Preparation method of high-wear-resistance super-hydrophobic coating and coating

By using hydrophobic nano-spherical SiO2 particles, micron-sized spherical SiO2 particles, and glass fibers as fillers, combined with hot-pressing mesh, spraying, and electrostatic flocking techniques, a highly wear-resistant superhydrophobic coating was prepared, solving the problem of poor coating wear resistance and achieving efficient and low-cost coating preparation.

CN118995010AActive Publication Date: 2024-11-22NANJING UNIV OF AERONAUTICS & ASTRONAUTICS
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411164968.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-22
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

Existing superhydrophobic coatings have poor wear resistance and are prone to failure, which limits their mass production and use in practical applications.

Method used

A highly wear-resistant superhydrophobic coating was prepared by using hydrophobic nano-spherical SiO2 particles, hydrophobic micron-spherical SiO2 particles, and hydrophobic glass fibers as fillers, combined with hot-pressing mesh, spraying, and electrostatic flocking techniques.

Benefits of technology

It improves the wear resistance and hydrophobicity of the coating, with a contact angle >155°, a roll-off angle <5°, and a wear resistance of ≥250 cycles. It is low in cost and suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995010A_ABST
    Figure CN118995010A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a high-wear-resistance super-hydrophobic coating and the coating. The preparation method comprises the following steps: carrying out hydrophobic modification on SiO2 and glass fiber powder; hydrophobic nano spherical SiO2 particles, hydrophobic micron spherical SiO2 and hydrophobic glass fiber powder are mixed with epoxy resin and ethyl acetate to prepare a super-hydrophobic coating; deionized water and absolute ethyl alcohol are sequentially used for cleaning the base body; the thermoplastic plastic screen is combined to the surface of the base body in a hot-pressing mode; the super-hydrophobic coating is sprayed on the surface of the treated matrix, then electrostatic flocking equipment is used for adsorbing hydrophobic fiber composite powder to the surface of the coating, and the coating is prepared after curing; the microstructure of the super-hydrophobic coating prepared by the method is composed of the reticular ribs and the cured super-hydrophobic complex filled in the grid structure, and the super-hydrophobic coating is excellent in hydrophobic performance, outstanding in wear resistance and low in preparation cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of super hydrophobic coating preparation, and specifically to a preparation method and coating of a highly wear-resistant super hydrophobic coating. Background Art

[0002] Superhydrophobic coatings have excellent water repellency and water droplets have difficulty wetting their surfaces. Generally, surfaces with a contact angle greater than 150° and a rolling angle less than 10° are defined as superhydrophobic surfaces. Superhydrophobic coatings have broad application prospects in the fields of metal anti-corrosion, anti-icing and anti-fouling of power systems, and anti-icing of aircraft due to their excellent self-cleaning, anti-icing, anti-corrosion, and drag reduction properties.

[0003] At present, the spraying method is a feasible method for batch preparation of super-hydrophobic coatings under practical conditions due to its advantages of simple process and low cost. However, poor wear resistance is the main problem that currently restricts the mass production and use of super-hydrophobic coatings. The reason why the super-hydrophobic coating prepared by the traditional spraying method is easy to fail is that the rough structure on its surface is easily destroyed. The coating system used is composed of low surface energy fillers, film-forming substances and solvents. The rough structure of the coating surface depends on the protrusions formed by the accumulation of filler particles and the holes formed by the rapid evaporation of the solvent. Since the filler particles are modified with low surface energy, their binding force with the film-forming substance is low, therefore, the rough structure formed by the accumulation of filler particles is easily destroyed and the coating fails. Researchers have improved the wear resistance of super-hydrophobic coatings from the perspective of optimizing coating formulations and constructing surface microstructures. Patent CN112210272B discloses "a wear-resistant super-hydrophobic composite material and a preparation method thereof". A composite material super-hydrophobic coating with a micro / nano-scale surface structure is prepared by combining a structurally stable micron-sized particle formed by hybridizing a combination of multi-level nanoparticles with strong mutual particle interaction with an epoxy system adhesive. This method improves the mechanical stability of the super-hydrophobic coating to a certain extent. However, the preparation process of the amino-terminated hyperbranched polysiloxane and ACNTB-SiO2-coupling agent particles used in the coating is complex, the reaction conditions are high, and it is not easy to prepare in batches. In addition, carbon nanotubes are used as one of the main fillers, which is costly and has limitations in actual use. Patent CN 115608586 B discloses "a simple and controllable method for preparing super-wear-resistant and super-hydrophobic surfaces". This method first sprays polydimethylsiloxane PDMS and a gas-phase hydrophobic SiO2 modifier on the surface of a metal substrate, and then uses an infrared nanosecond laser to ablate the coating surface to obtain a regular micron-level rough structure. This method can produce a super-hydrophobic coating with a designable surface morphology, and its mechanical stability is improved. However, the use of this method to prepare a super-hydrophobic coating requires the use of laser etching equipment, which has high equipment costs and poor production efficiency, so it also has great limitations in mass production and design applications.

[0004] Therefore, it is of great significance to the practical application of superhydrophobic coatings to develop a method for preparing highly wear-resistant superhydrophobic coatings under the premise of low cost and easy construction. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a highly wear-resistant super-hydrophobic coating and a coating, wherein the prepared super-hydrophobic coating has the advantages of excellent hydrophobicity and wear resistance, and can solve the problems of poor wear resistance and easy failure of traditional super-hydrophobic coatings under actual working conditions.

[0006] This application is implemented through the following technical solutions:

[0007] First, the present application provides a method for preparing a highly wear-resistant super-hydrophobic coating, which comprises the following steps:

[0008] (1) performing hydrophobic modification treatment on SiO2 particles and glass fiber powder to obtain hydrophobic nano-spherical SiO2 particles, hydrophobic micron-spherical SiO2 particles and hydrophobic glass fibers for standby use;

[0009] The above-mentioned SiO2 particles include micron spherical SiO2 particles and nano spherical SiO2 particles, and their particle sizes are 5-20μm and 15-30nm respectively; the single fiber diameter of the glass fiber is 11-17μm, and the aspect ratio is 20-50.

[0010] (2) Preparation of super-hydrophobic coating: Use a magnetic stirrer to mix epoxy resin, curing agent and ethyl acetate with hydrophobic nano-spherical SiO2, hydrophobic micron-spherical SiO2 and hydrophobic glass fiber powder at room temperature, with a stirring speed of about 450 r / min and a stirring time of 1.5-3 h to obtain a super-hydrophobic coating for standby use;

[0011] In the prepared super-hydrophobic coating, the mass fraction of epoxy resin (E51) is 2.48-4.96%, the mass fraction of curing agent (T31) is 0.62-1.24%, the mass fraction of hydrophobic nano-spherical SiO2 particles is 1.25-2.05%, the mass fraction of hydrophobic micron-spherical SiO2 particles is 1.25-2.05%, the mass fraction of hydrophobic glass fiber is 0.20-1.2%, and the balance is ethyl acetate.

[0012] (3) The hydrophobic nano-spherical SiO2 particles, the hydrophobic micron-spherical SiO2, and the hydrophobic glass fibers are uniformly mixed with a mechanical stirrer at a stirring speed of 140-300 r / min for a stirring time of 15-25 min to obtain a hydrophobic fiber composite powder for later use.

[0013] In the obtained hydrophobic fiber composite powder, the mass ratios of hydrophobic nano-spherical hydrophobic SiO2, hydrophobic micron-spherical SiO2 and hydrophobic glass fiber are 10:6:1-1.5 respectively.

[0014] (4) Pretreatment of the substrate: The substrate surface is cleaned with deionized water and anhydrous ethanol in turn, and dried for later use.

[0015] (5) Preparation of coating: First, a screen with a pore size of 11-850 μm is hot-pressed onto the surface of a substrate; secondly, the super-hydrophobic coating prepared in step (2) is sprayed onto the surface of the substrate to form a super-hydrophobic coating layer; then, within 10-15 minutes after the spraying is completed, the hydrophobic fiber composite powder prepared in step (3) is adsorbed onto the surface of the super-hydrophobic coating layer using an electrostatic flocking technique, and a highly wear-resistant super-hydrophobic coating is obtained after curing at 20-80° C. for 1.5-48 hours.

[0016] The coating material has a wide curing temperature range, which makes the coating have a wide range of applications. When the curing temperature is high, the curing time is short; lowering the curing temperature requires a longer curing time, but it can proceed naturally at room temperature without the need for external energy, which is more conducive to engineering applications.

[0017] Furthermore, the preparation process of the "hydrophobic modification treatment" in the above step (1) is specifically as follows: 1) anhydrous ethanol, 1H, 1H, 2H, 2H perfluorodecyl triethoxysilane (fluorosilane) and ammonia water (mass concentration 25%) are mixed in a mass ratio of 100:1-3:6 and ultrasonically dispersed for 15-30 minutes to obtain a modifier for standby use; 2) nano-spherical SiO2 particles, micron-spherical SiO2 and glass fiber are added to the above-mentioned modifier to obtain a nano-spherical SiO2 particle mixed solution (wherein the mass percentage of the nano-spherical SiO2 particles is 7.4%-10.7%), a micron-spherical SiO2 mixed solution ( The method comprises the following steps: 1) preparing a mixture of hydrophobic nano-spherical SiO2 particles, wherein the mass percentage of the micron-spherical SiO2 particles is 7.4%-10.7% and a glass fiber mixed solution (wherein the mass percentage of the glass fiber powder is 7.4%-10.7%); 2) placing the three mixed solutions obtained in step 2) into a heat-collecting magnetic stirrer respectively, and stirring continuously for 8-14 hours at a stirring speed of about 450r / min at 20-40°C; and then placing the slurry obtained after stirring into an infrared drying oven for drying at a drying temperature of 55-70°C and a drying time of 8-16 hours, to obtain hydrophobic nano-spherical SiO2 particles, hydrophobic micron-spherical SiO2, and hydrophobic glass fiber powder respectively. In this step, the glass fiber and silica particles are fluorinated to reduce their surface energy so that they have good hydrophobic properties.

[0018] Furthermore, the substrate material used in step (4) can be any material that can adhere to the screen (thermoplastic plastic), such as plastic, glass, fiberglass or aluminum alloy.

[0019] Further, in step (5), "hot pressing" refers to: using a hot press machine to hot press the screen to the substrate surface, forming a grid-like rib structure on the substrate surface; the hot pressing temperature is 110-140 ° C, the hot pressing pressure is 3.5-5MPa, and the holding time is 15-30min; the "spraying" refers to spraying the super-hydrophobic coating obtained in step (2) on the substrate surface using a spray gun, and the spraying pressure is 4-6Bar, the distance between the spray gun and the substrate is 10cm, and the spray gun moving speed is 1.5cm / s; the "electrostatic flocking" refers to using an electrostatic flocking machine to adsorb the hydrophobic fiber composite powder prepared in step (3) to the above-mentioned coating surface, and the flocking voltage is 30-50KV, the powder output is about 3-5g / min, the electrostatic flocking machine moving speed is 2cm / s, and the electrostatic flocking machine discharge port is 10-15cm away from the coating. The coating thickness obtained is 70-100μm.

[0020] Secondly, the present invention provides the highly wear-resistant super-hydrophobic coating prepared by the above method. The coating is composed of the screen on the substrate surface and the super-hydrophobic composite after curing (including hydrophobic nano-spherical SiO2, hydrophobic micron spherical SiO2, randomly arranged hydrophobic glass fibers, epoxy resins, hydrophobic glass fibers implanted in the coating perpendicular to the coating surface, etc.);The screen is hot-pressed on the substrate surface to form a grid-like rib structure, and the super-hydrophobic composite after curing is filled between the grids.

[0021] Compared with the prior art, the advantages and beneficial effects of the present invention are as follows:

[0022] 1. The present application adopts hydrophobic nanometer spherical SiO2 particles and hydrophobic micrometer spherical SiO2 particles of two different diameter hydrophobic fillers, and creatively introduces hydrophobic glass fiber into super hydrophobic coating system, to enhance the wear resistance of super hydrophobic coating. Large particle size powder has a larger contact area with substrate, and is more firmly combined with the resin in the cross-linked structure in the coating, and the glass fiber in the coating can also transfer the load axially when its surface is worn, so the coating obtained by the filler system consisting of hydrophobic nanometer SiO2, hydrophobic micrometer SiO2 and hydrophobic glass fiber has good wear resistance.

[0023] 2. The preparation steps of super-hydrophobic coating of the present application can be divided into hot-pressing grid, spraying coating, and electrostatic adsorption. The screen mesh hot-pressed on the substrate surface helps to enhance the combination of coating and substrate, and its closed grid structure helps to store gas to resist the wetting of liquid, which is beneficial to improve the hydrophobicity of coating; super-hydrophobic coating is sprayed, and after spraying, the hydrophobic fiber composite powder composed of hydrophobic SiO2 and hydrophobic glass fiber is adsorbed on the coating surface by electrostatic flocking technology, and under the action of electrostatic electric field, the glass fiber in the hydrophobic fiber composite powder can be longitudinally arranged along the direction of the electric field and implanted in the coating perpendicular to the coating surface, and after curing, the glass fiber part is implanted inside the coating, which is not easily pulled out and destroyed during the wear process, and the surface micro-morphology constructed by it has good stability, which improves the wear resistance of super-hydrophobic coating, and at the same time, the rich hydrophobic filler layer formed on the coating surface can effectively ensure the hydrophobicity of coating and improve its wear resistance.

[0024] 3. The super-hydrophobic coating prepared by the present invention has excellent hydrophobic properties and outstanding wear resistance, with a contact angle of >155° and a rolling angle of <5°. The wear resistance of the coating is tested by a sandpaper cyclic wear experiment, and the number of cyclic wear resistance of the coating is ≥250 times. At the same time, the super-hydrophobic coating prepared by the present invention has low cost, simple process, and is suitable for mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 Schematic diagram of the surface morphology of the super-hydrophobic coating prepared in the present invention.

[0026] In the figure, 1. super hydrophobic coating; 2. screen; 3. substrate; 4. epoxy resin; 5. hydrophobic glass fiber; 6. hydrophobic micron spherical SiO2 particles; 7. hydrophobic nano spherical SiO2 particles.

[0027] Figure 2 This is a SEM image of the surface morphology of the coating prepared in Example 2.

[0028] Figure 3 This is a photo of the coating obtained in Example 3. DETAILED DESCRIPTION

[0029] Fluorosilane (96%), ammonia (AR, 25%), SiO2 powder of different particle sizes, glass fiber powder, epoxy resin (E51), curing agent (T31) and ethyl acetate used in the following examples are all commercially available. Fluorosilane, ammonia, ethyl acetate, micron spherical SiO2 particles, nano spherical SiO2 particles are all purchased from Shanghai Aladdin Reagent Co., Ltd., and glass fiber powder is purchased from Taiyuan Hengtai Mineral Materials Co., Ltd.

[0030] Thermoplastic screens were purchased from Shanghai Haorui Wire Mesh Factory.

[0031] The stirring device used in the following examples is a heat-collecting magnetic stirrer (DF-101S) produced by Shanghai Lichen Bangxi Instrument Technology Co., Ltd., the mechanical stirrer is a DJ1C-60S power-enhancing electric stirrer, the drying oven is a DZF-6051 vacuum drying oven produced by Shanghai Heheng Instrument Equipment Co., Ltd., the hot press is a KH-6014H-10 veneer hot press, and the equipment used for electrostatic adsorption is an SFC11 electrostatic flocking machine.

[0032] The high wear-resistant super-hydrophobic coating prepared by the following examples, adopts contact angle meter to measure the static contact angle of coating by GB / T30447-2013, and simultaneously measures its rolling angle, to characterize the hydrophobicity of coating; Test the hardness of coating by GB / T6739-2006 with QHQ-A type portable pencil scratch tester; Adopt sandpaper cycle wear test to test its wear resistance, specific testing method is: by the sample of specification 2.5cm*6.5cm, make coating surface contact with No. 6 metallographic sandpaper, by the weight that mass is 100g is fixed to the back of sample, make sample move forward 10cm at a uniform speed under the pressure of 1.6KPa, rotate sample 90 °, continue to move forward 10cm, define above-mentioned complete process as a sandpaper wear cycle, repeat said process, until sample loses super-hydrophobicity (i.e. contact angle is less than 150 ° or rolling angle is greater than 10 °), record the number of wears experienced.

[0033] In order to make the contents of the present invention easier to understand, the technical solution of the present invention is further described below in conjunction with specific implementation methods, but the present invention is not limited thereto.

[0034] Example 1

[0035] 1. Preparation of hydrophobic modified materials: First, anhydrous ethanol, 1H, 1H, 2H, 2H perfluorodecyltriethoxysilane (fluorosilane) and ammonia water were ultrasonically dispersed at room temperature for 30 minutes in a mass ratio of 100:1:6 to obtain a modifier.

[0036] Adding nano-spherical SiO2 particles with a particle size of 15 nm, micron-spherical SiO2 particles with a particle size of 5 μm, and glass fiber powder with a single filament diameter of 11 μm and an aspect ratio of 20 to the modifier, respectively, to obtain a nano-spherical SiO2 particle mixed solution (wherein the mass percentage of the nano-spherical SiO2 particles is 9.2%), a micron-spherical SiO2 mixed solution (wherein the mass percentage of the micron-spherical SiO2 particles is 9.2%), and a glass fiber powder mixed solution (wherein the mass percentage of the glass fiber powder is 9.2%);

[0037] Use a heat-collecting magnetic stirrer to stir continuously at 40°C at a stirring speed of about 450 r / min for 8 hours, and dry at 55°C for 8 hours to obtain fluorinated-modified hydrophobic nano-spherical SiO2 particles, hydrophobic micron-spherical SiO2 particles and hydrophobic glass fiber powder for use.

[0038] 2. Preparation of super-hydrophobic coating: Using hydrophobic nano-spherical SiO2 particles, hydrophobic micron spherical SiO2 particles and hydrophobic glass fiber powder, epoxy resin (E51), curing agent (T31), and ethyl acetate as raw materials, the above raw materials were stirred at room temperature for 1.5h using a heat-collecting magnetic stirrer to prepare a super-hydrophobic coating; wherein the mass fraction of the epoxy resin (E51) is 4.96%, the mass fraction of the curing agent (T31) is 1.24%, the mass fraction of the 15nm hydrophobic SiO2 particles is 1.65%, the mass fraction of the 5μm hydrophobic SiO2 is 1.65%, the mass fraction of the hydrophobic glass fiber is 1.20%, and the remainder is ethyl acetate;

[0039] 3. The hydrophobic nano-spherical SiO2 particles, the hydrophobic micron-spherical SiO2, and the hydrophobic glass fiber are mixed in a mass ratio of 10:6:1, and mixed evenly with a mechanical stirrer at a stirring speed of 140 r / min and a stirring time of 15 min to obtain a hydrophobic fiber composite powder;

[0040] 4. Pretreatment of the substrate: Use 7101 type slide glass as the substrate, clean the substrate surface with deionized water and anhydrous ethanol in turn, and dry it at 80℃ for 1h;

[0041] 5. Preparation of coating: First, a hot press is used to hot-press the polypropylene screen with an aperture of 850 μm and the substrate, the hot pressing temperature is 120 ° C, the holding time is 20 min, and the hot pressing pressure is 3.5 MPa; secondly, the super hydrophobic coating obtained in step 2 is sprayed on the substrate surface using a spray gun, the spraying pressure is 4 Bar, the distance between the spray gun and the substrate is 10 cm, and the spray gun moves at a speed of 1.5 cm / s; then within 10-15 min after the spraying is completed, the hydrophobic fiber composite powder obtained in step 3 is adsorbed to the surface of the above-mentioned coating using an electrostatic flocking machine, the flocking voltage is 30 KV, the powder output is about 3 g / min, the flocking handle moving speed is 2 cm / s, the flocking handle discharge port and the coating distance are 10 cm, and finally, a highly wear-resistant super hydrophobic coating is obtained after curing for 48 hours at 20 ° C. The coating thickness obtained is 70-100 μm.

[0042] The super-hydrophobic coating obtained in this embodiment is composed of a screen on the surface of the substrate and a cured super-hydrophobic composite. After testing, in the cured super-hydrophobic composite, the mass percentage of hydrophobic nano-spherical SiO2 is 21.93%, the mass percentage of hydrophobic micron spherical SiO2 is 18.40%, the mass percentage of randomly arranged hydrophobic glass fibers is 9.53%, the mass percentage of hydrophobic glass fibers directionally implanted in the coating perpendicular to the coating surface is 0.88%, and the balance is epoxy resin.

[0043] The surface morphology of the super-hydrophobic coating prepared in this embodiment is shown in FIG. Figure 1 As shown, where B is a local enlarged schematic diagram of A.

[0044] Example 2

[0045] 1. Preparation of hydrophobic modified material: firstly, anhydrous ethanol, 1H, 1H, 2H, 2H perfluorodecyl triethoxysilane and ammonia water were ultrasonically dispersed at room temperature for 15 min in a mass ratio of 100:3:6 to obtain a modifier for standby use;

[0046] Then, nano-spherical SiO2 particles with a particle size of 20 nm, micron-spherical SiO2 particles with a particle size of 10 μm, and glass fiber powder with a single filament diameter of 12.5 μm and an aspect ratio of 35 are added to the modifier respectively; a nano-spherical SiO2 particle mixed solution (wherein the mass percentage of the nano-spherical SiO2 particles is 7.4%), a micron-spherical SiO2 mixed solution (wherein the mass percentage of the micron-spherical SiO2 particles is 7.4%), and a glass fiber powder mixed solution (wherein the mass percentage of the glass fiber powder is 7.4%) are obtained;

[0047] Then, the three mixed solutions were continuously stirred at a stirring speed of about 450 r / min at 35°C for 14 hours using a heat-collecting magnetic stirrer and dried at 60°C for 10 hours to obtain fluorinated-modified hydrophobic nano-spherical SiO2 particles, hydrophobic micron-spherical SiO2 particles and hydrophobic glass fibers.

[0048] 2. Preparation of super-hydrophobic coating: Using hydrophobic nano-spherical SiO2 particles, hydrophobic micron spherical SiO2 particles, hydrophobic glass fiber, epoxy resin (E51), curing agent (T31), and ethyl acetate as raw materials, the above raw materials are stirred at room temperature for 2h using a heat-collecting magnetic stirrer to prepare a super-hydrophobic coating; In the prepared super-hydrophobic coating, the mass fraction of epoxy resin (E51) is 4.4%, the mass fraction of curing agent (T31) is 1.1%, the mass fraction of 30nm hydrophobic nano-SiO2 particles is 2.05%, the mass fraction of 10μm hydrophobic micron SiO2 is 1.25%, the mass fraction of hydrophobic glass fiber is 0.50%, and the remainder is ethyl acetate;

[0049] 3. The hydrophobic nano-spherical SiO2 particles, the hydrophobic micron-spherical SiO2, and the hydrophobic glass fiber are mixed in a mass ratio of 10:6:1.5, and mixed evenly with a mechanical stirrer at a stirring speed of 200 r / min and a stirring time of 20 min to obtain a hydrophobic fiber composite powder;

[0050] 4. Pretreatment of the substrate: Use FR4 fiberglass as the substrate, clean the substrate surface with deionized water and anhydrous ethanol in turn, and dry it at 80℃ for 1h;

[0051] 5. Preparation of coating: First, a hot press is used to hot-press a polypropylene screen with an aperture of 62 μm and a substrate. The hot pressing temperature is 140°C, the holding time is 30 min, and the hot pressing pressure is 4 MPa; secondly, a spray gun is used to spray the super hydrophobic coating obtained in step 2 on the surface of the substrate. The spraying pressure is 5 Bar, the distance between the spray gun and the substrate is 10 cm, and the spray gun moves at a speed of 1.5 cm / s. Then, within 10-15 minutes after the spraying is completed, an electrostatic flocking machine is used to adsorb the hydrophobic fiber composite powder obtained in step 3 to the surface of the above-mentioned coating. The flocking voltage is 45 KV, the powder output is about 3.5 g / min, the flocking handle moving speed is 2 cm / s, and the distance between the flocking handle outlet and the coating is 15 cm. Finally, a highly wear-resistant super hydrophobic coating is obtained after curing at 60°C for 4 hours, and the obtained coating thickness is 70-100 μm.

[0052] The super-hydrophobic coating obtained in this embodiment is composed of a screen on the surface of a substrate and a cured super-hydrophobic composite. After testing, in the cured super-hydrophobic composite, the mass percentage of hydrophobic nano-spherical SiO2 is 27.31%, the mass percentage of hydrophobic micron-spherical SiO2 is 16.57%, the mass percentage of randomly arranged hydrophobic glass fibers is 4.57%, the mass percentage of hydrophobic glass fibers directionally implanted in the coating perpendicular to the coating surface is 1.29%, and the balance is epoxy resin.

[0053] The SEM image of the coating prepared in this example is as follows Figure 2 As shown in the figure, it can be seen that there are micro-nanoscale protrusions and a continuous network structure on the coating surface, which provides the coating with good hydrophobic properties.

[0054] Example 3

[0055] 1. Preparation of hydrophobic modified material: firstly, anhydrous ethanol, 1H, 1H, 2H, 2H perfluorodecyl triethoxysilane and ammonia water were ultrasonically dispersed at room temperature for 20 min in a mass ratio of 100:2:6 to obtain a modifier for standby use;

[0056] 30nm nano-SiO2 particles, 20μm micron SiO2 particles and glass fiber powder with a single filament diameter of 17μm and an aspect ratio of 50 are added to the modifier to obtain a nano-spherical SiO2 particle mixed solution (wherein the mass percentage of the nano-spherical SiO2 particles is 10.7%), a micron spherical SiO2 mixed solution (wherein the mass percentage of the micron spherical SiO2 particles is 10.7%) and a glass fiber powder mixed solution (wherein the mass percentage of the glass fiber powder is 10.7%);

[0057] Finally, a heat-collecting magnetic stirrer was used to continuously stir at a stirring speed of about 450 r / min at 20°C for 14 hours, and after drying at 70°C for 16 hours, fluorinated-modified hydrophobic nano-spherical SiO2 particles, hydrophobic micron-spherical SiO2 particles and hydrophobic glass fibers were obtained.

[0058] 2. Preparation of super-hydrophobic coating: Using hydrophobically treated SiO2 particles, glass fiber powder, epoxy resin, and ethyl acetate as raw materials, the above raw materials were stirred at room temperature for 3h using a heat-collecting magnetic stirrer to obtain a super-hydrophobic coating; in the prepared super-hydrophobic coating, the mass fraction of epoxy resin (E51) was 2.48%, the mass fraction of curing agent (T31) was 0.62%, the mass fraction of 30nm hydrophobic nano-SiO2 particles was 1.25%, the mass fraction of 20μm hydrophobic micron SiO2 was 2.05%, the mass fraction of hydrophobic glass fiber was 0.20%, and the remainder was ethyl acetate;

[0059] 3. The hydrophobic nano-spherical SiO2 particles, the hydrophobic micron-spherical SiO2, and the hydrophobic glass fiber are mixed in a mass ratio of 10:6:1.2, and mixed evenly with a mechanical stirrer at a stirring speed of 300 r / min and a stirring time of 25 min to obtain a hydrophobic fiber composite powder;

[0060] 4. Pretreatment of the substrate: 6101 aluminum alloy was used as the substrate, and the surface of the substrate was cleaned with deionized water and anhydrous ethanol in turn, and then dried at 80°C for 1h;

[0061] 5. Preparation of coating: First, a hot press is used to hot-press a polypropylene screen with an aperture of 11 μm and a substrate. The hot pressing temperature is 110°C, the holding time is 15 min, and the hot pressing pressure is 5 MPa; secondly, a spray gun is used to spray the super hydrophobic coating obtained in step 2 on the surface of the substrate. The spraying pressure is 6 Bar, the distance between the spray gun and the substrate is 10 cm, and the spray gun moves at a speed of 1.5 cm / s. Then, within 10-15 minutes after the spraying is completed, an electrostatic flocking machine is used to adsorb the hydrophobic fiber composite powder obtained in step 3 to the surface of the above-mentioned coating. The flocking voltage is 50 KV, the powder output is about 5 g / min, the flocking handle movement speed is 2 cm / s, and the distance between the flocking handle outlet and the coating is 12 cm. Finally, a highly wear-resistant super hydrophobic coating is obtained after curing at 80°C for 1.5 hours, and the obtained coating thickness is 70-100 μm.

[0062] The super-hydrophobic coating obtained in this embodiment is composed of a screen on the surface of the substrate and a cured super-hydrophobic composite. After testing, in the cured super-hydrophobic composite, the mass percentage of hydrophobic nano-spherical SiO2 is 24.82%, the mass percentage of hydrophobic micron spherical SiO2 is 31.63%, the mass percentage of randomly arranged hydrophobic glass fibers is 2.58%, the mass percentage of hydrophobic glass fibers directionally implanted in the coating perpendicular to the coating surface is 1.05%, and the balance is epoxy resin.

[0063] The actual photo of the coating prepared in this example is as follows Figure 3 shown.

[0064] Comparative Example 1

[0065] The super-hydrophobic coating used in step 2 of Example 1 does not contain hydrophobic micron-shaped spherical SiO2 particles and hydrophobic glass fiber powder. The mass fraction of hydrophobic nano-shaped spherical SiO2 in the coating is 4.50%. The remaining operations are the same as those of Example 1.

[0066] Comparative Example 2

[0067] During the preparation of the super-hydrophobic coating in step 5 of Example 1, the screen is not hot-pressed on the surface of the substrate, and the remaining operations are the same as in Example 1.

[0068] The hydrophobicity, coating hardness and wear resistance of Example 1, Example 2, Example 3 and Comparative Example 1 and Comparative Example 2 were tested using the aforementioned method, and the test results are shown in Tables 1 and 2.

[0069] Table 1 Hydrophobic performance test results of super hydrophobic coatings obtained in Examples 1 to 3 and Comparative Examples 1 to 2

[0070]

[0071] Table 2 Hardness and wear resistance test results of super hydrophobic coatings obtained in Examples 1 to 3 and Comparative Examples 1 to 2

[0072]

[0073] The above descriptions are only some embodiments of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.

Claims

1. A method for preparing a highly wear-resistant super-hydrophobic coating, characterized in that: The following steps are involved: 1) Performing hydrophobic modification treatment on nano-spherical SiO2 particles, micron-spherical SiO2 particles and glass fiber powder respectively to obtain hydrophobic nano-spherical SiO2 particles, hydrophobic micron-spherical SiO2 particles and hydrophobic glass fibers; the particle sizes of the nano-spherical SiO2 particles and micron-spherical SiO2 particles are 5-20 μm and 15-30 nm respectively; the monofilament diameter of the glass fiber is 11-17 μm, and the aspect ratio is 20-50; 2) Mix the hydrophobic nano-spherical SiO2, the hydrophobic micron-spherical SiO2, the hydrophobic glass fiber, the epoxy resin, the curing agent and the ethyl acetate at room temperature for 1.5-3 hours to obtain a super-hydrophobic coating for later use; In the super-hydrophobic coating obtained, the mass percentage shared by epoxy resin is 2.48-4.96%, the mass percentage shared by curing agent is 0.62-1.24%, the mass percentage shared by hydrophobic nano-spherical SiO2 particles is 1.25-2.05%, the mass percentage shared by hydrophobic micron spherical SiO2 particles is 1.25-2.05%, the mass percentage shared by hydrophobic glass fiber is 0.20-1.2%, and the remainder is ethyl acetate; 3) Evenly mix the hydrophobic nano-spherical SiO2 particles, the hydrophobic micron-spherical SiO2 and the hydrophobic glass fiber in a mass ratio of 10:6:1-1.5 to obtain a hydrophobic fiber composite powder for later use; 4) The surface of the substrate is cleaned and dried with deionized water and anhydrous ethanol in turn for later use; 5) hot pressing the screen onto the surface of the substrate, and then spraying the super hydrophobic coating prepared in step 2) to form a super hydrophobic coating layer; then electrostatically flocking the hydrophobic fiber composite powder prepared in step 3) onto the surface of the hydrophobic coating layer, and curing at 20-80° C. for 1.5-48 hours to obtain the highly wear-resistant super hydrophobic coating.

2. The method for preparing a highly wear-resistant super-hydrophobic coating according to claim 1, wherein The pore size of the sieve is 11-850 μm.

3. The method for preparing a highly wear-resistant super-hydrophobic coating according to claim 1, wherein The hydrophobic modification treatment in step 1) refers to the following specific steps: a) mixing anhydrous ethanol, 1H, 1H, 2H, 2H perfluorodecyl triethoxysilane and ammonia water in a mass ratio of 100:1-3:6, and ultrasonically dispersing to obtain a modifier; b) adding nano-spherical SiO2 particles, micron-spherical SiO2 and glass fiber to the modifier in a mass fraction of 7.4-10.7%, respectively, to obtain a nano-spherical SiO2 particle mixed solution, a micron-spherical SiO2 mixed solution and a glass fiber mixed solution; c) stirring the three mixed solutions obtained in step b) at 20-40°C for 8-14h, and then drying them at 55-70°C for 8-16h to obtain the hydrophobic nano-spherical SiO2 particles, hydrophobic micron-spherical SiO2 and hydrophobic glass fibers, respectively.

4. The method for preparing a highly wear-resistant super-hydrophobic coating according to claim 1, wherein Step 5) The hot pressing means that the hot pressing temperature is 110-140°C, the pressure is 3.5-5MPa, and the hot pressing time is 15-30min.

5. The method for preparing a highly wear-resistant super-hydrophobic coating according to claim 1, wherein Step 5) The coating thickness is 70-100 μm.

6. The method for preparing a highly wear-resistant super-hydrophobic coating according to claim 1, wherein: Step 5) The electrostatic flocking means that the flocking voltage is 30-50KV, the output of the hydrophobic fiber composite powder is 3-5g / min, the moving speed of the electrostatic flocking machine is 2cm / s, and the distance between the electrostatic flocking machine outlet and the coating is 10-15cm.

7. The method for preparing a highly wear-resistant super-hydrophobic coating according to claim 1, wherein: The screen is thermoplastic.

8. A highly wear-resistant super hydrophobic coating obtained as claimed in any one of claims 1 to 7.

Citation Information

Patent Citations

  • Exterior part with super-hydrophobic oleophobic coating, preparing method thereof and terminal

    CN110180762A

  • Preparation method of aluminum gusset plate with super-hydrophobic surface and aluminum gusset plate with super-hydrophobic surface

    CN110935603A

  • Micro-nano composite super-hydrophobic wear-resistant coating layer and preparation method thereof

    CN113429867A

  • Multifunctional composite coating for ice prevention and removal of wind driven generator blade

    CN116376083A

  • Transferable wear-resistant flexible super-hydrophobic film and preparation method therefor