Graphene-silver composite RFID tag and preparation method and application thereof
Through graphene-silver composite conductive paste and multi-layer ink direct writing technology, the problem of poor stability of RFID tag metal materials is solved, and a high conductivity and environmentally friendly RFID antenna preparation is achieved, which significantly improves production efficiency and service life.
Patent Information
- Application Number
- CN202411067551.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The metal materials of existing RFID tags have poor mechanical, chemical and thermal stability, are prone to damage and generate electronic waste, and lack environmentally friendly and highly conductive alternative materials.
Graphene-silver composite conductive paste is used to expand graphite by microwave heating and ultrasonic treatment in organic solvents. Combined with multi-layer direct ink technology, graphene-silver composite RFID antennas with high conductivity and good adhesion are prepared, using ascorbic acid The solution reduces silver ions to solve storage and reduction problems.
The environmentally friendly and non-toxic graphene-silver composite RFID antenna preparation is achieved, which significantly improves the conductivity, extends the service life, reduces production costs and time, and has a complete antenna structure and few defects.
Smart Images

Figure CN119008114A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of radio frequency identification (RFID) technology, and more specifically, relates to a graphene-silver composite conductive paste and a preparation method and application thereof. Background Art
[0002] The Internet of Things (IoT) connects any object to the Internet through information sensing devices such as radio frequency identification (RFID) and positioning systems, according to agreed protocols, to exchange information and communicate, so as to achieve intelligent identification, positioning, tracking, monitoring and management. It has been widely used in various independent fields such as retail, transportation, and military.
[0003] Radio frequency identification (RFID) technology is a technology that uses radio frequency (RF) waves to transmit information bidirectionally through spatial coupling to achieve intelligent target identification. RFID has been applied to various fields, including health care, logistics, smart shopping, and public safety, due to its strong anti-interference ability, long communication distance, ability to adapt to various complex application environments, improve work efficiency, and reduce management costs. RFID technology can be used to read and write information on RFID tags, thereby achieving the purpose of identifying objects and exchanging data.
[0004] RFID antennas are generally made of metal materials such as copper and aluminum. Metal tags have poor mechanical, chemical and thermal stability, so they are easily damaged in actual applications of the Internet of Things, and also generate electronic waste. Therefore, it is extremely urgent to replace metals with environmentally friendly and highly conductive materials. Summary of the invention
[0005] The purpose of the present invention is to provide a graphene-silver composite conductive paste with good dispersibility and environmental friendliness, and to use the conductive paste to prepare a graphene-silver composite RFID electronic tag with good conductivity, high adhesion and good toughness by using ink direct writing technology.
[0006] The technical solution adopted by the present invention is:
[0007] The present invention provides a method for preparing a graphene-silver composite conductive paste, comprising the following steps:
[0008] (1) heating the expanded graphite with microwaves, washing it with deionized water until the pH value is 6.5-7.5, vacuum drying it, dispersing it in an organic solvent, and performing ultrasonic treatment to obtain a graphene dispersion;
[0009] (2) filtering the graphene dispersion and vacuum drying to obtain graphene solids, and then mixing the graphene solids with an ethanol aqueous solution and a polymer stabilizer, and ultrasonically stirring to obtain a graphene conductive slurry;
[0010] (3) dropping the graphene conductive paste into a silver nitrate solution under stirring, and obtaining the graphene-silver composite conductive paste after ultrasonic treatment.
[0011] Furthermore, in step (1), the power of the microwave heating is 780-820W, and the time is 20-30s; preferably, the power of the microwave heating is 800W, and the time is 30s. The present invention uses mild microwave conditions to expand the expanded graphite for a second time to obtain expanded graphite with fewer layers in advance, and then intercalates and exfoliates in an organic solvent to obtain a graphene solid with distinct layers and better conductive properties.
[0012] Furthermore, in step (1), the vacuum drying condition is 4-6 hours at 100° C. Preferably, the drying time is 5 hours. The use of vacuum drying can prevent the peeled graphene from stacking and reforming into graphite during the drying process.
[0013] Furthermore, in step (1), the organic solvent is at least one of N,N-dimethylformamide, N-methylpyrrolidone, isopropanol or dihydro-levulinic acid ketone. Preferably, the organic solvent is dihydro-levulinic acid ketone, which has the characteristics of being non-toxic and biodegradable.
[0014] Furthermore, in step (1), the ultrasonic time is 6-10 hours, preferably, the ultrasonic time is 8 hours.
[0015] Furthermore, in step (2), the polymer stabilizer is at least one of cellulose acetate butyrate, polyvinyl pyrrolidone or polyvinyl alcohol.
[0016] Furthermore, in step (2), the volume ratio of ethanol to water in the ethanol aqueous solution is 1:(0.5-2); preferably, the volume ratio of ethanol to water in the ethanol aqueous solution is 1.5:1.
[0017] Furthermore, in step (2), the concentration of graphene in the graphene conductive slurry is 20-25 mg / ml.
[0018] Furthermore, in step (3), the amount of silver nitrate added to the graphene-silver composite conductive paste is 5-15% of the mass of the graphene solid.
[0019] The present invention also provides a graphene-silver composite conductive paste prepared by the method.
[0020] The present invention also provides application of the graphene conductive slurry in preparing a graphene RFID antenna.
[0021] The present invention also provides a method for preparing the above-mentioned graphene-based high-conductivity RFID antenna based on the conductive paste direct writing technology, comprising the following steps:
[0022] (1) Printing the above-mentioned graphene-silver composite conductive paste into an antenna circuit by a multi-layer ink direct writing technology;
[0023] (2) soaking the antenna circuit and antenna substrate in an ascorbic acid solution, taking them out and drying them;
[0024] (3) Covering the antenna circuit on the antenna substrate and performing compression processing.
[0025] Since the reduction reaction of glucose and silver ions is very rapid and the conductive slurry is not easy to preserve after reduction, the present invention adopts ascorbic acid solution to reduce silver ions, thereby solving the problem of long-term storage of the conductive slurry and the problem of reducing process control.
[0026] Furthermore, in step (1), the specific preparation method for printing the antenna circuit includes: placing the above-mentioned graphene-silver composite conductive paste into a syringe barrel, connecting the nozzle and installing it on a three-axis CNC platform, turning on the air pressure control system, and then fixing the antenna substrate on a heating plate, using a computer to set the nozzle movement speed and movement route, and at the same time setting the paste extrusion speed and turning on the heating plate. After starting the operation, the graphene-silver composite conductive paste is extruded from the nozzle through a spiral extrusion or pneumatic pressure control system and formed on the substrate. This technology can print a continuous antenna circuit with uniform thickness and good adhesion to the substrate in multiple layers on the substrate, accurately control the printing of complex circuit shapes, and has a short working time and high efficiency, greatly improving the circuit conductivity.
[0027] The usual manufacturing process of RFID antennas includes chemical etching and printed circuit boards, which are cumbersome and not environmentally friendly. Direct writing technology, as a rapidly developing forming technology in recent years, can accurately control the complex printing of antenna lines, with short working time, high efficiency and significant advantages. However, the direct writing parameters (pressure, speed) and direct writing environment (temperature, direct writing medium) of ink direct writing will have a great impact on the direct writing process. The ink needs to be matched with appropriate direct writing parameters and direct writing environment to build a stable structure.
[0028] Preferably, in the heating plate, the heating temperature is 60-80°C, the workbench moving speed is 5-8; the slurry extrusion speed is 10-100 μL / min; the inkjet needle is any one of No. 19, No. 20, No. 21, and No. 22; and the number of layers in multi-layer printing is 5-6.
[0029] Furthermore, in step (2), the concentration of the ascorbic acid solution is 40-60 mg / mL, preferably 50 mg / mL, the soaking time is 3-5 min, and the soaking temperature is room temperature.
[0030] Furthermore, in step (2), the antenna substrate is selected from any one of PET, PVC, PP, PC, cardboard, offset paper, coated paper, glass cardboard, laser paper, kraft paper, fluorescent paper, aluminum foil or anti-counterfeiting paper.
[0031] Furthermore, in step (3), the compression treatment condition is 5-30 MPa for 1-10 min. Preferably, the multi-layer printed antenna circuit and the substrate are covered with the same substrate and placed together on a manual press for compression.
[0032] The present invention also provides a graphene-based high-conductivity RFID antenna prepared by the above method.
[0033] The present invention also provides the use of the above-mentioned graphene RFID antenna in the preparation of RFID electronic tags.
[0034] The beneficial effects of the present invention are:
[0035] The present invention uses ascorbic acid solution to reduce silver ions in the antenna circuit to generate silver. Compared with other reduction methods, such as light reduction, the reduction method is environmentally friendly and simple to operate, and the reduction time is greatly shortened. The preparation and use process of the graphene-silver composite conductive slurry are both green and environmentally friendly, without toxic substance emissions, and harmless to the environment and human health. At the same time, the prepared graphene structure is complete and has few defects. Adding silver to graphene significantly improves the conductivity of the RFID antenna circuit, reduces the number of printing layers, and improves production efficiency.
[0036] The present invention also provides an RFID antenna prepared by using a graphene-silver composite conductive paste. The preparation method of the antenna is based on the multi-layer ink direct writing printing technology of the graphene-silver composite conductive paste, which can accurately control the complex printing of the antenna circuit, and has a short working time and high efficiency. The silver ion mixing operation and reduction method provided are environmentally friendly and simple to operate. The silver nanoparticles are evenly distributed in the graphene matrix to achieve electrical communication. The conductivity of the graphene / silver composite RFID antenna can reach 800S / mm. Among them, the multi-layer printing technology and compression treatment allow the antenna circuit to have high adhesion while improving the conductivity, not easy to fall off, good toughness, not easy to break, not easy to be physically worn and chemically oxidized, and increase the service life. It is stable and reduces the influence of environmental factors such as bending and wrinkling on its resistance value. Considering the tightness of the connection between the graphene sheets caused by multi-layer printing, the circuit is compressed by a manual press. The compression treatment not only improves the conductivity but also effectively improves the adhesion between the circuit and the substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 Actual picture of RFID antenna printed by multi-layer direct writing of graphene-silver composite conductive paste.
[0038] Figure 2 SEM image of the surface of RFID antenna printed by multi-layer direct writing of graphene-silver composite conductive paste and the corresponding EDS energy spectrum scan.
[0039] Figure 3 Raman spectra of graphene antenna and graphene / silver composite antenna.
[0040] Figure 4 Step profiler test results of 5-layer direct-write compression of graphene / silver composite antenna. DETAILED DESCRIPTION
[0041] The present invention is described in detail below in conjunction with specific embodiments. The embodiments are only preferred embodiments of the present invention and are not intended to limit the present invention.
[0042] 1. Preparation of graphene-silver composite conductive paste
[0043] Example 1
[0044] (1) Expandable graphite was placed in a ceramic crucible and then heated in an 800 W commercial microwave oven for 30 s to obtain expanded graphite with fewer layers. The expanded graphite flakes were stirred and washed in deionized water until the pH was close to 7, and then vacuum dried at 100 ° C for 5 h. The dried expanded graphite was deposited in dihydro-L-glucose ketone (10 mg / mL), and the mixture was ultrasonically treated in an ultrasonic bath. After ultrasonication for 8 h, a uniformly dispersed graphene dispersion was obtained.
[0045] (2) Filter the graphene dispersion to obtain graphene sheets. Add the graphene sheets to an ethanol / water mixed solution, add 1wt.% CAB, ultrasonicate, stir, and obtain a uniformly dispersed graphene conductive slurry. Ethanol and water are mixed in a volume ratio of 1:1.5, and dispersed with the graphene sheets to obtain a uniform graphene conductive slurry with a concentration of 30 mg / ml, 25 mg / ml, 20 mg / ml, and 15 mg / ml.
[0046] (3) Dissolve silver nitrate in deionized water, add the silver nitrate solution dropwise while stirring the graphene dispersion, and prepare mixed solutions with silver nitrate added in amounts of 1%, 5%, 10%, and 15% of the graphene solid mass, respectively, and then ultrasonicate the solution to obtain a uniformly dispersed graphene-silver composite conductive slurry.
[0047] Comparative Example 1
[0048] (1) Expandable graphite was placed in a ceramic crucible and then heated in an 800 W commercial microwave oven for 30 s to obtain expanded graphite with fewer layers. The expanded graphite flakes were stirred and washed in deionized water until the pH was close to 7, and then vacuum dried at 100 ° C for 5 h. The dried expanded graphite was deposited in dihydro-L-glucose ketone (10 mg / mL), and the mixture was ultrasonically treated in an ultrasonic bath. After ultrasonication for 8 h, a uniformly dispersed graphene dispersion was obtained.
[0049] (2) Filter the graphene dispersion to obtain graphene sheets. Add the graphene sheets to an ethanol / water mixed solution, add 1wt.% CAB, ultrasonicate, stir, and obtain a uniformly dispersed graphene conductive slurry. Ethanol and water are mixed in a volume ratio of 1:1.5, and dispersed with the graphene sheets to obtain a uniform graphene conductive slurry with a concentration of 15 mg / ml.
[0050] (3) silver ammonia solution was added dropwise while stirring the graphene conductive slurry to prepare a mixed solution in which the amount of silver added was 3.175% of the solid mass of graphene, and then the solution was ultrasonicated to obtain a uniformly dispersed graphene-silver ammonia composite conductive slurry.
[0051] (4) Adding a mixed solution of NaOH and ethylene glycol to the graphene-silver ammonia composite conductive slurry, adjusting the pH value to 10-12, sealing and microwave heating, magnetic stirring and cooling to room temperature, and then dropping glucose solution therein for reduction to obtain a graphene-silver composite conductive slurry.
[0052] 2. Preparation of graphene RFID antenna
[0053] Example 2
[0054] Weigh 4 ml of the 15 mg / ml graphene conductive paste obtained in step (2) of the above embodiment 1, prepare a graphene-silver composite conductive paste with an addition amount of silver nitrate of 5% of the solid mass of graphene according to the above step (3), put it into the syringe barrel, connect it with the nozzle and install it on the three-axis CNC platform, turn on the air pressure control system, then fix the PET substrate on the heating plate, set the nozzle movement speed to 7 by computer, set the nozzle movement route, set the slurry extrusion speed to 15 microliters per minute, turn on the heating plate, set the heating plate temperature to 70°C, start the operation after the heating plate temperature rises and stabilizes at 70°C, and the graphene conductive paste is extruded from the nozzle through the spiral extrusion or pneumatic pressure control system and formed on the substrate. Repeat the printing 1 to 6 times to obtain the antenna line.
[0055] The antenna substrate and circuit were immersed in ascorbic acid solution (50 mg / mL) for 5 minutes. After being taken out, they were dried. Then the formed antenna circuit covered substrate was placed in a manual press, and the pressure was set to 25 MPa. After maintaining the pressure for 3 minutes, the conductive silver glue was evenly applied on both ends of the antenna circuit. After the conductive silver glue was cured, the conductivity was tested as shown in Table 1 below.
[0056] Table 1 Effect of repeated printing times of graphene-silver conductive paste on conductivity in Example 1
[0057] Direct write layers 1 2 3 4 5 6 Conductivity / (S / mm) 0.26 3.62 8.57 24.38 68.41 68.57 Thickness / (μm) 0.4 0.5 0.8 1.2 1.5 1.7 Square resistance / (Ω / sq.) 9615 552 146 34.2 9.7 8.6
[0058] From the results in Table 1, it can be seen that compared with 5-layer direct writing, 6-layer direct writing has little effect on improving conductivity. More layers of direct writing have similar effects and the time cost is too high, which reduces efficiency. Therefore, the optimal number of layers for multi-layer printing is 5-6 layers.
[0059] Example 3
[0060] Weigh 4 ml of the 20 mg / ml graphene conductive paste obtained in step (2) of the above embodiment 1, prepare a graphene-silver composite conductive paste with an addition amount of silver nitrate of 5% of the solid mass of graphene according to the above step (3), put it into the syringe barrel, connect it with the nozzle and install it on the three-axis CNC platform, turn on the air pressure control system, then fix the PP substrate on the heating plate, set the nozzle movement speed to 7 by computer, set the nozzle movement route, set the slurry extrusion speed to 15 microliters per minute, turn on the heating plate, set the heating plate temperature to 70°C, start the operation after the heating plate temperature rises and stabilizes at 70°C, and the graphene conductive paste is extruded from the nozzle through the spiral extrusion or pneumatic pressure control system and formed on the substrate. Repeat the printing 5 times to obtain the antenna line.
[0061] The antenna substrate and circuit were immersed in ascorbic acid solution (50 mg / mL) for 5 minutes. After being taken out, they were dried. Then the formed antenna circuit covered substrate was placed in a manual press, and the pressure was set to 25 MPa. After maintaining the pressure for 3 minutes, the conductive silver glue was evenly applied on both ends of the antenna circuit. After the conductive silver glue was cured, the conductivity was tested as shown in Table 2 below.
[0062] Example 4
[0063] Weigh 4 ml of the 25 mg / ml graphene conductive paste obtained in step (2) of the above embodiment 1, prepare a graphene-silver composite conductive paste with an addition amount of silver nitrate of 5% of the solid mass of graphene according to the above step (3), put it into the syringe barrel, connect it with the nozzle and install it on the three-axis CNC platform, turn on the air pressure control system, then fix the PP substrate on the heating plate, set the nozzle movement speed to 7 by computer, set the nozzle movement route, set the slurry extrusion speed to 15 microliters per minute, turn on the heating plate, set the heating plate temperature to 70°C, start the operation after the heating plate temperature rises and stabilizes at 70°C, and the graphene conductive paste is extruded from the nozzle through the spiral extrusion or pneumatic pressure control system and formed on the substrate. Repeat the printing 5 times to obtain the antenna line.
[0064] The antenna substrate and circuit were immersed in ascorbic acid solution (50 mg / mL) for 5 minutes. After being taken out, they were dried. Then the formed antenna circuit covered substrate was placed in a manual press, and the pressure was set to 25 MPa. After maintaining the pressure for 3 minutes, the conductive silver glue was evenly applied on both ends of the antenna circuit. After the conductive silver glue was cured, the conductivity was tested as shown in Table 2 below.
[0065] Example 5
[0066] Weigh 4 ml of the 25 mg / ml graphene conductive paste obtained in step (2) of the above embodiment 1, prepare a graphene-silver composite conductive paste with an addition amount of silver nitrate of 10% of the solid mass of graphene according to the above step (3), put it into the syringe barrel, connect it with the nozzle and install it on the three-axis CNC platform, turn on the air pressure control system, then fix the coated paper on the heating plate, set the nozzle movement speed to 7 by computer, set the nozzle movement route, set the slurry extrusion speed to 15 microliters per minute, turn on the heating plate, set the heating plate temperature to 70°C, start the operation after the heating plate temperature rises and stabilizes at 70°C, and the graphene conductive paste is extruded from the nozzle through the spiral extrusion or pneumatic pressure control system and formed on the substrate. Repeat the printing 5 times to obtain the antenna line.
[0067] The antenna substrate and circuit were immersed in ascorbic acid solution (50 mg / mL) for 5 minutes. After being taken out, they were dried. Then the formed antenna circuit covered substrate was placed in a manual press, and the pressure was set to 25 MPa. After maintaining the pressure for 3 minutes, the conductive silver glue was evenly applied on both ends of the antenna circuit. After the conductive silver glue was cured, the conductivity was tested as shown in Table 2 below.
[0068] Comparative Example 2
[0069] Weigh 4 ml of the 30 mg / ml graphene conductive paste obtained in step (2) of the above embodiment 1, prepare a graphene-silver composite conductive paste with an addition amount of silver nitrate of 5% of the solid mass of graphene according to the above step (3), put it into the syringe barrel, connect it with the nozzle and install it on the three-axis CNC platform, turn on the air pressure control system, then fix the PP substrate on the heating plate, set the nozzle movement speed to 7 by computer, set the nozzle movement route, set the slurry extrusion speed to 15 microliters per minute, turn on the heating plate, set the heating plate temperature to 70°C, start the operation after the heating plate temperature rises and stabilizes at 70°C, and the graphene conductive paste is extruded from the nozzle through the spiral extrusion or pneumatic pressure control system and formed on the substrate. Repeat the printing 5 times to obtain the antenna circuit.
[0070] The antenna substrate and circuit were immersed in ascorbic acid solution (50 mg / mL) for 5 minutes. After being taken out, they were dried. Then the formed antenna circuit covered substrate was placed in a manual press, and the pressure was set to 25 MPa. After maintaining the pressure for 3 minutes, the conductive silver glue was evenly applied on both ends of the antenna circuit. After the conductive silver glue was cured, the conductivity was tested as shown in Table 2 below.
[0071] Comparative Example 3
[0072] Weigh 4 ml of the 25 mg / ml graphene conductive paste obtained in step (2) of the above embodiment 1, prepare a graphene-silver composite conductive paste with an addition amount of silver nitrate of 15% of the solid mass of graphene according to the above step (3), put it into the syringe barrel, connect it with the nozzle and install it on the three-axis CNC platform, turn on the air pressure control system, then fix the coated paper on the heating plate, set the nozzle movement speed to 7 by computer, set the nozzle movement route, set the slurry extrusion speed to 15 microliters per minute, turn on the heating plate, set the heating plate temperature to 70°C, start the operation after the heating plate temperature rises and stabilizes at 70°C, and the graphene conductive paste is extruded from the nozzle through the spiral extrusion or pneumatic pressure control system and formed on the substrate. Repeat the printing 5 times to obtain the antenna line.
[0073] The antenna substrate and circuit were immersed in ascorbic acid solution (50 mg / mL) for 5 minutes. After being taken out, they were dried. Then the formed antenna circuit covered substrate was placed in a manual press, and the pressure was set to 25 MPa. After maintaining the pressure for 3 minutes, the conductive silver glue was evenly applied on both ends of the antenna circuit. After the conductive silver glue was cured, the conductivity was tested as shown in Table 2 below.
[0074] Comparative Example 4
[0075] Weigh 4 ml of the 25 mg / ml graphene conductive paste obtained in step (2) of the above embodiment 1, prepare a graphene-silver composite conductive paste with an addition amount of silver nitrate of 10% of the solid mass of graphene according to the above step (3), put it into the syringe barrel, connect it with the nozzle and install it on the three-axis CNC platform, turn on the air pressure control system, then fix the coated paper on the heating plate, set the nozzle movement speed to 7 by computer, set the nozzle movement route, set the slurry extrusion speed to 15 microliters per minute, turn on the heating plate, set the heating plate temperature to 70°C, start the operation after the heating plate temperature rises and stabilizes at 70°C, and the graphene conductive paste is extruded from the nozzle through the spiral extrusion or pneumatic pressure control system and formed on the substrate. Repeat the printing 5 times to obtain the antenna line.
[0076] Soak the antenna substrate and circuit in ascorbic acid solution (50 mg / mL) for 5 minutes. Take it out and dry it. Then evenly apply conductive silver glue on both ends of the antenna circuit. After the conductive silver glue is cured, the test conductivity is shown in Table 2 below.
[0077] Comparative Example 5
[0078] Weigh 4 ml of the 25 mg / ml graphene conductive paste obtained in step (2) of the above embodiment 1, prepare a graphene-silver composite conductive paste with an addition amount of silver nitrate of 1% of the solid mass of graphene according to the above step (3), put it into the syringe barrel, connect it with the nozzle and install it on the three-axis CNC platform, turn on the air pressure control system, then fix the coated paper on the heating plate, set the nozzle movement speed to 7 by computer, set the nozzle movement route, set the slurry extrusion speed to 15 microliters per minute, turn on the heating plate, set the heating plate temperature to 70°C, start the operation after the heating plate temperature rises and stabilizes at 70°C, and the graphene conductive paste is extruded from the nozzle through the spiral extrusion or pneumatic pressure control system and formed on the substrate. Repeat the printing 5 times to obtain the antenna line.
[0079] The antenna substrate and circuit were immersed in ascorbic acid solution (50 mg / mL) for 5 minutes. After being taken out, they were dried. Then the formed antenna circuit covered substrate was placed in a manual press, and the pressure was set to 25 MPa. After maintaining the pressure for 3 minutes, the conductive silver glue was evenly applied on both ends of the antenna circuit. After the conductive silver glue was cured, the conductivity was tested as shown in Table 2 below.
[0080] Comparative Example 6
[0081] Take the graphene-silver composite conductive paste of the above comparative example 1, put it into the syringe barrel, connect it with the nozzle and install it on the three-axis CNC platform, turn on the air pressure control system, then fix the coated paper on the heating plate, set the nozzle movement speed to 7 by computer, set the nozzle movement route, set the slurry extrusion speed to 15 microliters per minute, turn on the heating plate, set the heating plate temperature to 70°C, and start running after the heating plate temperature rises and stabilizes at 70°C. The graphene conductive paste is extruded from the nozzle through a spiral extrusion or pneumatic pressure control system and formed on the substrate. Repeat the printing 5 times to obtain the antenna line.
[0082] Place the formed antenna line covering substrate into a manual press, set the pressure to 25 MPa, maintain the pressure for 3 minutes, and then evenly apply conductive silver glue on both ends of the antenna line. After the conductive silver glue is cured, test the conductivity as shown in Table 2.
[0083] Table 2 Test results of conductive properties of direct-written 5-layer antennas of Examples 2-5 and Comparative Examples 2-6
[0084]
[0085] From the results in Table 2, it can be seen that in Comparative Example 2, due to the high graphene concentration (30 mg / ml), the graphene polymerizes with the silver ions, and the silver ions are not evenly dispersed, resulting in low conductivity. The mass percentage of silver nitrate to graphene in the range of 5-10% can significantly improve the conductivity of the antenna. The mass percentage of silver nitrate to graphene in Comparative Example 5 is lower than 5%, and the conductivity improvement effect is not good. After the mass percentage of silver nitrate to graphene in Comparative Example 3 is higher than 10%, due to the high concentration of silver ions, the graphene polymerizes, and the silver ions are not evenly dispersed, resulting in low conductivity. According to the comparison between Comparative Example 4 and Example 5, the conductivity of the antenna can be significantly improved after compression treatment. Comparative Example 6 uses glucose solution to be directly added to the graphene-silver ammonia composite conductive slurry. Due to the excessively fast reduction rate, the size of the silver nanoparticles is uneven and the distribution on the graphene surface is uneven, resulting in low conductivity.
[0086] The antenna circuit obtained in Example 5 was continuously bent in half to test its conductivity and adhesion. The test results are shown in Tables 3 and 4 below.
[0087] Table 3 Test results of conductivity and adhesion of the antenna after bending and folding it 100 times at different angles
[0088] Bending angle / ° 30 60 90 120 150 180 Conductivity / (S / mm) 783.26 744.98 678.37 659.29 638.24 595.45 Adhesion / N 3.8 3.7 3.5 3.3 3.3 2.9
[0089] Table 4 Test results of conductivity and adhesion of the antenna after 90° bending for different times
[0090]
[0091]
[0092] It can be seen from the results in Tables 3 and 4 that the prepared antenna circuit has high adhesion, is not easy to fall off, has good toughness, is not easy to break, has a longer service life, has good stability, and reduces the influence of environmental factors such as bending and wrinkling on its resistance value.
[0093] In summary, the graphene-silver composite conductive paste and the multi-layer ink direct writing printing technology based on the graphene-silver composite conductive paste provided by the present invention are environmentally friendly and can significantly help improve the conductivity of RFID tag antennas, and can effectively improve production efficiency, reduce costs and save time in large-scale production.
[0094] It can be understood that the above specific embodiments are all further explanations of the present invention and are not intended to limit the scope of protection of the present invention. For those skilled in the art, all other modifications and changes obtained without creative work are within the scope of protection of the present invention.
Claims
1. A method for preparing a graphene-silver composite conductive paste, It is characterized in that The following steps are involved: (1) heating the expanded graphite with microwaves, washing it with deionized water until the pH value is 6.5-7.5, vacuum drying it, dispersing it in an organic solvent, and performing ultrasonic treatment to obtain a graphene dispersion; (2) filtering the graphene dispersion and vacuum drying to obtain graphene solids, and then mixing the graphene solids with an ethanol aqueous solution and a polymer stabilizer, and ultrasonically stirring to obtain a graphene conductive slurry; (3) dropping the graphene conductive paste into a silver nitrate solution under stirring, and obtaining the graphene-silver composite conductive paste after ultrasonic treatment.
2. The preparation method according to claim 1, It is characterized in that The power of the microwave heating in step (1) is 780-820 W, and the time is 20-30 s; the organic solvent is at least one of N,N-dimethylformamide, N-methylpyrrolidone, isopropanol or dihydro-levulinic acid ketone.
3. The preparation method according to claim 1, It is characterized in that The polymer stabilizer in step (2) is at least one of cellulose acetate butyrate, polyvinyl pyrrolidone or polyvinyl alcohol; the volume ratio of ethanol to water in the ethanol aqueous solution is 1: (0.5-2); and the concentration of graphene in the graphene conductive slurry is 20-25 mg / ml.
4. The preparation method according to claim 1, It is characterized in that The amount of silver nitrate added to the graphene-silver composite conductive paste in step (3) is 5-15% of the mass of the graphene solid.
5. A graphene-silver composite conductive paste prepared by the method according to any one of claims 1 to 4.
6. Use of the graphene conductive paste according to claim 5 in preparing a graphene RFID antenna.
7. A method for preparing a graphene-based highly conductive RFID antenna based on conductive paste direct writing technology. It is characterized in that The following steps are involved: (1) Printing the graphene-silver composite conductive paste described in claim 5 into an antenna circuit by a multi-layer ink direct writing technique; (2) soaking the antenna circuit and antenna substrate in an ascorbic acid solution, taking them out and drying them; (3) Covering the antenna circuit on the antenna substrate and performing compression processing.
8. The method for preparing an RFID antenna according to claim 7, It is characterized in that The concentration of the ascorbic acid solution in step (2) is 40-60 mg / mL, and the soaking time is 3-5 min.
9. A graphene-based highly conductive RFID antenna prepared by the method according to any one of claims 7-8.
10. Use of the graphene RFID antenna according to claim 9 in preparing an RFID electronic tag.
Citation Information
Patent Citations
Ink-jet printing type graphene doped nano-silver conductive ink and preparation method thereof
CN112608642A
Silver nanoparticle / multilayer graphene composite material and preparation method thereof
CN114477152A
Graphene-silver composite RFID tag and preparation method and application thereof
CN114639504A