Wet paper-based friction material as well as preparation method and application thereof
By using bent glass fiber wire and pressurized patch technology in paper-based friction materials, the friction performance of wet paper-based friction materials is improved, and the static friction of existing paper-based friction materials under high-speed and heavy-load conditions is solved. The problem of low coefficient has achieved the improvement of high static friction coefficient and dynamic pressure withstand voltage.
Patent Information
- Application Number
- CN202411103544.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
AI Technical Summary
The existing paper-based friction materials have low static friction coefficient and poor friction performance under high-speed and heavy-load conditions, which limits the excellent maneuverability of the mechanical system.
Wet paper-based friction materials are used, including core plate steel sheets and paper sheets that are bonded to core plate steel sheets. The raw materials for the preparation of paper sheets include paper-based friction materials, glass fiber wires and water. The glass fiber wires are bent and have a surface Set up barbs and prepare them through steps such as beating, papermaking, punching and glue dipping, combined with pressurized patch technology to improve friction performance.
The static friction coefficient and dynamic friction coefficient of wet paper-based friction materials are significantly improved, the wear rate is reduced, the dynamic pressure withstand and energy load value is enhanced, and the friction performance and service life is improved.
Smart Images

Figure CN118996914A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of friction materials, and in particular relates to a wet paper-based friction material and a preparation method and application thereof. Background Art
[0002] The friction clutch uses the friction between the friction pairs to achieve the engagement, separation or asynchronous operation of the active and driven parts of the mechanical mechanism or machine; the friction brake uses the friction between the friction pairs to achieve the deceleration, speed limit or stop of the mechanical mechanism or machine. The friction pair consists of a friction plate (friction material) and a dual plate, and the performance of the friction pair mainly depends on the friction and wear performance of the friction plate.
[0003] At present, high-performance friction materials used in high-speed and heavy-load conditions mainly include: powder metallurgy friction materials, carbon / carbon friction materials, ceramic-based friction materials, semi-metallic friction materials and paper-based friction materials. Chinese patent CN102942898A discloses a paper-based friction material that can increase the friction coefficient of the friction plate and extend its service life. However, the static friction coefficient of the above-mentioned paper-based friction material is 0.15, which is still relatively low, and the friction performance is poor, which restricts the excellent maneuverability of the mechanical system. Summary of the invention
[0004] The purpose of the present invention is to provide a wet paper-based friction material and a preparation method and application thereof. The wet paper-based friction material provided by the present invention has a static friction coefficient of ≥0.164, a high static friction coefficient and good friction performance.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] The present invention provides a wet paper-based friction material, comprising a core plate steel sheet and a paper sheet attached to one side or both sides of the core plate steel sheet; the raw materials for preparing the paper sheet include paper-based friction material, glass fiber yarn and water;
[0007] The glass fiber yarn is bent, and a plurality of barbs are arranged on the surface.
[0008] Preferably, the raw materials for preparing the paper-based friction material include, by weight, 22 to 25 parts of cotton pulp, 16 to 17 parts of carbon fiber, 6 to 8 parts of aramid fiber, 10 to 12 parts of petroleum coke, 5 to 8 parts of zirconium silicate, 5 to 8 parts of friction powder, 5 to 8 parts of feldspar powder, 3 to 5 parts of diatomaceous earth and 3 to 5 parts of latex.
[0009] Preferably, the mass ratio of the paper-based friction material to water is 24.5-25.5:1;
[0010] The ratio of the total mass of the paper-based friction material and water to the mass of the glass fiber yarn is 20 to 50:1.
[0011] Preferably, the friction powder includes aluminum oxide, silicon dioxide and calcium carbonate.
[0012] Preferably, the method for preparing the paper sheet comprises the following steps:
[0013] Mixing the paper-based friction material and water, and beating the mixture to obtain a mixed slurry;
[0014] The mixed slurry and glass fiber yarn are mixed to make paper to obtain a prefabricated wet paper sheet;
[0015] Punching the prefabricated wet paper sheet to obtain a prefabricated wet paper disc;
[0016] The wet paper disc is dipped in glue and then cured for the first time to obtain a paper sheet.
[0017] Preferably, the beating degree is 20-35°SR, the rotation speed is 1950-2050rpm, and the time is 150-180min.
[0018] Preferably, the dipping solution used in the dipping comprises modified resin glue and ethanol;
[0019] The volume ratio of the modified resin glue to ethanol is 29-30:70-71.
[0020] The present invention provides a method for preparing the wet paper-based friction material described in the above technical solution, comprising the following steps:
[0021] The paper sheet and the core plate steel sheet are laminated and then cured to obtain a wet paper-based friction material.
[0022] Preferably, the temperature of the patch is 180-185°C;
[0023] The patch method includes a pressurized patch, and the pressure of the pressurized patch is 230-240 kg / cm 3 , the holding time is 5-6min / mm;
[0024] The temperature of the second curing is 175-180° C., and the time is 1.8-2 hours.
[0025] The present invention provides the application of the wet paper-based friction material described in the above technical solution or the wet paper-based friction material prepared by the preparation method described in the above technical solution in a wet clutch brake system.
[0026] The present invention provides a wet paper-based friction material, comprising a core plate steel sheet and a paper sheet attached to one or both sides of the core plate steel sheet. The wet paper-based friction material provided by the present invention has the advantages of high static friction coefficient and dynamic friction coefficient and low wear rate, and high dynamic pressure resistance and energy load values; moreover, the present invention adopts bent glass fiber filaments, and the surface of the glass fiber filaments has a plurality of barbs, which can radially hook and fix the paper sheet in the wet paper-based friction material, improve the structural firmness of the paper sheet, reduce the molding thickness error, improve the shear stress and wear resistance coefficient of the paper sheet, and thus improve the friction performance of the wet paper-based friction material.
[0027] The present invention provides a method for preparing the wet paper-based friction material described in the above technical solution. The preparation method provided by the present invention is simple to operate, low in cost, and suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 Schematic diagram of glass fiber yarn, wherein 1 is the glass fiber yarn matrix and 2 is the barb. DETAILED DESCRIPTION
[0029] The present invention provides a wet paper-based friction material, comprising a core plate steel sheet and a paper sheet attached to one side or both sides of the core plate steel sheet; the raw materials for preparing the paper sheet include paper-based friction material, glass fiber yarn and water;
[0030] The glass fiber yarn is bent, and a plurality of barbs are arranged on the surface.
[0031] Unless otherwise specified, the materials and equipment used in the present invention are all commercially available products in the art.
[0032] In the present invention, the raw materials for preparing the paper-based friction material preferably include, by weight, 22 to 25 parts of cotton pulp, 16 to 17 parts of carbon fiber, 6 to 8 parts of aramid fiber, 10 to 12 parts of petroleum coke, 5 to 8 parts of zirconium silicate, 5 to 8 parts of friction powder, 5 to 8 parts of feldspar powder, 3 to 5 parts of diatomaceous earth and 3 to 5 parts of latex.
[0033] In parts by mass, the paper-based friction material preferably includes 22 to 25 parts of cotton pulp, and more preferably 23 to 24 parts.
[0034] Calculated by mass percentage of the cotton pulp, the paper-based friction material preferably includes 16 to 17 parts of carbon fibers, and more preferably 16 or 17 parts.
[0035] Calculated by mass fraction of the cotton pulp, the paper-based friction material preferably includes 6 to 8 parts of aramid fibers, more preferably 6 to 7 parts.
[0036] Calculated by mass fraction of the cotton pulp, the paper-based friction material preferably includes 10 to 12 parts of petroleum coke, and more preferably 10 to 11 parts.
[0037] Calculated by mass fraction of the cotton pulp, the paper-based friction material preferably includes 5 to 8 parts of zirconium silicate, and more preferably 6 to 7 parts.
[0038] The paper-based friction material preferably includes 5 to 8 parts of friction powder, more preferably 6 to 7 parts, based on the mass fraction of the cotton pulp. In the present invention, the friction powder preferably includes aluminum oxide, silicon dioxide and calcium carbonate.
[0039] Calculated by mass fraction of the cotton pulp, the paper-based friction material preferably includes 5 to 8 parts of feldspar powder, and more preferably 6 to 7 parts.
[0040] Calculated by mass fraction of the cotton pulp, the paper-based friction material preferably includes 3 to 5 parts of diatomaceous earth, and more preferably 3 to 4 parts.
[0041] Calculated by mass fraction of the cotton pulp, the paper-based friction material preferably includes 3 to 5 parts of latex, more preferably 3 to 4 parts.
[0042] In the present invention, the mass ratio of the paper-based friction material and water is preferably 24.5-25.5:1, more preferably 24.7-25.3:1, and most preferably 24.8-25:1; the ratio of the total mass of the paper-based friction material and water to the mass of the glass fiber yarn is preferably 20-50:1, more preferably 25-45:1, and most preferably 30-40:1.
[0043] In the present invention, the method for preparing the paper sheet preferably comprises the following steps:
[0044] Mixing the paper-based friction material and water, and beating the mixture to obtain a mixed slurry;
[0045] The mixed slurry and glass fiber yarn are mixed to make paper to obtain a prefabricated wet paper sheet;
[0046] Punching the prefabricated wet paper sheet to obtain a prefabricated wet paper disc;
[0047] The wet paper disc is dipped in glue and then cured for the first time to obtain a paper sheet.
[0048] The invention mixes the paper-based friction material and water, and performs pulping to obtain a mixed pulp.
[0049] In the present invention, the beating degree of the beating is preferably 20-35°SR, more preferably 25-30°SR, and most preferably 22-24°SR; the beating speed is preferably 1950-2050rpm, more preferably 1970-2020rpm, and most preferably 1980-2000rpm; the beating time is preferably 150-180min, more preferably 155-175min, and most preferably 160-170min. The beating degree, i.e., the beating degree, indicates the degree of water filtration of the slurry when paper is made on a copper mesh. The present invention is beneficial to improving the quality of the mixed slurry (paper pulp) by controlling the beating degree, thereby improving the friction performance of the wet paper-based friction material.
[0050] In the present invention, the paper-based friction material and water are mixed and the beating preferably comprises the following steps:
[0051] Mixing water and cotton pulp, performing first beating, and obtaining a first beating pulp;
[0052] The first beating slurry, carbon fiber and aramid fiber are mixed, and a second beating is performed to obtain a second beating slurry;
[0053] The second beating slurry, petroleum coke, zirconium silicate, friction powder, feldspar powder and carbon black diatomaceous earth are mixed, and a third beating is performed to obtain a third beating slurry;
[0054] The third beating slurry is mixed with latex and a fourth beating is performed.
[0055] In the present invention, the beating degree of the first beating is preferably 20-30°SR, more preferably 22-24°SR, and most preferably 22-23°SR; the rotation speed of the first beating is preferably 1950-2050rpm, more preferably 1970-2030rpm, and most preferably 1980-2000rpm; the time of the first beating is preferably 20-25min, more preferably 21-24min, and most preferably 22-23min.
[0056] In the present invention, the beating degree of the second beating is preferably 25-35°SR, more preferably 27-32°SR, and most preferably 28-30°SR; the rotation speed of the second beating is preferably 1950-2050rpm, more preferably 1970-2030rpm, and most preferably 1980-2000rpm; the time of the second beating is preferably 28-32min, more preferably 29-31min, and most preferably 29-30min.
[0057] In the present invention, the beating degree of the third beating is preferably 25-32°SR, more preferably 28-30°SR, and most preferably 29-30°SR; the rotation speed of the third beating is preferably 1950-2050rpm, more preferably 1970-2030rpm, and most preferably 1980-2000rpm; the time of the third beating is preferably 55-75min, more preferably 58-72min, and most preferably 62-68min.
[0058] In the present invention, the beating degree of the fourth beating is preferably 25-30°SR, more preferably 27-29°SR, and most preferably 28-29°SR; the rotation speed of the fourth beating is preferably 1950-2050rpm, more preferably 1970-2030rpm, and most preferably 1980-2000rpm; the time of the fourth beating is preferably 44-52min, more preferably 46-50min.
[0059] The present invention adopts a specific mixing sequence according to different beating degrees of raw materials, and performs beating for multiple times, so that all raw materials can form a uniform slurry after multiple beatings.
[0060] After obtaining the mixed slurry, the present invention mixes the mixed slurry with glass fiber filaments to make paper to obtain a prefabricated wet paper sheet.
[0061] In the present invention, the thickness ratio of the prefabricated wet paper sheet to the wet paper-based friction material is preferably 16 to 18: 1, more preferably 16.5 to 17.5: 1, and most preferably 17 to 17.2: 1. In the present invention, the papermaking is preferably carried out in a hand paper machine.
[0062] After obtaining the prefabricated wet paper sheet, the present invention punches the prefabricated wet paper sheet to obtain a prefabricated wet paper disc. The present invention punches the inner and outer circles of the prefabricated wet paper sheet according to the product drawing size of the wet paper-based friction material to obtain a prefabricated wet paper disc.
[0063] After obtaining the prefabricated wet paper disc, the present invention performs a first curing after the wet paper disc is dipped in glue to obtain a paper sheet.
[0064] In the present invention, the dipping solution used for the dipping preferably includes modified resin glue and ethanol; the volume ratio of the modified resin glue and ethanol is preferably 29-30:70-71, and specifically preferably 29:71 or 30:70.
[0065] In the present invention, the dipping preferably includes vacuum dipping; the vacuum dipping preferably includes the following steps: vacuumizing the prefabricated wet paper disc and then performing pressure-maintaining dipping.
[0066] In the present invention, the vacuum degree of the vacuum pumping is preferably 0.07-0.09 Pa, more preferably 0.08-0.09 Pa; the vacuum pumping time is preferably 14-16 min, more preferably 14-15 min. The present invention preferably has no special limitation on the time of the pressure-maintaining dipping, as long as the dipping solution can be completely soaked.
[0067] After the dipping is completed, the present invention preferably further comprises drying the dipped paper sheet obtained by the dipping to obtain a dried paper sheet.
[0068] In the present invention, the drying preferably includes the first drying, the second drying and the third drying, draining, natural drying and complete drying in sequence. In the present invention, the first drying preferably includes draining, and the time of the first drying is preferably 2 to 3 hours, more preferably 2.2 to 2.8 hours, and most preferably 2.4 to 2.6 hours; the second drying preferably includes natural drying, and the time of the second drying is preferably 2 minutes; the third drying preferably includes drying and / or sun drying; the drying temperature is preferably 175 to 180°C, more preferably 176 to 179°C, and most preferably 177 to 178°C. The present invention does not specifically limit the time of sun drying, as long as the drying paper sheet can be completely dried.
[0069] In the present invention, the first curing preferably includes a first heating, a first heat preservation, a second heating, a second heat preservation, a third heating and a third heat preservation in sequence. The present invention has no particular limitation on the heating rates of the first heating, the second heating and the third heating, as long as the temperature reaches the heat preservation temperature. In the present invention, the temperature of the first heat preservation is preferably 110-120°C, more preferably 112-118°C, and most preferably 114-116°C; the time of the first heat preservation is preferably 18-20min, and more preferably 18-19min; the temperature of the second heat preservation is preferably 135-140°C, more preferably 136-139°C, and most preferably 137-138°C; the time of the second heat preservation is preferably 25-30min, more preferably 26-29min, and most preferably 27-28min; the temperature of the third heat preservation is preferably 160-165°C, more preferably 161-164°C, and most preferably 162-163°C; the time of the third heat preservation is preferably 1.4-1.5h, more preferably 1.42-1.48h, and most preferably 1.44-1.46h. In the present invention, the second heat preservation and the third temperature rise preferably also include degassing.
[0070] The present invention provides a method for preparing the wet paper-based friction material described in the above technical solution, comprising the following steps: performing second curing after pasting a paper sheet and a core plate steel sheet to obtain the wet paper-based friction material.
[0071] In the present invention, the core plate steel sheet preferably also includes pretreatment before use. In the present invention, the pretreatment preferably includes the following steps: punching the core plate steel sheet into inner and outer circles, positioning with the inner hole, performing heat flattening and then stacking and heat preservation, and then performing heat treatment, grinding, cleaning and gluing and drying in sequence. In the present invention, the temperature of the heat flattening is preferably 650-680°C, more preferably 660-675°C, and most preferably 665-670°C; the time of stacking and heat preservation is preferably 2-2.5h, more preferably 2.1-2.4h, and most preferably 2.2-2.3h. In the present invention, the Rockwell hardness of the core plate steel sheet after the heat treatment is preferably 48-53, more preferably 49-52, and most preferably 50-51. In the present invention, the cleaning preferably includes water washing and organic solvent washing in sequence; the organic solvent used in the organic solvent washing is preferably acetone. In the present invention, the glue used for gluing preferably includes 204 glue. The present invention punches out the core plate steel sheet (punches inner and outer circles), then positions it based on the inner hole, ensures the flatness of the obtained wet paper-based friction material by stacking it positively and negatively for heat insulation, and performs heat treatment (quenching) to improve the friction performance of the wet paper-based friction material.
[0072] In the present invention, the temperature of the patch is preferably 180-185°C, more preferably 181-184°C, and most preferably 182-183°C. The patch preferably includes a pressurized patch, and the pressure of the pressurized patch is preferably 230-240 kg / cm 3 , more preferably 232 to 238 kg / cm 3 , the most preferred is 234-236 kg / cm 3 The holding time of the pressurized patch is preferably 5 to 6 min / mm, more preferably 5.2 to 5.8 min / mm, and most preferably 5.4 to 5.6 min / mm. In the present invention, the patch is preferably vulcanized in a hot plate vulcanizer.
[0073] In the present invention, the temperature of the second curing is preferably 175-180° C., more preferably 176-179° C., most preferably 177-178° C.; the time of the second curing is preferably 1.8-2 h, more preferably 1.8-1.9 h.
[0074] The present invention provides the application of the wet paper-based friction material described in the above technical solution or the wet paper-based friction material prepared by the preparation method described in the above technical solution in a wet clutch brake system. In the present invention, the wet clutch brake system preferably includes an automobile automatic transmission, a torque converter, a differential, a torque manager, a synchronizer ring, a motorcycle clutch or an engineering machinery gearbox. The wet paper-based friction material provided by the present invention is light in weight, high in specific strength and friction coefficient, low in wear rate, high in dynamic pressure resistance and energy load value, long in service life, less in fiber shedding phenomenon, better in heat decay resistance, and has broad application prospects in high and low speed small torque (such as motorcycles), high and low speed medium torque (such as automatic transmission cars) or high and low speed large torque (machine tools, ships, engineering machinery and agricultural machinery).
[0075] In order to further illustrate the present invention, a wet paper-based friction material provided by the present invention and its preparation method and application are described in detail below in conjunction with the accompanying drawings and embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0076] In all embodiments and comparative examples of the present invention, the schematic diagram of the glass fiber yarn is as follows Figure 1 As shown, 1 is a glass fiber matrix, 2 is a barb; the diameter of the hand-made paper machine is 350 mm; the composition of the dipping solution is: 30 v / v% modified resin glue and 70 v / v% anhydrous ethanol.
[0077] Example 1
[0078] The raw materials for preparing the wet paper-based friction material are as follows, by mass: 22 parts of cotton pulp, 16 parts of carbon fiber, 7 parts of aramid fiber, 12 parts of petroleum coke, 7 parts of zirconium silicate, 5 parts of friction powder, 8 parts of feldspar powder, 5 parts of diatomaceous earth, 5 parts of latex, 2 parts of glass fiber and 25 parts of water.
[0079] The preparation method of the wet paper-based friction material is as follows:
[0080] Punch the inner and outer circles of the core plate steel sheet to remove burrs, position it with the inner hole, perform heat flattening at 660℃, fold it positively and negatively and keep it warm for 2.5h, and then perform heat treatment to a Rockwell hardness of HRC52.8. Grind both sides of the core plate steel sheet, clean it with a degreasing agent on a cleaning machine to remove surface oil stains, and then dry it. Scrub both sides of the core plate steel sheet with acetone, apply glue to the core plate steel sheet on a glue coating machine, and let it dry for use.
[0081] Add water to a beating tank, first add cotton pulp, and beat at a rotation speed of 1950 rpm for 22 minutes, at which the beating degree is 25°SR, then add carbon fiber and aramid fiber, and beat at a rotation speed of 2050 rpm for 29 minutes, at which the beating degree is 26°SR, then add petroleum coke, zirconium silicate, friction powder, feldspar powder and carbon black diatomaceous earth, and beat at a rotation speed of 1990 rpm for 60 minutes, at which the beating degree is 28°SR, finally add latex, and beat at a rotation speed of 2050 rpm for 48 minutes, at which the beating degree is 27°SR, to obtain a mixed slurry;
[0082] The obtained mixed slurry was mixed with glass fiber filaments, and placed in a hand paper machine for papermaking to obtain a prefabricated wet paper sheet with a thickness of 1.22 mm;
[0083] Punching the obtained prefabricated wet paper sheet into inner and outer circles to obtain a prefabricated wet paper disc;
[0084] The obtained prefabricated wet paper discs were put into a basket, the prefabricated wet paper discs were separated by wire mesh, the basket was sunk into the impregnation device, the cover was tightened, the vacuum pump was turned on, and the vacuum was evacuated at a vacuum degree of 0.07 Pa for 16 minutes, and then the vacuum pump was turned off, and the impregnation solution was added to perform impregnation until it was soaked, and the basket containing the impregnated prefabricated wet paper discs was taken out and drained for 2.3 hours to obtain the impregnated prefabricated paper discs;
[0085] The obtained pre-impregnated paper sheet was naturally dried for 2 minutes, and then dried at 175°C until dry. The dried paper sheet was taken out and cooled to room temperature, and then placed in an oven. The temperature in the oven was raised to 112°C and the insulation time was 19 minutes. After the insulation was completed, the temperature in the oven was raised to 135°C and the insulation time was 30 minutes. The oven door was opened to vent once, and then the temperature in the oven was raised to 161°C and the insulation time was 1.41 hours to obtain a paper sheet.
[0086] The core steel sheet and paper sheet are put into the hot plate vulcanizer at 180℃ and 232kg / cm 3 The wet paper-based friction material was obtained by pressing the sheet under the conditions of (holding time of 5.2 min / mm) and drying at 175° C. for 1.82 h.
[0087] Example 2
[0088] The raw materials for preparing the wet paper-based friction material are as follows, in parts by mass: 24 parts of cotton pulp, 17 parts of carbon fiber, 8 parts of aramid fiber, 12 parts of petroleum coke, 6 parts of zirconium silicate, 8 parts of friction powder, 7 parts of feldspar powder, 4 parts of diatomaceous earth, 3 parts of latex, 3 parts of glass fiber and 24 parts of water.
[0089] The preparation method of the wet paper-based friction material is as follows:
[0090] Punch the inner and outer circles of the core plate steel sheet to remove burrs, position it with the inner hole, perform heat flattening at 660℃, fold it positively and negatively and keep it warm for 2.5h, and then perform heat treatment to a Rockwell hardness of HRC52.8. Grind both sides of the core plate steel sheet, clean it with a degreasing agent on a cleaning machine to remove surface oil stains, and then dry it. Scrub both sides of the core plate steel sheet with acetone, apply glue to the core plate steel sheet on a glue coating machine, and let it dry for use.
[0091] Add water to a beating tank, first add cotton pulp, and beat at a rotation speed of 1950 rpm for 22 minutes, at which the beating degree is 25°SR, then add carbon fiber and aramid fiber, and beat at a rotation speed of 2050 rpm for 29 minutes, at which the beating degree is 26°SR, then add petroleum coke, zirconium silicate, friction powder, feldspar powder and carbon black diatomaceous earth, and beat at a rotation speed of 1990 rpm for 60 minutes, at which the beating degree is 28°SR, finally add latex, and beat at a rotation speed of 2050 rpm for 48 minutes, at which the beating degree is 27°SR, to obtain a mixed slurry;
[0092] The obtained mixed slurry was mixed with glass fiber filaments, and placed in a hand paper machine for papermaking to obtain a prefabricated wet paper sheet with a thickness of 1.22 mm;
[0093] Punching the obtained prefabricated wet paper sheet into inner and outer circles to obtain a prefabricated wet paper disc;
[0094] The obtained prefabricated wet paper discs were put into a basket, the prefabricated wet paper discs were separated by wire mesh, the basket was sunk into the impregnation device, the cover was tightened, the vacuum pump was turned on, and the vacuum was evacuated at a vacuum degree of 0.07 Pa for 16 minutes, and then the vacuum pump was turned off, and the impregnation solution was added to perform impregnation until it was soaked, and the basket containing the impregnated prefabricated wet paper discs was taken out and drained for 2.3 hours to obtain the impregnated prefabricated paper discs;
[0095] The obtained pre-impregnated paper sheet was naturally dried for 2 minutes, and then dried at 175°C until dry. The dried paper sheet was taken out and cooled to room temperature, and then placed in an oven. The temperature in the oven was raised to 112°C and the insulation time was 19 minutes. After the insulation was completed, the temperature in the oven was raised to 135°C and the insulation time was 30 minutes. The oven door was opened to vent once, and then the temperature in the oven was raised to 161°C and the insulation time was 1.41 hours to obtain a paper sheet.
[0096] The core steel sheet and paper sheet are put into the hot plate vulcanizer at 180℃ and 232kg / cm 3 The wet paper-based friction material was obtained by pressing the sheet under the conditions of (holding time of 5.2 min / mm) and drying at 175° C. for 1.82 h.
[0097] Example 3
[0098] The raw materials for preparing the wet paper-based friction material are as follows, in parts by mass: 24 parts of cotton pulp, 16 parts of carbon fiber, 7 parts of aramid fiber, 12 parts of petroleum coke, 7 parts of zirconium silicate, 6 parts of friction powder, 6 parts of feldspar powder, 5 parts of diatomaceous earth, 4 parts of latex, 3 parts of glass fiber and 25 parts of water.
[0099] The preparation method of the wet paper-based friction material is as follows:
[0100] Punch the inner and outer circles of the core plate steel sheet to remove burrs, position it with the inner hole, perform heat flattening at 670℃, fold it positively and negatively and keep it warm for 2.3h, and then perform heat treatment to a Rockwell hardness of HRC52.3. Grind both sides of the core plate steel sheet, clean it with a degreasing agent on a cleaning machine to remove surface oil stains, and then dry it. Scrub both sides of the core plate steel sheet with acetone, apply glue to the core plate steel sheet on a glue coating machine, and let it dry for use.
[0101] Add water to a beating tank, first add cotton pulp, and beat at a rotation speed of 1970 rpm for 21 minutes, at which the beating degree is 26°SR, then add carbon fiber and aramid fiber, and beat at a rotation speed of 2010 rpm for 28 minutes, at which the beating degree is 27°SR, then add petroleum coke, zirconium silicate, friction powder, feldspar powder and carbon black diatomaceous earth, and beat at a rotation speed of 1980 rpm for 56 minutes, at which the beating degree is 26°SR, finally add latex, and beat at a rotation speed of 1990 rpm for 45 minutes, at which the beating degree is 26°SR, to obtain a mixed slurry;
[0102] The obtained mixed slurry was mixed with glass fiber filaments, and placed in a hand paper machine for papermaking to obtain a prefabricated wet paper sheet with a thickness of 1.19 mm;
[0103] Punching the obtained prefabricated wet paper sheet into inner and outer circles to obtain a prefabricated wet paper disc;
[0104] The obtained prefabricated wet paper discs are placed in a basket, the prefabricated wet paper discs are separated by wire mesh, the basket is sunk into the impregnation device, the cover is tightened, the vacuum pump is turned on, and the vacuum is evacuated at a vacuum degree of 0.07 Pa for 16 minutes, and then the vacuum pump is turned off, and the impregnation liquid is added to perform impregnation until it is soaked, and the basket containing the impregnated prefabricated wet paper discs is taken out and drained for 2.6 hours to obtain the impregnated prefabricated paper discs;
[0105] The obtained pre-impregnated paper sheet was naturally dried for 2 minutes, and then dried at 176°C until dry. The dried paper sheet was taken out and cooled to room temperature, and then placed in an oven. The temperature in the oven was raised to 115°C and the insulation time was 19 minutes. After the insulation was completed, the temperature in the oven was raised to 140°C and the insulation time was 27 minutes. The oven door was opened to vent once, and then the temperature in the oven was raised to 164°C and the insulation time was 1.5 hours to obtain a paper sheet.
[0106] The core steel sheet and paper sheet are put into the hot plate vulcanizer at 181℃ and 238kg / cm 3 The wet paper-based friction material was obtained by pressing the sheet under the conditions of (holding time of 5.8 min / mm) and drying at 176° C. for 1.95 h.
[0107] Example 4
[0108] The raw materials for preparing the wet paper-based friction material are as follows, in parts by mass: 23 parts of cotton pulp, 17 parts of carbon fiber, 7 parts of aramid fiber, 11 parts of petroleum coke, 8 parts of zirconium silicate, 7 parts of friction powder, 5 parts of feldspar powder, 4 parts of diatomaceous earth, 5 parts of latex, 2 parts of glass fiber and 25 parts of water.
[0109] The preparation method of the wet paper-based friction material is as follows:
[0110] Punch the inner and outer circles of the core plate steel sheet to remove burrs, position it with the inner hole, heat-level it at 675℃, fold it positively and negatively and keep it warm for 2.2h, and then heat-treat it to a Rockwell hardness of HRC51.8. Grind both sides of the core plate steel sheet, clean it with a degreasing agent on a cleaning machine to remove surface oil, and then dry it. Scrub both sides of the core plate steel sheet with acetone, apply glue to the core plate steel sheet on a glue coating machine, and let it dry for use.
[0111] Add water to a beating tank, first add cotton pulp, and beat at a rotation speed of 1965 rpm for 23 minutes, at which the beating degree is 28°SR, then add carbon fiber and aramid fiber, and beat at a rotation speed of 1985 rpm for 31 minutes, at which the beating degree is 29°SR, then add petroleum coke, zirconium silicate, friction powder, feldspar powder and carbon black diatomaceous earth, and beat at a rotation speed of 1995 rpm for 58 minutes, at which the beating degree is 27°SR, finally add latex, and beat at a rotation speed of 1980 rpm for 49 minutes, at which the beating degree is 28°SR, to obtain a mixed slurry;
[0112] The obtained mixed slurry was mixed with glass fiber filaments, and placed in a hand paper machine for papermaking to obtain a prefabricated wet paper sheet with a thickness of 1.26 mm;
[0113] Punching the obtained prefabricated wet paper sheet into inner and outer circles to obtain a prefabricated wet paper disc;
[0114] The obtained prefabricated wet paper discs were put into a basket, the prefabricated wet paper discs were separated by wire mesh, the basket was sunk into the impregnation device, the cover was tightened, the vacuum pump was turned on, and the vacuum was evacuated at a vacuum degree of 0.09 Pa for 15 minutes, and then the vacuum pump was turned off, and the impregnation solution was added to perform impregnation until it was soaked, and the basket containing the impregnated prefabricated wet paper discs was taken out and drained for 2.7 hours to obtain the impregnated prefabricated paper discs;
[0115] The obtained pre-impregnated paper sheet was naturally dried for 2 minutes, and then dried at 177°C until dry. The dried paper sheet was taken out and cooled to room temperature, and then placed in an oven. The temperature in the oven was raised to 118°C and the insulation time was 18 minutes. After the insulation was completed, the temperature in the oven was raised to 137°C and the insulation time was 28 minutes. The oven door was opened to vent once, and then the temperature in the oven was raised to 162°C and the insulation time was 1.44 hours to obtain a paper sheet.
[0116] The core steel sheet and paper sheet are put into the hot plate vulcanizer at 185℃ and 234kg / cm 3 The wet paper-based friction material was obtained by pressing the sheet under the conditions of (holding time of 5.6 min / mm) and drying at 180°C for 1.88 h.
[0117] Example 5
[0118] The raw materials for preparing the wet paper-based friction material are as follows, by mass: 22 parts of cotton pulp, 16 parts of carbon fiber, 7 parts of aramid fiber, 10 parts of petroleum coke, 5 parts of zirconium silicate, 7 parts of friction powder, 8 parts of feldspar powder, 3 parts of diatomaceous earth, 4 parts of latex, 2 parts of glass fiber and 26 parts of water.
[0119] The preparation method of the wet paper-based friction material is as follows:
[0120] Punch the inner and outer circles of the core plate steel sheet to remove burrs, position it with the inner hole, perform heat flattening at 678℃, fold it positively and negatively and keep it warm for 2.1h, and then perform heat treatment to a Rockwell hardness of HRC51.5. Grind both sides of the core plate steel sheet, clean it with a degreasing agent on a cleaning machine to remove surface oil stains, and then dry it. Scrub both sides of the core plate steel sheet with acetone, apply glue to the core plate steel sheet on a glue coating machine, and let it dry for use.
[0121] Add water to a beating tank, first add cotton pulp, and beat at a rotation speed of 2000 rpm for 24 minutes, at which time the beating degree is 23°SR, then add carbon fiber and aramid fiber, and beat at a rotation speed of 2010 rpm for 32 minutes, at which time the beating degree is 28°SR, then add petroleum coke, zirconium silicate, friction powder, feldspar powder and carbon black diatomaceous earth, and beat at a rotation speed of 2020 rpm for 62 minutes, at which time the beating degree is 31°SR, finally add latex, and beat at a rotation speed of 2030 rpm for 51 minutes, at which time the beating degree is 30°SR, to obtain a mixed slurry;
[0122] The obtained mixed slurry was mixed with glass fiber filaments, and placed in a hand paper machine for papermaking to obtain a prefabricated wet paper sheet with a thickness of 1.18 mm;
[0123] Punching the obtained prefabricated wet paper sheet into inner and outer circles to obtain a prefabricated wet paper disc;
[0124] The obtained prefabricated wet paper discs are placed in a basket, the prefabricated wet paper discs are separated by wire mesh, the basket is sunk into the impregnation device, the cover is tightened, the vacuum pump is turned on, and the vacuum is evacuated at a vacuum degree of 0.08 Pa for 15 minutes, and then the vacuum pump is turned off, and the impregnation liquid is added to perform impregnation until it is soaked, and the basket containing the impregnated prefabricated wet paper discs is taken out and drained for 2.4 hours to obtain the impregnated prefabricated paper discs;
[0125] The obtained pre-impregnated paper sheet was naturally dried for 2 minutes, and then dried at 179°C until dry. The dried paper sheet was taken out and cooled to room temperature, and then placed in an oven. The temperature in the oven was raised to 114°C and the insulation time was 20 minutes. After the insulation was completed, the temperature in the oven was raised to 136°C and the insulation time was 26 minutes. The oven door was opened to vent once, and then the temperature in the oven was raised to 165°C and the insulation time was 1.45 hours to obtain a paper sheet.
[0126] The core steel sheet and paper sheet are put into the hot plate vulcanizer at 182℃ and 235kg / cm 3 The wet paper-based friction material was obtained by pressing the sheet under the conditions of (holding time of 5.4 min / mm) and drying at 177°C for 1.86 h.
[0127] Example 6
[0128] The raw materials for preparing the wet paper-based friction material are as follows, in parts by mass: 25 parts of cotton pulp, 17 parts of carbon fiber, 6 parts of aramid fiber, 11 parts of petroleum coke, 5 parts of zirconium silicate, 6 parts of friction powder, 7 parts of feldspar powder, 5 parts of diatomaceous earth, 5 parts of latex, 4 parts of glass fiber and 24 parts of water.
[0129] The preparation method of the wet paper-based friction material is as follows:
[0130] Punch the inner and outer circles of the core plate steel sheet to remove burrs, position it with the inner hole, heat-flatten it at 680℃, fold it positively and negatively and keep it warm for 2 hours, and then heat-treat it to a Rockwell hardness of HRC50.3. Grind both sides of the core plate steel sheet, clean it with a degreasing agent on a cleaning machine to remove surface oil stains, and then dry it. Scrub both sides of the core plate steel sheet with acetone, apply glue to the core plate steel sheet on a glue coating machine, and dry it for use.
[0131] Add water to a beating tank, first add cotton pulp, and beat at a rotation speed of 1975 rpm for 22 minutes, at which time the beating degree is 22°SR, then add carbon fiber and aramid fiber, and beat at a rotation speed of 2000 rpm for 30 minutes, at which time the beating degree is 30°SR, then add petroleum coke, zirconium silicate, friction powder, feldspar powder and carbon black diatomaceous earth, and beat at a rotation speed of 2000 rpm for 65 minutes, at which time the beating degree is 30°SR, finally add latex, and beat at a rotation speed of 2010 rpm for 50 minutes, at which time the beating degree is 29°SR, to obtain a mixed slurry;
[0132] The obtained mixed slurry was mixed with glass fiber filaments, and placed in a hand paper machine for papermaking to obtain a prefabricated wet paper sheet with a thickness of 1.20 mm;
[0133] Punching the obtained prefabricated wet paper sheet into inner and outer circles to obtain a prefabricated wet paper disc;
[0134] The obtained prefabricated wet paper discs are placed in a basket, the prefabricated wet paper discs are separated by wire mesh, the basket is sunk into the impregnation device, the cover is tightened, the vacuum pump is turned on, and the vacuum is evacuated at a vacuum degree of 0.09 Pa for 14 minutes, and then the vacuum pump is turned off, and the impregnation liquid is added to perform impregnation until it is soaked, and the basket containing the impregnated prefabricated wet paper discs is taken out and drained for 2.5 hours to obtain the impregnated prefabricated paper discs;
[0135] The obtained pre-impregnated paper sheet was naturally dried for 2 minutes, and then dried at 178°C until dry. The dried paper sheet was taken out and cooled to room temperature, and then placed in an oven. The temperature in the oven was raised to 116°C and the insulation time was 19 minutes. After the insulation was completed, the temperature in the oven was raised to 138°C and the insulation time was 27 minutes. The oven door was opened to vent once, and then the temperature in the oven was raised to 163°C and the insulation time was 1.46 hours to obtain a paper sheet.
[0136] The core steel sheet and paper sheet are put into the hot plate vulcanizer at 183℃ and 236kg / cm 3 The wet paper-based friction material was obtained by pressing the sheet under the conditions of (holding time of 5.5 min / mm) and drying at 178° C. for 1.85 h.
[0137] Table 1 Performance test results of wet paper-based friction materials prepared in Examples 1 to 6
[0138]
[0139]
[0140] As can be seen from Table 1, the wet paper-based friction material provided by the present invention has high dynamic friction coefficient and static friction coefficient, low wear rate, high dynamic pressure resistance and energy load values, and excellent friction performance.
[0141] Comparative Example 1
[0142] The paper-based friction material disclosed in Example 3 of Chinese patent CN102942898A.
[0143] The performance comparison results of the wet paper-based friction materials prepared in Examples 1 to 6 and the paper-based friction material prepared in Comparative Example 1 are shown in Table 2.
[0144] Table 2 Performance comparison results of the wet paper-based friction materials prepared in Examples 1 to 6 and the paper-based friction materials prepared in Comparative Example 1
[0145] Performance Project Examples 1 to 6 Comparative Example 1 Average dynamic friction coefficient 0.132~0.162 0.14 Average static friction coefficient 0.164~0.181 0.15 <![CDATA[Wear rate (cm 3 / J)]]> <![CDATA[<1×10 -9 ]]> <![CDATA[1.0×10 -9 ]]> Dynamic withstand pressure (mpa) ≥3.5 2~3 <![CDATA[Energy load value (J·W / cm 4 )]]> ≥66000 50000~63000
[0146] As can be seen from Table 2, the wet paper-based friction material provided by the present invention has higher static friction coefficient, dynamic pressure resistance and energy load value than the paper-based friction material provided by Comparative Example 1.
[0147] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A wet paper-based friction material, characterized in that: It comprises a core plate steel sheet and a paper sheet attached to one side or both sides of the core plate steel sheet; the raw materials for preparing the paper sheet include paper-based friction material, glass fiber yarn and water; The glass fiber yarn is bent, and a plurality of barbs are arranged on the surface.
2. The wet paper-based friction material according to claim 1, characterized in that: The raw materials for preparing the paper-based friction material include, by weight, 22 to 25 parts of cotton pulp, 16 to 17 parts of carbon fiber, 6 to 8 parts of aramid fiber, 10 to 12 parts of petroleum coke, 5 to 8 parts of zirconium silicate, 5 to 8 parts of friction powder, 5 to 8 parts of feldspar powder, 3 to 5 parts of diatomaceous earth and 3 to 5 parts of latex.
3. The wet paper-based friction material according to claim 1, characterized in that: The mass ratio of water to paper-based friction material is 24.5-25.5:1; The ratio of the total mass of the paper-based friction material and water to the mass of the glass fiber yarn is 20 to 50:
1.
4. The wet paper-based friction material according to claim 2, characterized in that: The friction powder includes aluminum oxide, silicon dioxide and calcium carbonate.
5. The wet paper-based friction material according to any one of claims 1 to 4, characterized in that: The method for preparing the paper sheet comprises the following steps: Mixing the paper-based friction material and water, and beating the mixture to obtain a mixed slurry; The mixed slurry and glass fiber yarn are mixed to make paper to obtain a prefabricated wet paper sheet; Punching the prefabricated wet paper sheet to obtain a prefabricated wet paper disc; The wet paper disc is dipped in glue and then cured for the first time to obtain a paper sheet.
6. The wet paper-based friction material according to claim 5, characterized in that: The beating degree of the beating is 20-35°SR, the rotation speed is 1950-2050rpm, and the time is 150-180min.
7. The wet paper-based friction material according to claim 5, characterized in that: The dipping solution used in the dipping process includes modified resin glue and ethanol; The volume ratio of the modified resin glue to ethanol is 29-30:70-71.
8. The method for preparing a wet paper-based friction material according to any one of claims 1 to 7, characterized in that: The following steps are involved: The paper sheet and the core plate steel sheet are laminated and then cured to obtain a wet paper-based friction material.
9. The preparation method according to claim 8, characterized in that: The temperature of the patch is 180-185°C; The patch method includes a pressurized patch, and the pressure of the pressurized patch is 230-240 kg / cm 3 , the holding time is 5-6min / mm; The temperature of the second curing is 175-180° C., and the time is 1.8-2 hours.
10. Use of the wet paper-based friction material according to any one of claims 1 to 7 or the wet paper-based friction material prepared by the preparation method according to any one of claims 8 to 9 in a wet clutch brake system.
Citation Information
Cited By
Fiber-reinforced wet-type friction material with ultralow friction coefficient and preparation method of fiber-reinforced wet-type friction material
CN121022029A