Photonic crystal coating as well as preparation method and application thereof
Directly preparing photonic crystal coatings through hard-core-soft shell colloidal nano microspheres, solving the problems of complex and high cost of existing photonic crystal coatings, and achieving high structural stability and significant iridescent effect photonic crystal coatings are suitable for multiple type of substrate.
Patent Information
- Application Number
- CN202411214358.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-31
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-31
AI Technical Summary
The existing photonic crystal coating preparation process is complex and costly, and the application of curing methods under ultraviolet light is limited. The packaging polymer enters the coating and causes negative impacts, and the preparation process is not conducive to widespread application.
The photonic crystal coating is directly prepared by hard-core-soft shell colloidal nano microspheres. Through coating, heating assembly and packaging processes, a structural color coating with high structural stability and high color saturation is formed, with a significant iridescent effect.
It realizes a photonic crystal coating with simple process, low cost, bright and bright structural colors, with high color fastness and significant iridescent effect, and is suitable for a variety of substrates.
Smart Images

Figure CN118994994A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a photonic crystal coating, a preparation method and application thereof, and belongs to the technical field of photonic crystal structure color generation. Background Art
[0002] Color plays an important role in our daily lives, whether it is household items, building decoration, or traffic signs. Color not only enhances the visual beauty of the environment, but also provides functional information.
[0003] Paint coloring is one of the main ways to give color to objects. Paints are usually composed of organic pigments (coloring components) and film-forming components (adhesives or coating agents) as well as other auxiliary components (leveling agents, thickeners, etc.). Although organic pigments have advantages such as strong tinting power and hiding power, they usually also have insufficient light fastness and environmental protection issues related to chemical colorants. Photonic crystals are an optical material formed by materials with different refractive indices arranged in a certain periodicity in space. Its basic feature is that it has a photon bandgap. When the photon bandgap falls in the visible light range, the visible light within the bandgap is prohibited from propagating, so it is selectively reflected, and the reflective light of constructive interference stimulates the human eye, giving people a visual effect of structural color. Photonic crystal structural color is a physical color, which usually has color characteristics such as high brightness, high saturation, iridescence effect, and good light resistance and environmental stability. Therefore, photonic crystals are an excellent material for preparing coatings.
[0004] Chinese patent CN117004315A mixes a polymerizable liquid crystal monomer, a chain extender, an ultraviolet light initiator and a low-boiling point solvent and applies it to the surface of the substrate, and cures it under ultraviolet light. The liquid crystal monomer and the chain extender self-assemble into a photonic crystal structural color coating. The structural color coating prepared by this method has bright colors and strong structural stability. However, it can only be cured under ultraviolet light, and the application scenarios are relatively limited. Chinese patent CN118287357A introduces a cross-linking agent into the polymerization process of styrene (St) to obtain high-refractive index nano-microspheres, prepares them into liquid photonic crystal coatings, applies them on the surface of the substrate to construct a photonic crystal color-forming structure, and obtains a photonic crystal structural color coating after polymer curing and encapsulation. This method has a simple preparation process and low cost. However, the encapsulated polymer will enter the interior of the PS photonic crystal, which will have a negative impact on the color of the coating, and the encapsulated polymer selection is limited. Chinese patent CN116200125A coats a layer of copper-tin alloy coating on the surface of the substrate, and coats a photonic crystal layer with a columnar pore structure and a thin film interference layer of multiple thin films with different refractive indices on the surface of the copper-tin alloy coating, thereby enhancing the optical properties of the coating, and finally coats a covering layer made of thermoplastic polymer material on the surface of the photonic crystal layer and the thin film interference layer to provide the mechanical strength of the coating. This method can form two reflection effects by setting a photonic crystal layer and a thin film interference layer. However, the preparation process is relatively complicated, the cost is high, and it is not conducive to wide application. Chinese invention patent CN116656169A first coats a ceramic precursor in an opal structure photonic crystal, sinters the ceramic material at high temperature, removes the polymer opal template at the same time, obtains an inverse opal photonic crystal, and then crushes the inverse opal photonic crystal to obtain an inverse opal structure photonic crystal pigment powder, and finally mixes with a film-forming substance and auxiliary components to obtain a photonic crystal coating. The photonic crystal coating prepared by this method has rich colors and metallic luster, but the preparation process is complicated and energy consumption is large.
[0005] Therefore, a photonic crystal coating with simple preparation process, low cost and bright structural color is invented, which has very important practical application value. Summary of the invention
[0006] The purpose of the present invention is to provide a photonic crystal coating, which is directly prepared from hard-core-soft-shell colloidal nano-microspheres. The structural color coating prepared by the coating has excellent structural stability, high saturation of structural color, good color fastness, and exhibits a significant iridescence effect.
[0007] The technical solution adopted by the present invention to solve its technical problem is:
[0008] A photonic crystal coating, comprising the following components in parts by weight: 100 parts of hard core-soft shell nano-microsphere dispersion, 1 to 8 parts of leveling agent, 0.1 to 0.4 parts of stray light absorber, and 0 to 6 parts of high boiling point additive;
[0009] The hard-core-soft-shell nano-microspheres have an inner core of one of highly cross-linked polystyrene (PS), polymethyl methacrylate (PMMA), polymethacrylic acid (PMAA), poly(styrene-methyl methacrylate) (P(St-MMA)) or poly(styrene-methacrylic acid) (P(St-MAA));
[0010] The shell layer is one of soft and hard monomer copolymers of poly(butyl acrylate-methyl methacrylate) (P(MMA-BA)), poly(hydroxyethyl acrylate-hydroxyethyl methacrylate) (P(HEA-HEMA)), poly(ethyl acrylate-methacrylic acid) (P(EA-MAA)), poly(isobutyl acrylate-methyl methacrylate) (P(MMA-IBA)), poly(tert-butyl acrylate-methyl methacrylate) (P(MMA-TBA)) or poly(isooctyl acrylate-methyl methacrylate) (P(MMA-2-EHA));
[0011] The weight ratio of the soft shell to the hard core is 1:0.5-1.5; the weight ratio of the soft monomer in the soft shell to the hard monomer is 1:0.5-2.
[0012] Preferably, the hard core-soft shell nano-microspheres have a diameter of 150-350 nm, good sphericity, and a monodispersity of less than 0.12.
[0013] Preferably, the content of nanospheres in the hard core-soft shell nanosphere dispersion is 15-50 wt %, and the balance is water.
[0014] Preferably, the photonic crystal coating comprises the following components in parts by weight:
[0015] 100 parts of a hard-core-soft-shell nano-microsphere dispersion with a mass fraction of 30 to 50 wt%, 1 to 8 parts of a surfactant, 0.1 to 0.4 parts of a black pigment, and 0 to 6 parts of a high boiling point additive; or
[0016] 100 parts of hard-core-soft-shell nano-microsphere dispersion liquid with a mass fraction of 15-30wt%, 1-8 parts of surfactant, 0.1-0.4 parts of black pigment, and 2-6 parts of high boiling point additive.
[0017] Preferably, the leveling agent is one or a mixture of fatty alcohol polyoxyethylene ether, polyoxyethylene sorbitan fatty acid ester, fatty acid polyoxyethylene ester, fatty acid methyl ester ethoxylate or polypropylene glycol ethylene oxide adduct;
[0018] The stray light absorber is one or a mixture of carbon black, water-soluble or water-dispersible black pigment;
[0019] The high boiling point auxiliary agent is selected from one or a mixture of glycerol, propylene glycol, formamide or ethylene glycol.
[0020] A method for preparing the photonic crystal coating comprises: placing 100 parts by weight of a hard core-soft shell nano-microsphere dispersion, 1 to 8 parts by weight of a leveling agent, 0.1 to 0.4 parts by weight of a stray light absorber, and 0 to 6 parts by weight of a high boiling point additive into a container, and fully stirring the mixture to obtain the photonic crystal coating.
[0021] A photonic crystal structural color coating is prepared by coating the photonic crystal coating according to claim 1.
[0022] A method for preparing a photonic crystal structure color coating, the method comprising the following steps:
[0023] S1. Coating: applying the photonic crystal coating evenly on the surface of the substrate;
[0024] S2, heating assembly: heating and assembling the substrate coated with S1 to evaporate the water inside the photonic crystal, inducing the microspheres to move toward a highly regular arrangement structure, and obtaining a photonic crystal structural color coating; the heating assembly conditions are a temperature of 50 to 95°C and a time of 5 to 40 minutes;
[0025] For the photonic crystal coating made of hard core-soft shell nano-microspheres with a weight ratio of soft monomer to hard monomer of 1:0.5-1 in the soft shell, the obtained photonic crystal structure color coating needs to be assembled for the second time to further improve the regularity of the photonic crystal structure and obtain a photonic crystal structure color coating with beautiful color and significant iridescence effect; the secondary assembly conditions are temperature 110-140°C and time 2-10min;
[0026] S3, encapsulation: applying an encapsulation polymer to the surface of the photonic crystal structural color coating obtained in S2 and heat treating it, so that the photonic crystal layer is further stably cured to obtain a structural color coating with high color fastness and significant iridescent effect; the heating treatment conditions are drying at a temperature of 50-100°C for 5-40 minutes and baking at 110-140°C for 2-10 minutes.
[0027] Preferably, the substrate in S1 is textile, wood, steel, plastic, paper or glass.
[0028] Preferably, the application method described in S1 is a scraping method or a spraying method.
[0029] Preferably, when the application method selected in S1 is the scraping method, the weight of the photonic crystal coating is: 100 parts of a hard-core-soft-shell nano-microsphere dispersion with a mass fraction of 30-50wt%, 1-8 parts of a surfactant, 0.1-0.4 parts of a black pigment, and 0-6 parts of a high boiling point additive. The concentration of the hard-core-soft-shell nano-microsphere dispersion is preferably 40-45wt%.
[0030] Preferably, when the application method selected in S1 is spraying, the weight of the photonic crystal coating is 100 parts of a hard-core-soft-shell nano-microsphere dispersion with a mass fraction of 15-30wt%, 1-8 parts of a surfactant, 0.1-0.4 parts of a black pigment, and 2-6 parts of a high boiling point additive. The concentration of the hard-core-soft-shell nano-microsphere dispersion is preferably 20-25wt%.
[0031] Preferably, when the application method selected in S1 is the scraping method, the paint is evenly applied by a shear-induced method using a putty knife, a wire rod, a roller, a brush, or the like.
[0032] Preferably, when the application method selected in S1 is spraying, the tool used is a gravity, suction, pressure-feeding or pump-feeding spray gun.
[0033] Preferably, the encapsulating polymer in S4 is water-based polyurethane or water-based polyacrylate.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] 1. The method of the present invention breaks through the usual process of preparing photonic crystal pigments from nano-microspheres and then preparing photonic crystal coatings from photonic crystal pigments. It adopts a new method of directly constructing a photonic crystal coating system from colloidal nano-microspheres, which has a simple process and low energy consumption;
[0036] 2. The present invention uses hard core-soft shell nano-microspheres with a refractive index difference as assembly primitives, and after assembly, a non-close-packed photonic crystal with a hard core as the skeleton and a soft shell as the continuous phase is formed. The microspheres have their own adhesive components, and no additional adhesive or film-forming components need to be added to the coating system. The system has good stability and strong tolerance;
[0037] 3. The constructed structural color coating has the characteristics of high structural stability (high color fastness) and high color saturation, and has a significant iridescent effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 This is a digital photo of the photonic crystal coating (left) and the structural color coating (right) prepared with a soft-hard monomer weight ratio of 1:0.57 in Example 1;
[0039] Figure 2This is a digital photo of the photonic crystal coating (left) and structural color coating (right) prepared using P MAA@P (MMA-BA) nanospheres in Example 2;
[0040] Figure 3 This is the reflectivity curve of the structural color coating prepared by the blade coating method with a nano-microsphere concentration of 45 wt% in Example 3;
[0041] Figure 4 The digital photo (left) and reflectivity curve (right) of the structural color coating prepared by spraying method with the nano-microsphere concentration of 25 wt% in Example 4;
[0042] Figure 5 This is a digital photo of the structural color coating with a nano-microsphere particle size of 230 nm in Example 5;
[0043] Figure 6 This is a digital photo of the structural color coating prepared by secondary assembly at 130° C. for 5 min in Example 6;
[0044] Figure 7 This is a digital photo of the photonic crystal coating prepared in Comparative Example 1 with a soft-hard monomer weight ratio of 1:0.2;
[0045] Figure 8 This is a digital photo of the structural color coating prepared in comparative example 2 with a weight ratio of soft to hard monomers of 1:3;
[0046] Fig. 9 This is a digital photo of the structural color coating prepared using PS@PMMA nanospheres in Comparative Example 3;
[0047] Fig.10 This is the reflectivity curve of the structural color coating prepared by the scraping method in Comparative Example 4 with a nano-microsphere concentration of 10 wt%;
[0048] Fig.11 The digital photo (left) and reflectivity curve (right) of the structural color coating prepared by spraying method with a nano-microsphere concentration of 45wt% in Comparative Example 5;
[0049] Fig.12 This is a digital photograph of the structural color coating prepared in Example 5 after secondary assembly at 150° C. for 2 minutes. DETAILED DESCRIPTION
[0050] The technical solution of the present invention is further described in detail below through specific embodiments. It should be understood that the implementation of the present invention is not limited to the following embodiments, and any form of modification and / or change made to the present invention will fall within the protection scope of the present invention.
[0051] In the present invention, unless otherwise specified, all parts and percentages are by weight, and the equipment and raw materials used can be purchased from the market or are commonly used in the art. The methods in the following embodiments are all conventional methods in the art unless otherwise specified.
[0052] Unless otherwise specified, the reagents used in the following examples can be purchased from conventional biochemical reagent stores.
[0053] In the present invention, nano-microspheres with a hard core-soft shell structure are prepared according to the Chinese invention patent "A method for preparing flexible photonic crystal elementary nano-microspheres" (ZL201911112794.X, CN110804127B).
[0054] Example 1
[0055] 20g of PS@P(MMA-BA) nanosphere dispersion with a particle size of 260nm and a mass fraction of 45wt%, 0.8g of fatty alcohol polyoxyethylene ether surfactant, and 0.048g of carbon black were mixed, and stirred by a magnetic stirrer to make them evenly mixed to obtain a photonic crystal coating. In the PS@P(MMA-BA) nanospheres, the weight ratio of shell / core monomers is 1:0.63, and the weight ratio of shell soft / hard monomers is 1:0.57.
[0056] The photonic crystal coating obtained by the above method is used to prepare a photonic crystal structural color coating, the method is as follows:
[0057] S1. Coating: The photonic crystal coating prepared by the above method is evenly coated on the surface of the PPS plastic substrate through a wire rod;
[0058] S2. Heating assembly: The coated PPS plastic substrate is placed in an oven at 80°C for heating assembly for 15 minutes to evaporate the water inside the photonic crystal and induce the microspheres to move toward a highly regular arrangement structure to obtain a photonic crystal structural color coating;
[0059] S3, secondary assembly: placing the heated assembled photonic crystal structural color coating in a 140°C oven for secondary assembly for 2 minutes, further improving the regularity of the photonic crystal structure, and obtaining a structural color coating with beautiful colors and significant iridescence effect;
[0060] S4. Packaging: Spray water-based polyurethane on the surface of the secondary assembled structural color coating and dry it at 80°C for 15 minutes and bake it at 140°C for 2 minutes to further stabilize and solidify the photonic crystal layer to obtain a structural color coating with high color fastness and significant iridescence effect.
[0061] Example 2 A photonic crystal coating
[0062] 20g of PMAA@P(MMA-BA) nanosphere dispersion with a particle size of 252nm and a mass fraction of 45wt%, 1.0g of fatty alcohol polyoxyethylene ether surfactant, and 0.052g of carbon black were mixed, and stirred by a magnetic stirrer to make them uniformly mixed to obtain a photonic crystal coating. In the PMAA@P(MMA-BA) nanospheres, the weight ratio of shell / core monomers is 1:0.8, and the weight ratio of shell soft / hard monomers is 1:0.57.
[0063] The photonic crystal coating obtained by the above method is used to prepare a photonic crystal structural color coating, the method is as follows:
[0064] S1. Coating: The photonic crystal coating obtained by the above method is evenly coated on the surface of the PPS plastic substrate by a roller;
[0065] S2. Heating assembly: placing the coated PPS plastic substrate in a 90°C oven for heating assembly for 10 minutes to evaporate the water inside the photonic crystal and induce the microspheres to move toward a highly regularly arranged structure, thereby obtaining a photonic crystal structural color coating;
[0066] S3, secondary assembly: placing the heated assembled photonic crystal structural color coating in a 110°C oven for secondary assembly for 10 minutes, further improving the regularity of the photonic crystal structure, and obtaining a structural color coating with beautiful colors and significant iridescence effect;
[0067] S4. Packaging: Spray water-based polyurethane on the surface of the secondary assembled structural color coating and dry it at 90°C for 10 minutes and bake it at 110°C for 10 minutes to further stabilize and solidify the photonic crystal layer to obtain a structural color coating with high color fastness and significant iridescence effect.
[0068] Example 3 A photonic crystal coating
[0069] 20g of PS@P(EA-MMA) nanosphere dispersion with a particle size of 252nm and a mass fraction of 45wt%, 0.8g of fatty alcohol polyoxyethylene ether surfactant, and 0.052g of carbon black were mixed and stirred by a magnetic stirrer to make them uniformly mixed to obtain a photonic crystal coating. In the PS@P(EA-MMA) nanosphere, the weight ratio of shell / core monomers is 1:1, and the weight ratio of shell soft / hard monomers is 1:1.5.
[0070] The photonic crystal coating obtained by the above method is used to prepare a photonic crystal structural color coating, the method is as follows:
[0071] S1. Coating: The photonic crystal coating obtained by the above method is evenly coated on the surface of the metal substrate by a brush;
[0072] S2. Heating assembly: placing the coated plastic substrate in a 90°C oven for heating assembly for 10 minutes to evaporate the water inside the photonic crystal and induce the microspheres to move toward a highly regular arrangement structure, thereby obtaining a photonic crystal structural color coating;
[0073] S3. Packaging: Spray water-based polyurethane on the surface of the heated assembled structural color coating and dry it at 90°C for 10 minutes and bake it at 110°C for 10 minutes to further stabilize and solidify the photonic crystal layer to obtain a structural color coating with high color fastness and significant iridescence effect.
[0074] Example 4
[0075] 20g of PS@P(MMA-BA) nanosphere dispersion with a particle size of 265nm and a mass fraction of 25wt%, 0.8g of fatty alcohol polyoxyethylene ether surfactant, 0.048g of carbon black, and 0.8g of glycerol were mixed and stirred with a magnetic stirrer to make them uniformly mixed to obtain a photonic crystal coating. In the PS@P(MMA-BA) nanospheres, the weight ratio of shell / core monomers is 1:1, and the weight ratio of shell soft / hard monomers is 1:0.57.
[0076] The photonic crystal coating obtained by the above method is used to prepare a photonic crystal structural color coating, the method is as follows:
[0077] S1. Coating: The photonic crystal coating obtained by the above method is sprayed on the surface of the PPS plastic substrate by a pump-type spray gun;
[0078] S2. Heating assembly: The coated PPS plastic substrate is placed in an oven at 80°C for heating assembly for 15 minutes to evaporate the water inside the photonic crystal and induce the microspheres to move toward a highly regular arrangement structure to obtain a photonic crystal structural color coating;
[0079] S3, secondary assembly: placing the heated assembled photonic crystal structural color coating in a 140°C oven for secondary assembly for 2 minutes, further improving the regularity of the photonic crystal structure, and obtaining a structural color coating with beautiful colors and significant iridescence effect;
[0080] S4. Packaging: Spray water-based polyurethane on the surface of the secondary assembled structural color coating and dry it at 80°C for 15 minutes and bake it at 140°C for 2 minutes to further stabilize and solidify the photonic crystal layer to obtain a structural color coating with high color fastness and significant iridescence effect.
[0081] Example 5
[0082] 20g of PS@P(MMA-BA) nanosphere dispersion with a particle size of 230nm and a mass fraction of 25wt%, 1.6g of fatty alcohol polyoxyethylene ether surfactant, 0.030g of carbon black, and 0.6g of glycerol were mixed and stirred with a magnetic stirrer to make them uniformly mixed to obtain a photonic crystal coating. In the PS@P(MMA-BA) nanospheres, the weight ratio of shell / core monomers is 1:0.5, and the weight ratio of shell soft / hard monomers is 1:1.3.
[0083] The photonic crystal coating obtained by the above method is used to prepare a photonic crystal structural color coating, the method is as follows:
[0084] S1. Coating: The photonic crystal coating obtained by the above method is evenly coated on the surface of the metal substrate by a pump-type spray gun;
[0085] S2. Heating assembly: placing the coated plastic substrate in a 60°C oven for heating assembly for 30 minutes to evaporate the water inside the photonic crystal and induce the microspheres to move toward a highly regular arrangement structure, thereby obtaining a photonic crystal structural color coating;
[0086] S3. Packaging: Spray water-based polyurethane on the surface of the secondary assembled structural color coating and dry it at 60°C for 30 minutes and bake it at 110°C for 10 minutes to further stabilize and solidify the photonic crystal layer to obtain a structural color coating with high color fastness and significant iridescence effect.
[0087] Example 6
[0088] 20g of PS@P(MMA-BA) nanosphere dispersion with a particle size of 260nm and a mass fraction of 50wt%, 0.8g of fatty alcohol polyoxyethylene ether surfactant, and 0.048g of carbon black were mixed, and stirred by a magnetic stirrer to make them uniformly mixed to obtain a photonic crystal coating. In the PS@P(MMA-BA) nanospheres, the weight ratio of shell / core monomers is 1:0.8, and the weight ratio of shell soft / hard monomers is 1:0.57.
[0089] The photonic crystal coating obtained by the above method is used to prepare a photonic crystal structural color coating, the method is as follows:
[0090] S1. Coating: The photonic crystal coating obtained by the above method is evenly coated on the surface of the wooden substrate by a brush;
[0091] S2. Heating assembly: placing the coated plastic substrate in a 70°C oven for heating assembly for 20 minutes to evaporate the water inside the photonic crystal and induce the microspheres to move toward a highly regular arrangement structure, thereby obtaining a photonic crystal structural color coating;
[0092] S3, secondary assembly: placing the heated assembled photonic crystal structural color coating in a 130°C oven for secondary assembly for 5 minutes, further improving the regularity of the photonic crystal structure, and obtaining a structural color coating with beautiful colors and significant iridescence effect;
[0093] S4. Packaging: Spray water-based polyurethane on the surface of the secondary assembled structural color coating and dry it at 70°C for 20 minutes and bake it at 130°C for 5 minutes to further stabilize and solidify the photonic crystal layer to obtain a structural color coating with high color fastness and significant iridescence effect.
[0094] Comparative Example 1
[0095] 20g of PS@P(MMA-BA) nanosphere dispersion with a particle size of 260nm and a mass fraction of 45wt%, 0.8g of fatty alcohol polyoxyethylene ether surfactant, 0.048g of carbon black, and 0.8g of glycerol were mixed, and stirred with a magnetic stirrer to make them evenly mixed to obtain a photonic crystal coating. In the PS@P(MMA-BA) nanospheres, the weight ratio of shell / core monomers is 1:0.63, and the weight ratio of shell soft / hard monomers is 1:0.2.
[0096] The photonic crystal coating obtained by the above method is used to prepare a photonic crystal structural color coating, the method is as follows:
[0097] S1. Coating: The photonic crystal coating obtained by the above method is evenly coated on the surface of the PPS plastic substrate through a wire rod;
[0098] S2. Heating assembly: The coated PPS plastic substrate is placed in an oven at 80°C for heating assembly for 15 minutes to evaporate the water inside the photonic crystal and induce the microspheres to move toward a highly regular arrangement structure to obtain a photonic crystal structural color coating;
[0099] S3, secondary assembly: placing the heated assembled photonic crystal structural color coating in a 140°C oven for secondary assembly for 2 minutes, further improving the regularity of the photonic crystal structure, and obtaining a structural color coating with low color saturation and no red color effect;
[0100] Comparative Example 2
[0101] 20g of PS@P(MMA-BA) nanosphere dispersion with a particle size of 260nm and a mass fraction of 45wt%, 0.8g of fatty alcohol polyoxyethylene ether surfactant, and 0.048g of carbon black were mixed, and stirred by a magnetic stirrer to make them evenly mixed to obtain a photonic crystal coating. In the PS@P(MMA-BA) nanospheres, the weight ratio of shell / core monomers is 1:0.63, and the weight ratio of shell soft / hard monomers is 1:3.
[0102] The photonic crystal coating obtained by the above method is used to prepare a photonic crystal structural color coating, the method is as follows:
[0103] S1. Coating: The photonic crystal coating obtained by the above method is evenly coated on the surface of the PPS plastic substrate through a wire rod;
[0104] S2. Heating assembly: The PPS-coated plastic substrate is placed in an oven at 80°C for heating assembly for 15 minutes to evaporate the water inside the photonic crystal and induce the microspheres to move toward a highly regular arrangement structure, thereby obtaining a photonic crystal structural color coating;
[0105] Comparative Example 3
[0106] 20g of PS@PMMA nanosphere dispersion with a particle size of 252nm and a mass fraction of 45wt%, 1.0g of fatty alcohol polyoxyethylene ether surfactant, and 0.052g of carbon black were mixed and stirred with a magnetic stirrer to make them uniformly mixed to obtain a photonic crystal coating. In the PS@PMMA nanospheres, the weight ratio of shell / core monomers is 1:0.8, and the weight ratio of shell soft / hard monomers is 1:0.57.
[0107] The photonic crystal coating obtained by the above method is used to prepare a photonic crystal structural color coating, the method is as follows:
[0108] S1. Coating: The photonic crystal coating obtained by the above method is evenly coated on the surface of the PPS plastic substrate by a roller;
[0109] S2. Heating assembly: The coated PPS plastic substrate is placed in a 90°C oven for heating assembly for 10 minutes to evaporate the water inside the photonic crystal and induce the microspheres to move toward a highly regularly arranged structure to obtain a photonic crystal structural color coating.
[0110] Comparative Example 4
[0111] 20g of PS@P(EA-MMA) nanosphere dispersion with a particle size of 210nm and a mass fraction of 10wt%, 0.8g of fatty alcohol polyoxyethylene ether surfactant, and 0.052g of carbon black were mixed and stirred with a magnetic stirrer to make them uniformly mixed to obtain a photonic crystal coating. In the PS@P(EA-MMA) nanosphere, the weight ratio of shell / core monomers is 1:1, and the weight ratio of shell soft / hard monomers is 1:1.5.
[0112] The photonic crystal coating obtained by the above method is used to prepare a photonic crystal structural color coating, the method is as follows:
[0113] S1. Coating: The photonic crystal coating obtained by the above method is evenly coated on the surface of the PPS plastic substrate through a wire rod;
[0114] S2. Heating assembly: placing the coated PPS plastic substrate in a 90°C oven for heating assembly for 10 minutes to evaporate the water inside the photonic crystal and induce the microspheres to move toward a highly regularly arranged structure, thereby obtaining a photonic crystal structural color coating;
[0115] S3. Packaging: spray water-based polyurethane on the surface of the heated assembled structural color coating, dry it at 90° C. for 10 min, and bake it at 110° C. for 10 min, so that the photonic crystal layer is further stably cured to obtain the structural color coating.
[0116] Comparative Example 5
[0117] 20g of PS@P(MMA-BA) nanosphere dispersion with a particle size of 265nm and a mass fraction of 45wt%, 0.8g of fatty alcohol polyoxyethylene ether surfactant, 0.048g of carbon black, and 0.8g of glycerol were mixed, and stirred with a magnetic stirrer to make them uniformly mixed to obtain a photonic crystal coating. In the PS@P(MMA-BA) nanospheres, the weight ratio of shell / core monomers is 1:1, and the weight ratio of shell soft / hard monomers is 1:0.57.
[0118] The photonic crystal coating obtained by the above method is used to prepare a photonic crystal structural color coating, the method is as follows:
[0119] S1. Coating: The photonic crystal coating obtained by the above method is sprayed on the surface of the PPS plastic substrate by a pump-type spray gun;
[0120] S2. Heating assembly: The coated PPS plastic substrate is placed in an oven at 80°C for heating assembly for 15 minutes to evaporate the water inside the photonic crystal and induce the microspheres to move toward a highly regular arrangement structure to obtain a photonic crystal structural color coating;
[0121] S3. Secondary assembly: The heated assembled photonic crystal structural color coating is placed in a 140°C oven for secondary assembly for 2 minutes to further improve the regularity of the photonic crystal structure and obtain a darker color of the structural color coating.
[0122] Comparative Example 6
[0123] 20 g of PS@P (MMA-BA) nanosphere dispersion with a particle size of 260 nm and a mass fraction of 50 wt%, 0.8 g of fatty alcohol polyoxyethylene ether surfactant, and 0.048 g of carbon black were mixed, and stirred with a magnetic stirrer to make them evenly mixed to obtain a photonic crystal coating.
[0124] In PS@P(MMA-BA) nanospheres, the weight ratio of shell / core monomers is 1:0.8, and the weight ratio of shell soft / hard monomers is 1:0.57.
[0125] The photonic crystal coating obtained by the above method is used to prepare a photonic crystal structural color coating, the method is as follows:
[0126] S1. Coating: The photonic crystal coating obtained by the above method is evenly coated on the surface of the metal substrate by a brush;
[0127] S2. Heating assembly: placing the coated plastic substrate in a 70°C oven for heating assembly for 20 minutes to evaporate the water inside the photonic crystal and induce the microspheres to move toward a highly regular arrangement structure, thereby obtaining a photonic crystal structural color coating;
[0128] S3, secondary assembly: The heated assembled photonic crystal structural color coating is placed in a 150°C oven for secondary assembly for 2 minutes, in the hope of further improving the regularity of the photonic crystal structure, but the color of the structural color coating is damaged.
[0129] Digital photos of the photonic crystal coating and structural color coating constructed in Example 1 are shown in Figure 1 The photonic crystal coating has high brightness, and the prepared structural color coating has beautiful color and significant iridescence effect, indicating that the photonic crystal coating can effectively construct a structural color coating on a plastic substrate by coating.
[0130] The digital photos and SEM images of the structural color coating constructed in Example 2 are shown in Figure 2 As shown in the figure, the photonic crystals assembled by nano-microspheres have excellent structural regularity and beautiful colors.
[0131] The reflectivity curve of the structural color coating constructed in Example 3 is shown in Figure 3 ,As shown in the figure, the reflection peak at 45wt% concentration is high and narrow, indicating that the brightness and saturation of its structural color are high.
[0132] The optical properties of the structural color coating constructed in Example 4 are shown in Figure 4 As shown in the figure, the reflection peak at 25wt% concentration is high and narrow, the coating color is bright, and the structural color brightness and saturation are high.
[0133] The digital photo of the structural color coating constructed in Example 5 is shown in Figure 5 The structural color coating has bright colors and a significant iridescent effect, indicating that the photonic crystal coating can effectively construct a structural color coating on a metal substrate by spraying.
[0134] The digital photo of the structural color coating constructed in Example 6 is shown in Figure 6 The structural color coating has bright colors and a significant iridescent effect, indicating that the photonic crystal coating can be used to construct a structural color coating on a wood substrate by brushing.
[0135] The structural color coating prepared in Comparative Example 1 is shown in the digital photo. Figure 7Compared with Example 1, the proportion of hard monomer in the shell layer of Comparative Example 1 is too low, and the prepared structural color coating is dull in color and has no iridescent effect.
[0136] The structural color coating prepared in Comparative Example 2 is shown in the digital photo. Figure 8 Compared with Example 1, the proportion of hard monomers in the shell layer of Comparative Example 2 is too high, the prepared structural color coating cannot form a film, and the structural stability is poor.
[0137] The structural color coating prepared in Comparative Example 3 is shown in Fig. 9 Compared with Example 2, the microsphere shell layer of Comparative Example 3 has only hard monomers. When preparing the coating, the structural color coating is broken and the structural stability is poor.
[0138] The structural color coating prepared in Comparative Example 4 is shown in Fig.10 Compared with Example 3, when the structural color coating was prepared by the scraping method in Comparative Example 4, the concentration of nano-microspheres was too low (10 wt %), and the reflectivity of the prepared structural color coating was low, and the color saturation and brightness were poor.
[0139] The structural color coating prepared in Comparative Example 5 is shown in Fig.11 Compared with Example 4, when the structural color coating in Comparative Example 5 was prepared by spraying, the concentration of nano-microspheres was too high (45wt%), and the uniformity of spraying was poor. Moreover, since there was less water in the spray droplets and more microspheres, the microspheres did not have enough time to arrange regularly, and the reflectivity of the prepared structural color coating was low, and the color saturation and brightness were poor.
[0140] The structural color coating prepared in Comparative Example 6 is shown in Fig.12 Compared with Example 6, in Comparative Example 6, the assembly temperature was too high during the secondary assembly, and the color of the prepared structural color coating was dark.
[0141] In summary, the core of the present invention is to use hard-core-soft-shell nano-microsphere dispersion liquid to evenly mix with leveling agent, stray light absorber, and high boiling point additive to prepare photonic crystal coating, and the coating system has good film-forming ability. Through coating, drying, baking, and packaging processes, photonic crystal structural color coating can be prepared in a simple and large area. This method is simple in process and widely applicable to substrates. The constructed structural color coating has both high structural stability (high color fastness) and high color saturation, and has the characteristics of significant iridescent effect.
[0142] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.
[0143] The above is a detailed introduction to a photonic crystal coating, a preparation method and an application thereof provided by the present invention. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present invention, several improvements and modifications can be made to the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A photonic crystal coating, characterized in that The photonic crystal coating comprises the following components in parts by weight: 100 parts of hard core-soft shell nano-microsphere dispersion, 1 to 8 parts of leveling agent, 0.1 to 0.4 parts of stray light absorber, and 0 to 6 parts of high boiling point additive; The hard-core-soft-shell nano-microspheres have an inner core of one of highly cross-linked polystyrene (PS), polymethyl methacrylate (PMMA), polymethacrylic acid (PMAA), poly(styrene-methyl methacrylate) (P(St-MMA)) or poly(styrene-methacrylic acid) (P(St-MAA)); The shell layer is one of soft and hard monomer copolymers of poly(butyl acrylate-methyl methacrylate) (P(MMA-BA)), poly(hydroxyethyl acrylate-hydroxyethyl methacrylate) (P(HEA-HEMA)), poly(ethyl acrylate-methacrylic acid) (P(EA-MAA)), poly(isobutyl acrylate-methyl methacrylate) (P(MMA-IBA)), poly(tert-butyl acrylate-methyl methacrylate) (P(MMA-TBA)) or poly(isooctyl acrylate-methyl methacrylate) (P(MMA-2-EHA)); The weight ratio of the soft shell to the hard core is 1:0.5~1.5; the weight ratio of the soft monomer in the soft shell to the hard monomer is 1:0.5~2.
2. The photonic crystal coating according to claim 1, characterized in that: The hard core-soft shell nano-microspheres have a diameter of 150-350 nm, good sphericity, and a monodispersity of less than 0.
12.
3. The photonic crystal coating according to claim 1, characterized in that: The content of nano-microspheres in the hard-core-soft-shell nano-microsphere dispersion is 15-50wt%, and the balance is water.
4. The photonic crystal coating according to claim 1, characterized in that: The photonic crystal coating comprises the following components in parts by weight: 100 parts of 30-50wt% hard-core-soft-shell nanosphere dispersion, 1-8 parts of surfactant, 0.1-0.4 parts of black pigment, 0-6 parts of high boiling point additive; or 100 parts of hard-core-soft-shell nano-microsphere dispersion with a mass fraction of 15-30wt%, 1-8 parts of surfactant, 0.1-0.4 parts of black pigment, and 2-6 parts of high boiling point additive.
5. The photonic crystal coating according to claim 1, characterized in that: The leveling agent is one or a mixture of fatty alcohol polyoxyethylene ether, polyoxyethylene sorbitan fatty acid ester, fatty acid polyoxyethylene ester, fatty acid methyl ester ethoxylate or polypropylene glycol ethylene oxide adduct; The stray light absorber is one or a mixture of carbon black, water-soluble or water-dispersible black pigment; The high boiling point auxiliary agent is selected from one or a mixture of glycerol, propylene glycol, formamide or ethylene glycol.
6. A method for preparing the photonic crystal coating according to claim 1, characterized in that The method comprises the following steps: placing 100 parts of hard core-soft shell nano microsphere dispersion, 1-8 parts of leveling agent, 0.1-0.4 parts of stray light absorber and 0-6 parts of high boiling point auxiliary agent into a container by weight, and fully stirring to obtain photonic crystal coating.
7. A photonic crystal structure color coating, characterized in that: The photonic crystal structural color coating is prepared by coating the photonic crystal coating according to claim 1.
8. A method for preparing a photonic crystal structure color coating, characterized in that The method comprises the following steps: S1. Coating: uniformly applying the photonic crystal coating according to claim 1 on the surface of the substrate; S2, heating assembly: heating the substrate coated with S1 to evaporate the water inside the photonic crystal, inducing the microspheres to move toward a highly regular arrangement structure, and obtaining a photonic crystal structural color coating; the heating assembly conditions are 50-95°C and 5-40 min; For the photonic crystal coating made of hard core-soft shell nano-microspheres with a weight ratio of soft monomer to hard monomer of 1:0.5~1 in the soft shell, the obtained photonic crystal structure color coating needs to be assembled for the second time to further improve the regularity of the photonic crystal structure and obtain a photonic crystal structure color coating with beautiful colors and significant iridescence effect; the secondary assembly conditions are temperature 110~140℃, time 2~10 min; S3, encapsulation: applying an encapsulation polymer to the surface of the photonic crystal structural color coating obtained in S2 and heat treating it, so that the photonic crystal layer is further stably solidified to obtain a structural color coating with high color fastness and significant iridescent effect; the heating treatment conditions are drying at a temperature of 50~100℃ for 5~40min and baking at 110~140℃ for 2~10min.
9. The method for preparing a photonic crystal structure color coating according to claim 8, characterized in that: The substrate in S1 is textile, wood, steel, plastic, paper or glass.
10. The method for preparing a photonic crystal structure color coating according to claim 8, characterized in that: The application method described in S1 is a knife coating method or a spray coating method.
Citation Information
Patent Citations
Flexible photonic crystal element nano microspheres and preparation method thereof
CN110804127A
Method for preparing color generating material with photonic crystal structure by spraying method
CN115558145A
High-saturation photonic crystal structural color coating and preparation method thereof
CN118287357A
Chromogenic double inverse opals photonic crystal resin film using water as ink and the preparation thereof
US20230183407A1
Cited By
Structural color ink and application thereof
CN119531158A