Method for regulating and controlling texture and magnetic performance of non-oriented silicon steel through rare earth yttrium and application
By adding rare earth yttrium to non-oriented silicon steel and carrying out specific process processing, the texture control problem of non-oriented silicon steel is solved, and its magnetic performance is significantly improved, meeting the high efficiency and high frequency requirements of power equipment.
Patent Information
- Application Number
- CN202410811569.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art is difficult to effectively control the {100} texture of non-oriented silicon steel, resulting in insufficient magnetic properties, complex preparation process and low strength, making it difficult to meet the requirements of high efficiency, energy saving, miniaturization and high frequency of power equipment such as motors.
By adding an appropriate amount of rare earth yttrium to non-oriented silicon steel and adopting hot rolling, regular annealing, cold rolling and final annealing processes, the rare earth purified steel is used to reduce grain boundary activation energy, optimize texture, and improve magnetic properties.
The prepared non-oriented electrical steel plate has soft magnetic properties of low, medium and high frequency iron loss, high magnetic permeability, high magnetic induction and low noise. It is suitable for the iron core in the power electronics industry, meeting high efficiency, energy saving, miniaturization and high frequency Requirements for transformation.
Smart Images

Figure CN118996085A_ABST
Abstract
Description
[Technical field]
[0001] The invention relates to the technical field of metal material preparation, and in particular to a method and application of regulating the texture and magnetic properties of non-oriented silicon steel by using rare earth yttrium. [Background technology]
[0002] Non-oriented silicon steel is widely used in power equipment such as motors, transformers, and generators due to its excellent electromagnetic properties. In the field of motors, non-oriented silicon steel is mainly used to manufacture stator and rotor cores to improve the efficiency and performance of motors. In the field of transformers, non-oriented silicon steel is used to manufacture transformer cores to reduce iron loss and temperature rise and improve the energy efficiency of transformers. In addition, non-oriented silicon steel can also be used to manufacture cores for electrical equipment such as generators and welding machines. The magnetic properties of non-oriented silicon steel are closely related to the texture and finished grain size. Improving the {100} texture that is beneficial to magnetic properties and suppressing the unfavorable {111} texture are issues that researchers of non-oriented electrical steel have been working on. Compared with the control of Gaussian texture, the control of {100} texture in electrical steel is far from mature, and most research results remain in the laboratory development stage, making it difficult to apply industrially. In the long-term exploration, people have obtained two ideas to control the {100} texture: one is to use the initial coarse columnar crystals and initial crystallographic characteristics of ND type columnar crystals, and use the heredity of {100} texture to prepare non-oriented silicon steel. The other is to use cast and rolled thin strips, hot rolled at a medium reduction rate, normalized at 1000℃×5min, and then cold rolled at a small reduction rate for multiple passes to obtain {112} <110> The main α texture and {111} <112> The main γ texture, after annealing at 900℃, {100} <021> Both methods can form a certain strength of λ texture, but due to the complex preparation process and the low strength of λ texture, the performance of the finished plate is higher than that of the traditional CVD method, but there is still a lot of room for improvement.
[0003] Rare earth yttrium (Yttrium), as an important rare earth element, is widely distributed and exists in nature. Its unique physical and chemical properties have a wide range of applications in many fields, and its addition will also affect the microstructure and properties of electrical steel. Current research on rare earth electrical steel mainly focuses on the modification of inclusions by rare earths. Patent CN201811531176.4 uses rare earth yttrium elements to improve the warm deformation plasticity of high silicon steel slabs, and patent CN202111457976.8 uses rare earth yttrium as an inhibitor to prepare oriented silicon steel. Generally speaking, an appropriate amount of rare earth yttrium can effectively transform nano-scale square TiN and Al2O3 inclusions into spherical TiO2, Al2O3, and Y2O2S composite inclusions, and coarsen the size of the inclusions, which helps to accelerate the growth rate of the grains of the finished electrical steel plate, and reduce the activation energy of grain boundary migration, which is beneficial to grain boundary migration, thereby facilitating {100}, {113} <361> and Goss texture development.
[0004] In view of the accelerated pace of motor upgrading under the current dual-carbon background, higher requirements are placed on the performance of non-oriented electrical steel. The super-strong ability of rare earth Y to purify molten steel significantly affects the development of the microstructure and texture of non-oriented electrical steel.
[0005] Therefore, it is necessary to study a method and application of rare earth yttrium to regulate the texture and magnetic properties of non-oriented silicon steel to address the shortcomings of the existing technology and to solve or alleviate one or more of the above problems. [Summary of the invention]
[0006] In view of this, the present invention provides a method and application of regulating the texture and magnetic properties of non-oriented silicon steel with rare earth yttrium, by adding different rare earth Y in combination with subsequent processing technology, namely hot rolling, normalizing annealing, cold rolling and final annealing, using rare earth to purify molten steel, reduce grain boundary activation energy, and facilitate texture development and organization coarsening, thereby improving the magnetic properties of non-oriented electrical steel. In addition, the addition of rare earth makes the steel pure, the surface energy effect is prominent, and the advantages of {100} and {110} low surface energy will cause secondary recrystallization, significantly optimize the texture of electrical steel plates, and also facilitate the magnetic properties of non-oriented electrical steel.
[0007] On the one hand, the present invention provides a method for regulating the texture and magnetic properties of non-oriented silicon steel by rare earth yttrium, wherein the method comprises preparing a silicon-containing rare earth steel ingot and forging the ingot, and then preparing the non-oriented electrical steel through hot rolling, normalizing, cold rolling and final annealing.
[0008] According to the above aspects and any possible implementation, there is further provided an implementation, wherein the rare earth yttrium content in the silicon-containing rare earth steel ingot is controlled within a range of 0.006-0.012%.
[0009] According to the above aspects and any possible implementation, there is further provided an implementation, wherein the silicon content in the silicon-containing rare earth steel ingot is 2.5% to 3.5%.
[0010] According to the above aspects and any possible implementation, there is further provided an implementation, in which during the preparation of the silicon-containing rare earth steel ingot, rare earth yttrium is added during the solidification process.
[0011] According to the above aspects and any possible implementation, there is further provided an implementation, wherein the rare earth yttrium content in the silicon-containing rare earth steel ingot is an actual amount after full consideration of burnout.
[0012] According to the above aspects and any possible implementation, an implementation is further provided, wherein the hot rolling temperature is controlled at 1050° C. to 1150° C., rolling is performed within this temperature range, and the total hot rolling reduction rate is controlled at 80% to 90%.
[0013] According to the above aspects and any possible implementation, an implementation is further provided, wherein the normalizing annealing temperature is 900° C. to 1050° C., and the heat preservation time is 30 min to 60 min.
[0014] According to the above aspects and any possible implementation, a further implementation is provided, wherein the cold rolling reduction ratio is 60% to 80%, and the cold rolling texture significantly weakens γ( <111> / / ND) components.
[0015] According to the above aspects and any possible implementation, an implementation is further provided, wherein the final annealing temperature is 800° C. to 1150° C., and the texture of the finished plate includes {100} and {113} textures.
[0016] According to the above aspects and any possible implementation, a method for regulating the texture and magnetic properties of non-oriented silicon steel by rare earth yttrium is further provided, wherein the application is to regulate the non-oriented silicon steel by the method to obtain non-oriented electrical steel, wherein the magnetic induction intensity B of the non-oriented electrical steel is 50 ≥1.7T, core loss P under medium frequency service conditions 10 / 400 ≤1.75W / kg.
[0017] Compared with the prior art, the present invention can achieve the following technical effects:
[0018] The non-oriented electrical steel sheet prepared by the present invention has the soft magnetic properties of low medium and high frequency iron loss, high magnetic permeability, high magnetic induction and low noise. As a soft magnetic alloy widely used in the power electronics industry, it is suitable for making the iron cores of generators, motors, transformers and other instruments, and can meet the requirements of high efficiency, energy saving, miniaturization and high frequency of power electronic equipment.
[0019] Of course, any product implementing the present invention does not necessarily need to achieve all of the above-mentioned technical effects at the same time.
Brief Description of the Drawings
[0020] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0021] Figure 1 are grain orientation images after annealing of Examples 1 to 5 of the present invention, wherein (a) corresponds to Example 1, (b) corresponds to Example 2, (c) corresponds to Example 3, (d) corresponds to Example 4, and (e) corresponds to Example 5;
[0022] Figure 2 This is a 45° ODF diagram of Example 6 of the present invention after high temperature annealing. [Specific implementation method]
[0023] In order to better understand the technical solution of the present invention, the embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0024] It should be clear that the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. The singular forms "a", "said" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0026] The present invention provides a method for regulating the texture and magnetic properties of non-oriented silicon steel based on rare earth yttrium. By adding different rare earth Y in combination with subsequent processing techniques, namely hot rolling, normalizing annealing, cold rolling and final annealing, rare earth is used to purify molten steel, reduce grain boundary activation energy, facilitate texture development and organization coarsening, thereby improving the magnetic properties of non-oriented electrical steel. In addition, the addition of rare earth makes the steel pure, the surface energy effect is prominent, and the advantages of {100} and {110} low surface energy will cause secondary recrystallization, significantly optimize the texture of electrical steel plates, and also facilitate the magnetic properties of non-oriented electrical steel.
[0027] The invention prepares non-oriented electrical steel by forging a rare earth steel ingot with a silicon content of 2.5% to 3.5%, performing hot rolling, normalizing, cold rolling and final annealing.
[0028] In a specific embodiment, the rare earth yttrium content is controlled at 0.006-0.012%, and the content is the actual amount after full consideration of burnout, that is, it is added during the solidification process.
[0029] In a specific embodiment, the hot rolling temperature is controlled at 1050° C. to 1150° C., and rolling is performed within this temperature range. The total hot rolling reduction rate is controlled at 80% to 90%.
[0030] In a specific embodiment, the normalizing annealing temperature is 900° C. to 1050° C. and the insulation time is 30 min to 60 min.
[0031] In a specific embodiment, the cold rolling reduction rate is 60% to 80%, and the cold rolling texture is significantly weakened γ( <111> / / ND) components.
[0032] In a specific embodiment, the final annealing temperature is 800° C. to 1150° C., and the texture of the finished plate is mainly {100} and {113} textures.
[0033] The present invention also provides an application of a method for regulating the texture and magnetic properties of non-oriented silicon steel by rare earth yttrium, wherein the application is to regulate the non-oriented silicon steel by the above-mentioned regulation method to obtain non-oriented electrical steel, wherein the non-oriented electrical steel has excellent soft magnetic properties, and the magnetic induction intensity B under medium frequency service conditions is 50 Between 1.65 and 1.75T, core loss P 10 / 400 Between 11.5 and 13.6 W / kg.
[0034] The invention is based on the rare earth yttrium purification of molten steel to control the texture, utilizes the advantage of {100} low surface energy to induce {100} grain secondary recrystallization, optimizes the recrystallization texture, and prepares a finished product with strong {100} and medium {113} texture, significantly weakening γ( <111> / / ND) texture, which significantly improves the magnetic properties of non-oriented electrical steel sheets.
[0035] The basic principles of the present invention are as follows:
[0036] (1) Rare earth addition: An appropriate amount of rare earth yttrium can effectively transform nano-sized square TiN and Al2O3 inclusions into spherical TiO2, Al2O3, and Y2O2S composite inclusions, coarsen the size of the inclusions, which helps to accelerate the growth rate of the grains of the finished electrical steel plate and reduce the activation energy of grain boundary migration. However, excessive rare earth yttrium will lead to an increase in fine inclusions and enhanced grain boundary pinning, thereby reducing the grain size of the finished plate. In addition, excessive rare earth yttrium will affect the processing properties of steel, especially cold processing properties. Since the precipitation temperature of yttrium-based rare earths in steel is relatively high, excessive addition will reduce the bonding strength between the solid solution and the precipitates in the steel. This may cause problems such as cracks and deformation in the steel during processing.
[0037] (1) Hot rolling: Based on the academic idea that {100} oriented grains are stable under plane strain compression and not easy to recrystallize, the hot rolling shear deformation is avoided to retain the {100} texture. Low temperature lubrication rolling can be used. Low temperature lubrication rolling weakens the shear texture of the surface and subsurface of the hot rolled plate and increases the near cubic texture component of the deformation.
[0038] (2) Normalizing annealing: Normalizing annealing causes recrystallization of non-oriented electrical steel, which helps soften the structure and facilitates subsequent cold rolling. On the other hand, it improves the uniformity of the steel sheet's structure, provides a large number of shear bands for subsequent cold rolling, and promotes the development of favorable textures.
[0039] (3) Cold rolling: The cold rolling reduction rate cannot be too high. Generally speaking, the grain rotation trajectory of medium reduction rate is {100} <001> →{100} <021> →{113} <361> , that is, from cubic to α*, the rotation trajectory of the grain at large reduction rate is {100} <001> →{100} <011> , that is, from the cubic to the α line, and {100} <011> The orientation is extremely stable and cannot be eliminated by recrystallization, which is not conducive to the development of favorable texture. Medium reduction rate {113} <361> There are a large number of cubic and near-cubic nuclei, which will form a favorable recrystallization texture after annealing. In addition, if the reduction rate is too large, the γ-ray grains have higher deformation storage energy, and are more likely to recrystallize at the grain boundaries during the subsequent annealing process, forming new γ-oriented grains, which is not conducive to the magnetic properties of electrical steel.
[0040] (4) High temperature annealing: Annealing should be carried out at high temperature. On the one hand, it can increase the grain size and improve the high-frequency magnetic properties of the electrical steel plate. On the other hand, the heating rate should be controlled. Rapid heating, i.e. 50℃~100℃ / min, can control the size of the primary recrystallized grains and provide a favorable orientation environment for the secondary recrystallization of the {100} component.
[0041] Example 1
[0042] (1) Raw material preparation: The square steel ingot has a silicon content of 3.0%, a rare earth yttrium content of 0%, and a thickness of 20 mm. The steel ingot is placed in a heating furnace and heated to 1150° C.
[0043] (2) Hot rolling: The hot rolling start temperature is 1150°C, the final rolling temperature is 1000°C, the final slab is rolled to 1.2 mm, and the total hot rolling reduction rate is 94%;
[0044] (3) Cold rolling: 1.2mm rolled to 0.3mm, cold rolling reduction rate is 75%;
[0045] (4) Final annealing: The cold-rolled sheet was annealed at 800°C in a pure hydrogen atmosphere at a heating rate of 50°C / min.
[0046] Example 2
[0047] (1) Raw material preparation: The square steel ingot has a silicon content of 3.0%, a rare earth yttrium content of 0.006%, and a thickness of 20 mm. The steel ingot is placed in a heating furnace and heated to 1150°C.
[0048] (2) Hot rolling: The hot rolling start temperature is 1150°C, the final rolling temperature is 1000°C, the final slab is rolled to 1.2 mm, and the total hot rolling reduction is 94%;
[0049] (3) Cold rolling: 1.2mm rolled to 0.3mm, cold rolling reduction rate is 75%;
[0050] (4) Final annealing: The cold-rolled sheet was annealed at 800°C in a pure hydrogen atmosphere at a heating rate of 50°C / min.
[0051] Example 3
[0052] (1) Raw material preparation: The square steel ingot has a silicon content of 3.0%, a rare earth yttrium content of 0.008%, and a thickness of 20 mm. The steel ingot is placed in a heating furnace and heated to 1150° C.
[0053] (2) Hot rolling: The hot rolling start temperature is 1150°C, the final rolling temperature is 1000°C, the final slab is rolled to 1.2 mm, and the total hot rolling reduction is 94%;
[0054] (3) Cold rolling: 1.2mm rolled to 0.3mm, with a cold rolling reduction rate of 75%;
[0055] (4) Final annealing: The cold-rolled sheet was annealed at 800°C in a pure hydrogen atmosphere at a heating rate of 50°C / min.
[0056] Example 4
[0057] (1) Raw material preparation: The square steel ingot has a silicon content of 3.0%, a rare earth yttrium content of 0.010%, and a thickness of 20 mm. The steel ingot is placed in a heating furnace and heated to 1150° C.
[0058] (2) Hot rolling: The hot rolling start temperature is 1150°C, the final rolling temperature is 1000°C, the final slab is rolled to 1.2 mm, and the total hot rolling reduction is 94%;
[0059] (3) Cold rolling: 1.2mm rolled to 0.3mm, with a cold rolling reduction rate of 75%;
[0060] (4) Final annealing: The cold-rolled sheet was annealed at 800°C in a pure hydrogen atmosphere at a heating rate of 50°C / min.
[0061] Example 5
[0062] (1) Raw material preparation: The square steel ingot has a silicon content of 3.0%, a rare earth yttrium content of 0.012%, and a thickness of 20 mm. The steel ingot is placed in a heating furnace and heated to 1150° C.
[0063] (2) Hot rolling: The hot rolling start temperature is 1150°C, the final rolling temperature is 1000°C, the final slab is rolled to 1.2 mm, and the total hot rolling reduction is 94%;
[0064] (3) Cold rolling: 1.2mm rolled to 0.3mm, with a cold rolling reduction rate of 75%;
[0065] (4) Final annealing: The cold-rolled sheet was annealed at 800°C in a pure hydrogen atmosphere at a heating rate of 100°C / min.
[0066] Examples 1, 2, 3, 4, and 5 are mainly used to study the effect of rare earth yttrium content on the evolution of hot rolling, cold rolling, and recrystallization annealing structure texture under the same rolling annealing process, and to find the yttrium content with the best magnetic properties. Figure 1 As shown in the figure, the rare earth yttrium content significantly affects the hot rolling structure and texture. The steel plate without yttrium addition has obvious dynamic recrystallization structure on the surface after hot rolling. The influence of rare earth yttrium content on cold rolling structure and texture is mainly reflected in the shear band nucleation. The shear band nucleation of the steel plate without yttrium addition is mainly γ, and the shear band nucleation of the steel plate with rare earth yttrium addition is mainly near cubic. The rare earth yttrium content has a great influence on the cold rolling structure and texture. The grain size of the steel plate without yttrium addition is small, and the proportion of favorable texture is small. The grain size of the steel plate with yttrium addition is large, which significantly increases the favorable texture components. However, excessive rare earth yttrium is not conducive to the development of texture. The optimal rare earth yttrium content is 0.010%.
[0067] Comparative Example 1
[0068] (1) Raw material preparation: The square steel ingot has a silicon content of 3.0%, a rare earth yttrium content of 0.010%, and a thickness of 20 mm. The steel ingot is placed in a heating furnace and heated to 1150° C.
[0069] (2) Hot rolling: The hot rolling start temperature is 1150°C, the final rolling temperature is 1000°C, the final slab is rolled to 1.2 mm, and the total hot rolling reduction rate is 94%;
[0070] (3) Cold rolling: 1.2mm rolled to 0.3mm, with a cold rolling reduction rate of 75%;
[0071] (4) Final annealing: The cold-rolled sheet was annealed at 800°C in a pure hydrogen atmosphere at a heating rate of 100°C / min.
[0072] Comparative Example 1 is compared with Example 4 to study the effect of annealing heating rate on the microstructure, texture and magnetic properties of the finished plate. From the perspective of microscopic orientation, when the heating rate is low (50℃ / min), the grain size after annealing is 100 microns. When the heating rate is high (100℃ / min), the silicon steel strip has an abnormal growth trend, and the individual grain size is close to 500 microns. In terms of magnetic properties, the magnetic induction can reach 1.73T with rapid heating, and 1.69T with slow heating.
[0073] Example 6
[0074] (1) Raw material preparation: The square steel ingot has a silicon content of 3.0%, a rare earth yttrium content of 0.010%, and a thickness of 20 mm. The steel ingot is placed in a heating furnace and heated to 1150° C.
[0075] (2) Hot rolling: The hot rolling start temperature is 1150°C, the final rolling temperature is 1000°C, the final slab is rolled to 1.2 mm, and the total hot rolling reduction rate is 94%;
[0076] (3) Cold rolling: 1.2mm rolled to 0.3mm, with a cold rolling reduction rate of 75%;
[0077] (4) Final annealing: The cold-rolled sheet was annealed at 1150°C in a pure hydrogen atmosphere at a heating rate of 100°C / min.
[0078] Example 6 is compared with Comparative Example 1, mainly to study the effect of the final annealing temperature on the microstructure and magnetic properties of the silicon steel strip. When annealed at 1150°C, the proportion of secondary grains in the silicon steel strip exceeds 70%, and when annealed at 800°C, only a few grains have a tendency to grow abnormally, the grain size is small, and the magnetic properties are significantly lower than when annealed at 1150°C.
[0079] The performance of the finished plate of Example 6 is compared with that of the non-oriented silicon steel product for new energy vehicles in Pohang, South Korea, as shown in Table 1. It can be seen that the use of 0.010% rare earth yttrium, 94% reduction rate hot rolling, medium reduction rate cold rolling (75%), 1150℃ with rapid high temperature annealing (100℃ / min) can significantly increase the proportion of {100} and {113} textures, weaken the γ( <111> / / ND) components significantly improve the magnetic properties of non-oriented silicon steel.
[0080] Table 1
[0081]
[0082] The present invention uses silicon steel ingots containing 2.5% to 3.5% Si, 0.006% to 0.012% rare earth yttrium, and the balance Fe and inevitable impurities as raw materials, and adjusts the texture of non-oriented electrical steel through hot rolling, normalizing annealing, cold rolling and final annealing, with the {100} texture accounting for more than 35%, the {113} texture accounting for more than 30%, weakening the {111} texture, and the grain size is coarse after annealing, and the magnetic properties are significantly improved. This non-oriented silicon steel is widely used and can be used as the iron core of electrical equipment such as motors, generators, high-efficiency power supplies, inductors, etc.
[0083] The above is a detailed introduction to the method and application of rare earth yttrium to control the texture and magnetic properties of non-oriented silicon steel provided in the embodiment of the present application. The description of the above embodiment is only used to help understand the method and its core idea of the present application; at the same time, for those skilled in the art, according to the idea of the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as limiting the present application.
[0084] For example, certain words are used in the specification and claims to refer to specific components. Those skilled in the art should understand that hardware manufacturers may use different nouns to refer to the same component. This specification and claims do not use differences in names as a way to distinguish components, but use differences in the functions of components as the criteria for distinction. As mentioned throughout the specification and claims, "including" and "comprising" are open-ended terms, so they should be interpreted as "including / including but not limited to". "Approximately" means that within an acceptable error range, those skilled in the art can solve the technical problem within a certain error range and basically achieve the technical effect. The subsequent description of the specification is a preferred embodiment of the present application, but the description is for the purpose of illustrating the general principles of the present application, and is not used to limit the scope of the present application. The scope of protection of the present application shall be determined by the definition of the attached claims.
[0085] It should also be noted that the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a product or system including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such a product or system. In the absence of more restrictions, the elements defined by the sentence "comprises a ..." do not exclude the existence of other identical elements in the product or system including the elements.
[0086] It should be understood that the term "and / or" used in this article is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0087] The above description shows and describes several preferred embodiments of the present application, but as mentioned above, it should be understood that the present application is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the application concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art do not deviate from the spirit and scope of the present application, and should be within the scope of protection of the claims attached to the present application.
Claims
1. A method for regulating the texture and magnetic properties of non-oriented silicon steel by rare earth yttrium, characterized in that: The method prepares a silicon-containing rare earth steel ingot and forges the ingot, and prepares the non-oriented electrical steel through hot rolling, normalizing, cold rolling and final annealing.
2. The method according to claim 1, characterized in that The rare earth yttrium content in the silicon-containing rare earth steel ingot is controlled at 0.006-0.012%.
3. The method according to claim 1, characterized in that The silicon content in the silicon-containing rare earth steel ingot is 2.5% to 3.5%.
4. The method according to claim 1, characterized in that: During the preparation of the silicon-containing rare earth steel ingot, rare earth yttrium is added during the solidification process.
5. The method according to claim 2, characterized in that: The rare earth yttrium content in the silicon-containing rare earth steel ingot is the actual amount after fully considering the burning loss.
6. The method according to claim 1, characterized in that The hot rolling temperature is controlled at 1050° C. to 1150° C., and rolling is performed within this temperature range. The total reduction rate of hot rolling is controlled at 80% to 90%.
7. The method according to claim 1, characterized in that The normalizing annealing temperature is 900° C. to 1050° C., and the temperature is kept for 30 min to 60 min.
8. The method according to claim 1, characterized in that The cold rolling reduction rate is 60% to 80%, and the cold rolling texture is significantly weakened γ( <111> / / ND) components.
9. The method according to claim 1, characterized in that: The final annealing temperature is 800° C. to 1150° C., and the finished plate texture includes {100} and {113} textures.
10. Application of a method for regulating the texture and magnetic properties of non-oriented silicon steel by rare earth yttrium, characterized in that: The application is specifically to control the non-oriented silicon steel by the method according to any one of claims 1 to 9 to obtain non-oriented electrical steel, wherein the non-oriented electrical steel has excellent soft magnetic properties, and the magnetic induction intensity B 50 Between 1.65 and 1.75T, core loss P 10 / 400 Between 11.5 and 13.6 W / kg.
Citation Information
Patent Citations
Method for manufacturing non-oriented electrical sheet having excellent magnetic properties
CN101528385A
Non-oriented electromagnetic steel sheet
CN103582716A
High-silicon steel plate modified by rare-earth yttrium and production method thereof
CN110042312A
Non-oriented electrical steel sheet and manufacturing method therefor
CN110088328A
Non-oriented electrical steel sheet and method for preparing same
CN111566231A