Vacuum heat treatment process of high-speed steel broach

Through the combined process of segmented heating, vacuum pre-cooling, oil cooling and tempering, the problems of bending, uneven hardness and cracks of high-speed steel broaches in vacuum heat treatment are solved, and high hardness, high strength and wear resistance are achieved Performance avoids environmental pollution and operational hazards of salt furnaces.

CN118996103APending Publication Date: 2024-11-22AECC AERO SCI & TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410786481.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In vacuum heat treatment, high-speed steel broaches are prone to bending, uneven hardness, overflow of alloy elements, high-temperature remelting and adhesion between parts and fixtures, cracks caused by too fast cooling speed, and difficult deformation to correct. In addition, traditional salt furnaces are polluted by the environment and Operators are very harmful.

Method used

Using a combination of segmented heating, vacuum pre-cooling, oil cooling, tempering and sand blowing, the quenching temperature and cooling speed are controlled, and through destressing annealing, segmented heating, vacuum pre-cooling, oil cooling, tempering and sand blowing Steps to ensure the control of the heating and quenching temperature and cooling process, reduce cracks and deformation, and use VOQ2-65 dual-chamber oil quenching and air-cooled vacuum furnace equipment for treatment.

Benefits of technology

Effectively reduce cracks and deformation during vacuum quenching of high-speed steel broaches, improve hardness, strength and red hardness, avoid environmental pollution and operational hazards of salt furnaces, and ensure high hardness, high strength and wear resistance of broaches .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides a vacuum heat treatment process for a high-speed steel broach, and belongs to the technical field of heat treatment. S2, carrying out segmented heating, controlling the heating speed to be 10-15 DEG C / min, and controlling the vacuum degree to be 1.0 * 100-1.9 * 10 < 1 > Pa; s3, quenching and final heating; s4, performing vacuum pre-cooling; s5, oil cooling; s6, tempering is conducted; and S7, sand blasting. According to the vacuum heat treatment process of the high-speed steel broach, the problem that in the prior art, a salt furnace pollutes the environment is solved, the vacuum furnace is adopted for treatment, the probability that cracks are generated in the broach vacuum quenching process is reduced by selecting the quenching temperature and controlling the oil outlet temperature, and the production efficiency of the broach is improved. The broach treated by the process has the use performances of high hardness, high strength, red hardness and wear resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of heat treatment, and in particular relates to a vacuum heat treatment process for a high-speed steel broach. Background Art

[0002] High-speed steel broaches are generally used to process inner holes (round holes, spline holes, internal gears, and formed holes). This type of tool is difficult to produce. Because it is thin and long, the slenderness ratio is generally around 1:20, and it is easy to bend. Whether in mechanical processing or heat treatment, it is easy to cause bending, especially the bending caused by heat treatment is greater. After heat treatment quenching and tempering, the broach must be calibrated to the process technology requirements (length l≤900, bending ≤0.25 length l900, bending ≤0.30), and it is indeed difficult to keep the broach continuous. At present, most of the heating and quenching of high-speed steel broaches are carried out in deep well salt furnaces, but the volatilization of lava in deep well salt furnaces is harmful to the operator's body, and deep well salt furnaces will pollute the environment. Salt furnaces are facing the prospect of being eliminated.

[0003] However, the vacuum heat treatment process of broaches has the following difficulties: 1. The vacuum heat treatment of broaches uses air cooling. The broaches are thicker and longer, and it is difficult to control the uniform cooling of the airflow, resulting in large deformation; uneven hardness; overflow of alloy elements; high-temperature remelting and adhesion of parts and fixtures; 2. The vacuum heat treatment of broaches uses oil cooling. The cooling speed is too fast and it is easy to crack. Surface carburization occurs during oil cooling; 3. The final heating and quenching temperature of the broach vacuum heat treatment process is a range. The selection of the final heating and quenching temperature affects the red hardness and other properties of the broach; 4. The deformation of vacuum quenching is smaller than that of traditional quenching. The broach is longer and there is still some deformation. It has high hardness and is difficult to correct.

[0004] Therefore, a heat treatment process for high speed steel broaches is required. Summary of the invention

[0005] In order to solve the problem of imperfect vacuum heat treatment process of broaches, the present invention provides a vacuum heat treatment process of broaches, which determines the parameters of final heating and quenching temperature selection and control, cooling scheme determination, and how to implement quenching deformation correction. The correction method for reducing vacuum quenching cracks of broaches and controlling quenching deformation is a good vacuum heat treatment process for controlling quenching cracks of broaches and correcting quenching deformation after quenching.

[0006] In order to achieve the above object, the present invention provides the following technical solution, a vacuum heat treatment process for a high-speed steel broach, comprising:

[0007] S1: stress relief annealing;

[0008] S2: Heating in stages, controlling the heating rate to 10℃-15℃ / min, and the vacuum degree to 1.0×10 0Pa-1.9×10 1 Pa;

[0009] S3: quenching final heating;

[0010] S4: vacuum pre-cooling;

[0011] S5: Oil cooling;

[0012] S6: Tempering;

[0013] S7: Sand blowing.

[0014] The vacuum heat treatment process for high-speed steel broaches provided by the present invention also has the following characteristics: S1 includes heat preservation at 500-550° C. for 1-2 hours and air cooling.

[0015] The vacuum heat treatment process for high-speed steel broaches provided by the present invention also has the following characteristics: the segmented heating in S2 is divided into two stages, the first stage heating temperature is 500-650°C, and the second stage heating temperature is 800-850°C.

[0016] The vacuum heat treatment process for the high-speed steel broach provided by the present invention also has the characteristic that the quenching temperature is 1170-1290°C.

[0017] The vacuum heat treatment process of the high-speed steel broach provided by the present invention also has the following characteristics: the quenching temperatures of high-speed steel broaches of different material types are as follows:

[0018] Material Model Quenching temperature Grain size W18Cr4V 1280±10℃ 9-10 W12Cr4MO4V 1255±5℃ 9.5-10.5 W6MO5Cr4V2 1230±10℃ 10-11 W2MO9Cr4V2CO8 1180±10℃ 10-10.5 W6MO5Cr4V2AL 1210±10℃ 10-11 .

[0019] The vacuum heat treatment process for high-speed steel broaches provided by the present invention also has the following characteristics: the heat preservation time t = a × k × D,

[0020] Among them, a is the heating coefficient, k is the furnace loading correction coefficient, D is the effective thickness of the workpiece, and k = 1-1.5.

[0021] The vacuum heat treatment process for high-speed steel broaches provided by the present invention also has the following characteristics: the heating coefficient is as follows:

[0022]

[0023] The vacuum heat treatment process for high-speed steel broaches provided by the present invention also has the following feature: the oil in S5 is cooled to 200-300° C. and then discharged.

[0024] The vacuum heat treatment process for high-speed steel broaches provided by the present invention also has the following characteristics: the tempering temperature in S6 is 550±10° C., and the time interval between the second tempering and the first tempering does not exceed 8 hours.

[0025] The vacuum heat treatment process for high-speed steel broaches provided by the present invention also has the characteristic that the process further comprises quality inspection of the broaches after sand blasting.

[0026] Beneficial effects:

[0027] The vacuum heat treatment process for high-speed steel broaches provided by the present invention solves the environmental pollution problem of salt furnaces in the prior art. A vacuum furnace is used for treatment, and the probability of cracks occurring during the vacuum quenching of the broaches is reduced by selecting the quenching temperature and controlling the oil outlet temperature. The broaches treated by this process achieve high hardness, high strength, red hardness, and wear resistance. DETAILED DESCRIPTION

[0028] The present invention is further described in detail below in conjunction with examples, but it should be noted that these implementation modes are not limitations of the present invention, and any equivalent transformations or substitutions in functions, methods, or structures made by ordinary technicians in the field based on these implementation modes are all within the protection scope of the present invention.

[0029] In the description of the embodiments of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate orientations or positional relationships as shown, which are only for the convenience of describing the invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the invention.

[0030] In addition, the terms "first", "second", "third", etc. are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first", "second", etc. may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "plurality" means two or more.

[0031] The terms "installed", "connected" and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the invention can be understood according to specific circumstances.

[0032] The embodiment of the present invention provides a vacuum heat treatment process for a high-speed steel broach, which is implemented using a VOQ2-65 double-chamber oil quenching and air cooling vacuum furnace device, and includes the following steps:

[0033] S1: stress relief annealing;

[0034] S2: Heating in stages, controlling the heating rate to 10℃-15℃ / min, and the vacuum degree to 1.0×10 0 Pa-1.9×10 1 Pa;

[0035] S3: quenching final heating;

[0036] S4: vacuum pre-cooling;

[0037] S5: Oil cooling;

[0038] S6: Tempering;

[0039] S7: Sand blowing.

[0040] In the above embodiment, the vacuum degree is controlled at 1.0×10 0 Pa-1.9×10 1 Pa can prevent high alloy steel parts from easily leaking out alloy elements at high temperature in vacuum. After several tests, the spark direct reading spectrometer was used to detect the material composition, and no alloy element loss was found before and after vacuum quenching.

[0041] In some embodiments, S1 includes maintaining the temperature at 500-550° C. for 1-2 hours and air cooling to eliminate processing stress and other stresses.

[0042] In some embodiments, the stepwise heating in S2 is divided into two stages, the first stage heating temperature is 500-650° C., and the second stage heating temperature is 800-850° C. In the above embodiments, the spectrum detection before and after the heat treatment did not find the alloy element loss phenomenon, and the two-stage heating can reduce thermal stress and shorten the high temperature heating time.

[0043] In some embodiments, the quenching temperature is 1170-1290° C. In the above embodiments, the final determination of the quenching temperature is determined according to the following principles: first, the carbon content of the raw material is compared with the standard. If the carbon content is closer to the upper limit, the final heating temperature can be lowered; if the carbide size, band distribution and morphology are compared with the standard, the carbide segregation is serious, and the final heating temperature can be lowered.

[0044] In some embodiments, the quenching temperature of the following commonly used material types of high-speed steel broaches is as follows:

[0045]

[0046]

[0047] In some embodiments, the holding time t = a × k × D,

[0048] Among them, a is the heating coefficient, k is the furnace loading correction coefficient, D is the effective thickness of the workpiece, and k = 1-1.5.

[0049] In some embodiments, the heating coefficient is as follows:

[0050]

[0051] In some embodiments, in S4: in order to slow down the entire cooling process, the vacuum heating chamber is first exited, and precooled in the quenching oil chamber to reduce the temperature to below 900°C, which can reduce surface carburization during oil cooling and reduce quenching stress. Lowering the temperature of the parts to below 900°C can solve the problem of surface carbon increase during oil cooling. The spark direct reading spectrometer detects the material composition, and no significant increase in carbon is found before and after vacuum quenching.

[0052] In some embodiments, the oil in S5 is cooled to 200-300℃ and the oil is discharged. In this embodiment, the oil cooling operation is not easy to master, the deformation is large, and cracks may appear. The cooling in oil should not be too long, and the oil outlet temperature should not be too low. Generally, for a broach with an effective thickness of 25mm, cooling for 6-8 minutes is better. The oil is discharged at about 200℃-300℃ and straightened while hot.

[0053] In some embodiments, the straightening is performed while hot after oil cooling, and air cooling is performed to about 150°C. At this time, the temperature is below the Ms point, austenite is transforming into martensite, and there is a lot of residual austenite. However, the broach has a particularly good plasticity stage, which is conducive to straightening. The opportunity of transformation from austenite to martensite is seized for timely straightening.

[0054] In some embodiments, the tempering temperature in S6 is 550±10°C, and the time interval between the second tempering and the first tempering does not exceed 8 hours. There is a lot of residual austenite after quenching, and generally 3 or 4 temperings are required to reduce the residual austenite. When the residual austenite transforms into martensite, it is timely straightened. For the first tempering, the amount of residual austenite is still large, the plasticity is good, and the straightening effect is good. However, the straightening effect of the second and third tempering is poor. The residence time of the broach after quenching cannot exceed 24 hours, the time interval between the second tempering and the first tempering should not exceed 8 hours, and the tempering temperature of the broach is 550±10°C.

[0055] In some embodiments, S7 includes dipping the broach in kerosene and inspecting for cracks after sandblasting.

[0056] In some embodiments, the process further includes a quality inspection of the broach after sand blasting. The quality inspection includes metallographic inspection, hardness inspection, deformation inspection and appearance inspection to confirm that the internal and external quality of the broach meets the requirements. The metallographic structure is tempered martensite + carbide + a small amount of retained austenite, and there is no overheating and insufficient tempering. The tempering degree is qualified when the retained retained austenite is less than level 2.

[0057] In some embodiments, the part and the fixture are easily melted and adhered under vacuum and high temperature, and a ceramic sheet or a stainless steel mesh can be placed between the part and the fixture.

[0058] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention shall be included in the protection scope of the present invention. The above description is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present invention. These improvements and variations should also be regarded as the protection scope of the present invention.

Claims

1. A vacuum heat treatment process for high-speed steel broaches, characterized in that: include: S1: stress relief annealing; S2: Heating in stages, controlling the heating rate to 10℃-15℃ / min, and the vacuum degree to 1.0×10 0 Pa-1.9×10 1 Pa; S3: quenching final heating; S4: vacuum pre-cooling; S5: Oil cooling; S6: Tempering; S7: Sand blowing.

2. The vacuum heat treatment process for high-speed steel broaches according to claim 1, characterized in that: The S1 includes maintaining the temperature at 500-550° C. for 1-2 hours and air cooling.

3. The vacuum heat treatment process for high speed steel broaches according to claim 1, characterized in that: The stepwise heating in S2 is divided into two stages, the first stage heating temperature is 500-650°C, and the second stage heating temperature is 800-850°C.

4. The vacuum heat treatment process for high-speed steel broaches according to claim 1, characterized in that: The quenching temperature is 1170-1290°C.

5. The vacuum heat treatment process for high speed steel broaches according to claim 4, characterized in that: The quenching temperature of high speed steel broaches of different material types is as follows: 。 6. The vacuum heat treatment process for high speed steel broaches according to any one of claims 3 to 5, characterized in that: Insulation time t = a × k × D, Among them, a is the heating coefficient, k is the furnace loading correction coefficient, D is the effective thickness of the workpiece, and k = 1-1.

5.

7. The vacuum heat treatment process for high speed steel broaches according to claim 6, characterized in that: The heating coefficients are as follows: 。 8. The vacuum heat treatment process for high speed steel broaches according to claim 1, characterized in that: The oil in S5 is cooled to 200-300°C and discharged.

9. The vacuum heat treatment process for high-speed steel broaches according to claim 1, characterized in that: The tempering temperature in S6 is 550±10° C., and the time interval between the second tempering and the first tempering is no more than 8 hours.

10. The vacuum heat treatment process for high speed steel broaches according to claim 1, characterized in that: The process also includes a quality inspection of the broach after sandblasting.

Citation Information

Cited By

  • High-speed steel vacuum oil quenching surface white and bright layer control process

    CN121852696A

  • Process for controlling white layer on surface of high speed steel vacuum oil quenched

    CN121852696B