing different concentrations of Ga / In and S / Se.

4. A colored coating for radiation cooling according to claim 1, characterized in that: The organic coating matrix solution of the color layer can be one of polystyrene, polyacrylate, polyalkyl acrylate, polymethacrylate, polyalkyl methacrylate, polycarbonate, polyacrylic acid, polymethacrylic acid, mixtures thereof and copolymers thereof.

5. The color coating for radiation cooling according to claim 1, characterized in that: The organic coating matrix solution of the radiation cooling layer may be one of polystyrene, polyacrylate, polyalkyl acrylate, polymethacrylate, polyalkyl methacrylate, polycarbonate, polyacrylic acid, polymethacrylic acid, mixtures thereof, and copolymers thereof.

6. A colored coating for radiation cooling according to claim 1, characterized in that: The core-shell structure quantum dot microspheres have a diameter of 0.25 to 3 μm.

7. A colored coating for radiation cooling according to claim 1, characterized in that: The shell thickness of the core-shell structure quantum dot microsphere is 0.1-0.5 um.

8. The color coating for radiation cooling according to claim 1, characterized in that: The mass fraction of the organic coating matrix solution of the color layer is 5-50%.

9. The color coating for radiation cooling according to claim 1, characterized in that: The high electron band gap particles have a diameter of 0.25 to 3 μm.

10. The color coating for radiation cooling according to claim 1, characterized in that: The mass fraction of the organic coating matrix solution of the radiation cooling layer is 5-50%.

11. A method for preparing a colored coating for radiation cooling, characterized in that: The steps include: Step 100, preparing core-shell structure quantum dot microspheres by hydrothermal method; Step 200, mixing the core-shell structure quantum dot microspheres with the organic coating matrix solution of the color layer, and adding anhydrous ethanol for dispersion and stirring to obtain a pre-dispersed coating for the color layer; Step 300, ultrasonically treat the pre-dispersed coating of the color layer, and then add a defoamer, a thickener and a dispersant to obtain a finished coating of the color layer; Step 400, mixing the high electron band gap particles with the organic coating matrix solution of the radiation cooling layer, and adding anhydrous ethanol for dispersion and stirring to obtain a pre-dispersed coating; Step 500, ultrasonically treating the pre-dispersed coating of the radiation cooling layer, and then adding a defoamer, a thickener and a dispersant to obtain a finished coating of the radiation cooling layer; Step 600: After brushing the radiation cooling layer coating prepared in step 500, the color layer coating prepared in step 300 is directly applied on top of the radiation cooling layer, and the two are combined to form a color coating for radiation cooling.

12. The method for preparing a colored coating for radiation cooling according to claim 11, characterized in that: In step 100, preparing core-shell structure quantum dot microspheres specifically includes: 1 to 1.5 parts by volume of a mixed solution of a water-soluble reactant and ethanol, 1 to 1.5 parts by volume of sodium linoleate, and 1 to 1.5 parts by volume of a mixed solution of ethanol and linoleic acid are sequentially added into a hydrothermal kettle, stirred at a first preset temperature for a first preset time, hydrothermally reacted at a second preset temperature for a second preset time, the reactor is taken out and allowed to cool naturally, the powder in the reactor is filtered out and washed with water until neutral, and dried at a third preset temperature to obtain core-shell structure quantum dot microspheres. Wherein, the first preset temperature is 20-40°C; The first preset time is 0.5 to 2 hours; The second preset temperature is 100-300°C; The second preset time is 5 to 15 hours; The third preset temperature is 60-80°C.

13. The method for preparing a colored coating for radiation cooling according to claim 11, characterized in that: In step 200, the dispersion stirring is achieved by a high-speed disperser; Wherein, the dispersion frequency of the high-speed disperser is 6000r / min-8000r / min, and the dispersion time is 3-5h.

14. The method for preparing a colored coating for radiation cooling according to claim 11, characterized in that: In step 300, ultrasonic treatment is achieved by a cell disruptor; Among them, the ultrasonic treatment time is 30 to 50 minutes; Ultrasonic power is 600-900W; The ultrasound interval was set to 2 s.

15. The color coating for radiation cooling and the preparation method thereof according to claim 11, characterized in that: In step 400, the dispersion stirring is achieved by a high-speed disperser; Wherein, the dispersion frequency of the high-speed disperser is 6000r / min-8000r / min, and the dispersion time is 3-5h.

16. The method for preparing a colored coating for radiation cooling according to claim 11, characterized in that: In step 500, ultrasonic treatment is performed by a cell disruptor; Among them, the ultrasonic treatment time is 30 to 50 minutes; Ultrasonic power is 600-900W; The ultrasound interval was set to 2 s.

17. The method for preparing a colored coating for radiation cooling according to claim 11, characterized in that: The solar emissivity of the radiation cooling layer coating in the sunlight band is above 95%, and the infrared emissivity of the atmospheric window is above 95%.

Citation Information

Cited By

  • Double-layer radiation refrigeration colored paint and preparation method thereof

    CN120173457A

  • Hydrochromic self-adaptive color radiation refrigeration coating and application thereof

    CN122255799A