Method for reducing warping of silicon carbide ultrathin wafer
By making a reactive film and a silicon nitride film with reverse stress on the front process film layer of the silicon carbide wafer, the problem of warping during the thinning process of the ultra-thin wafer is solved, and stress adjustment is achieved and reduce warpage, while improving the stability and waterproof gas performance of the wafer.
Patent Information
- Application Number
- CN202410972233.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art is difficult to effectively reduce the warpage caused by the silicon carbide ultra-thin wafer in the back thinning process, and conventional methods increase costs or cannot adjust the initial warpage.
The first reactive film layer is made on the surface of the front process film layer of the silicon carbide wafer. The first reactive film layer is opposite to the stress direction generated by the front process film layer. It is used to buffer and adjust the warping stress and on its surface A second reactive force film layer is then prepared, and the stress directions of the two are the same to offset the stress caused by the front process film layer and thinning.
Effectively reduce the warping of ultra-thin silicon carbide wafers, reduce stress during processing, reduce wafer thickness, and isolate water vapor through the silicon nitride film layer to protect the wafer.
Smart Images

Figure CN119008378A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of wafer processing, and in particular to a method for reducing warping of an ultra-thin silicon carbide wafer. Background Art
[0002] For SIC power devices, the thinner the SIC wafer is, the lower the threshold voltage VF is, and the higher the surge parameters are. Ultra-thin wafers with the same threshold voltage and surge parameters can make more single dies, reducing the cost of a single die. However, SIC ultra-thin wafers, i.e. wafers with a thickness of less than 150um, gradually increase their warpage as the thickness becomes thinner during the thinning process. The large warpage causes abnormal wafer transfer during the back-side processes including thinning and cleaning, back-side ohms, laser annealing, decarbonization, and back-side metallization, and even the situation where the wafer is picked up and placed and hits the robotic arm. Therefore, it is necessary to reduce the warpage of ultra-thin wafers in a timely manner.
[0003] In the conventional SIC ultra-thin wafer backside process, the first method to reduce wafer warpage is to use bonding and debonding processes, but this method will increase the backside process cost. The second method is to add a stress-reducing film layer on the backside of the wafer, but many ultra-thin wafers are not compatible with the ultra-thin wafer film forming process after thinning, or the fragmentation rate is high, resulting in increased costs.
[0004] Some methods of thinning silicon carbide wafers are to deposit a protective layer on the front of the wafer after the front process is completed, and after the back process thinning step, a sacrificial oxide layer is grown on the back of the wafer by thermal oxidation, and then the front protective layer and the back sacrificial oxide layer are stripped off simultaneously by wet etching or etching, in this way, the internal stress of the wafer caused by grinding is released. However, this method can only solve the wafer warpage caused by the device thinning process, and the stress release is limited. There is no way to adjust the wafer warpage caused by the silicon carbide wafer before entering the back process.
[0005] Therefore, a method is needed to timely offset the stress generated during back thinning and reduce warping without affecting the front-end process. Summary of the invention
[0006] In order to overcome the problems existing in the related art, the purpose of the present invention is to provide a method for reducing the warping of silicon carbide ultra-thin wafers. This method can timely offset the stress generated during back thinning and reduce the warping without affecting the front-end process.
[0007] A method for reducing warpage of an ultra-thin silicon carbide wafer, comprising:
[0008] Performing front process processing on the front side of the silicon carbide substrate of the silicon carbide wafer to form a front process film layer;
[0009] A first reaction force film layer is manufactured on the surface of the front process film layer; the stress direction generated by the first reaction force film layer is opposite to that of the front process film layer.
[0010] The method for reducing the warpage of silicon carbide ultra-thin wafers provided by the present invention includes performing front process processing on the front side of the silicon carbide substrate of the silicon carbide wafer to form a front process film layer. After the front process is completed, a first reaction force film layer is made on the surface of the front process film layer. The first reaction force film layer can provide reverse stress to the wafer warpage while also playing a role of buffering and transition. The first reaction force film layer itself can adjust the warpage stress. The present invention makes the first reaction force film layer on the surface of the front process film layer, which can better reduce the stress generated during the processing, thereby reducing warpage and further reducing the thickness of the silicon carbide wafer.
[0011] In a preferred technical solution of the present invention, a second reactive force film layer is manufactured on the surface of the first reactive force film layer; the stress direction generated by the second reactive force film layer is the same as that of the first reactive force film layer.
[0012] The first reaction force film layer can buffer the second reaction force film layer. The first reaction force film layer and the second reaction force film layer work together to offset the stress generated by the front process film layer and thinning, reduce the warping of the silicon carbide wafer, and further reduce the thickness of the silicon carbide wafer. Using the second reaction force film layer to isolate water vapor can better protect the silicon carbide wafer.
[0013] In a preferred technical solution of the present invention, the first reactive film layer is a silicon dioxide film layer.
[0014] In a preferred technical solution of the present invention, the raw materials of the first reactive force film layer include silane, nitrogen and nitrous oxide; the sputtering parameters of the first reactive force film layer include: sputtering power of 50-300W, deposition temperature of 150-400°C, pressure of 500-2000mTorr, stress of 200-600Mpa, and thickness of 400nm-2000nm.
[0015] The stress adjustment of the first reaction force film layer is mainly achieved through comprehensive adjustment of sputtering power, gas flow, pressure, raw material gas ratio and temperature, and the process parameters are adjusted according to the needs of the processing production line.
[0016] In a preferred technical solution of the present invention, the second reactive force film layer is a silicon nitride film layer.
[0017] The silicon nitride film layer can work together with the silicon dioxide film layer to adjust the warpage stress, and the silicon nitride film layer can also isolate water vapor.
[0018] In a preferred technical solution of the present invention, the raw materials of the second reactive force film layer include silane, nitrogen and ammonia, and the sputtering parameters of the second reactive force film layer include: sputtering power of 50-300W, deposition temperature of 150-400°C, pressure of 500-2000mTorr, stress of 200-600Mpa, and thickness of 400nm-2000nm.
[0019] The stress of the second reaction force film layer is comprehensively adjusted by sputtering power, gas flow, pressure, raw material gas ratio and temperature. The raw materials of the second reaction force film layer 4 are 5% silane / nitrogen, pure nitrogen and ammonia. 5% silane / nitrogen means that silane is diluted with nitrogen, and the volume ratio of silane is 5%. Pure silane is an explosive gas, so nitrogen needs to be mixed with silane.
[0020] In a preferred technical solution of the present invention, the front side process of the silicon carbide substrate of the silicon carbide wafer is performed to form a front side process film layer, including:
[0021] depositing a metal electrode on the front side of the silicon carbide substrate;
[0022] removing metal from areas outside the metal electrode;
[0023] An electrode lead is connected to the metal electrode.
[0024] Metal electrodes are deposited on the front of the silicon carbide substrate of the silicon carbide wafer, and the areas where metal is not needed are removed by photolithography, so that only the electrode area on the surface of the silicon carbide substrate has metal, and other areas have no metal. After the silicon carbide wafer is processed, it is packaged and the electrode leads are connected to the metal electrodes.
[0025] In a preferred technical solution of the present invention, after the second reactive film layer is formed on the surface of the first reactive film layer, the method further includes:
[0026] If the silicon carbide wafer is used for a diode, the first reactive force film layer and the second reactive force film layer corresponding to the front electrode are removed.
[0027] If the silicon carbide wafer is used for a diode, the front electrode is exposed, that is, the front electrode is not covered with the first reactive film layer and the second reactive film layer, and other areas are covered with the first reactive film layer and the second reactive film layer.
[0028] In a preferred technical solution of the present invention, after the second reactive film layer is formed on the surface of the first reactive film layer, the method further includes:
[0029] If the silicon carbide wafer is used for a MOS tube, the first reactive force film layer and the second reactive force film layer corresponding to the gate, the source and the Kelvin electrode are removed.
[0030] If the silicon carbide wafer is used for a MOS tube, the gate, source and Kelvin electrode are exposed, that is, the gate, source and Kelvin electrode are not covered by the first reaction force film layer and the second reaction force film layer, and other areas are covered by the first reaction force film layer and the second reaction force film layer.
[0031] The beneficial effects of the present invention are:
[0032] The method for reducing the warpage of silicon carbide ultra-thin wafers provided by the present invention comprises performing a front process on the front side of the silicon carbide substrate of the silicon carbide wafer to form a front process film layer. After the front process is completed, a first reaction force film layer is formed on the surface of the front process film layer. The stress direction generated by the first reaction force film layer is opposite to that of the front process film layer, and the first reaction force film layer can play a role of buffering and transition. The first reaction force film layer itself can adjust the warpage stress. The present invention manufactures the first reaction force film layer on the surface of the front process film layer, which can better reduce the stress generated during the processing, thereby reducing warpage and further reducing the thickness of the silicon carbide wafer. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 is a schematic diagram of a semiconductor structure provided by the present invention;
[0034] Figure 2 It is a schematic diagram of an existing semiconductor structure;
[0035] Figure 3 is a schematic diagram of a semiconductor structure provided with an exposure area provided by the present invention;
[0036] Figure 4 is a schematic diagram of the diode exposure area provided by the present invention;
[0037] Figure 5 It is a schematic diagram of the exposed area of the MOS tube provided by the present invention;
[0038] Figure 6 It is a schematic diagram of the process of processing the improved silicon carbide power device provided by the present invention;
[0039] Figure 7 It is a schematic diagram of the existing process of processing silicon carbide power devices.
[0040] Figure numerals: 1. Silicon carbide substrate; 2. Front process film layer; 3. First reaction force film layer; 4. Second reaction force film layer; 5. Front electrode exposure area; 6. Front electrode lead; 7. Gate exposure area; 8. Gate lead; 9. Kelvin exposure area; 10. Kelvin lead; 11. Source exposure area; 12. Source lead. DETAILED DESCRIPTION
[0041] The preferred embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. Although the preferred embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art.
[0042] Example 1
[0043] like Figure 1 and Figure 6 As shown, this embodiment provides a method for reducing the warpage of a silicon carbide ultra-thin wafer, comprising:
[0044] S1: performing front process processing on the front side of the silicon carbide substrate of the silicon carbide wafer to form a front process film layer.
[0045] S2: forming a first reaction force film layer on the surface of the front process film layer; the stress direction generated by the first reaction force film layer is opposite to that of the front process film layer.
[0046] like Figure 2 and Figure 7 As shown, conventional silicon carbide power devices are processed on the front side of the wafer and on the back side of the wafer. In this embodiment, after the front side process of the silicon carbide wafer substrate is completed, the first reaction force film layer is added, which does not affect any front-end process and does not require the addition of other equipment for subsequent processing, and has little impact on the unthinned silicon carbide wafer.
[0047] At the same time, as the silicon carbide wafer is thinned, the reaction force can be released in time to offset the stress generated during the thinning of the back side and reduce warping.
[0048] The front process film layer 2 is processed to form a first reaction force film layer 3. The processing method is sputtering, and the raw material of the first reaction force film layer 3 is silicon dioxide. The first reaction force film layer 3 can generate stress, and the direction of the stress is opposite to the direction of the stress generated by the front process film layer 2 and thinning, thereby offsetting the stress generated by the front process film layer 2 and thinning.
[0049] Sputtering is divided into DC sputtering, AC sputtering, reactive sputtering and magnetron sputtering. The principle of sputtering is to bombard the target material with charged particles. When the accelerated ions bombard the solid surface, surface atoms collide and energy and momentum are transferred, causing the target atoms to escape from the surface and deposit on the front process film layer 2. Charged particles such as gas positive ions are used to bombard the target surface of a certain raw material, causing atoms or molecules on the surface of the target to escape. Since the sputtering process involves momentum conversion, the sputtered particles are directional. Using the sputtering processing method, metal, alloy or dielectric films can be obtained on the surface of the substrate, which is suitable for the manufacture of thin film integrated circuits, chip lead devices and semiconductor devices. One of the main means of controlling film cracks and surface shape is to regulate the SiO 2 The stress of the film is determined by changing the SiO 2 The evaporation process of the thin film is used to change the stress matching and thus control the film cracking.
[0050] The method for reducing the warpage of the silicon carbide ultra-thin wafer in this embodiment includes performing a front process on the front side of the silicon carbide substrate 1 of the silicon carbide wafer to form a front process film layer 2. After the front process is completed, a first reaction force film layer 3 is formed on the surface of the front process film layer 2. The stress direction generated by the first reaction force film layer 3 is opposite to that of the front process film layer 2. The first reaction force film layer 3 can play a role of buffering and transition. The first reaction force film layer 3 itself can adjust the warpage stress. The present invention manufactures the first reaction force film layer 3 on the surface of the front process film layer 2, which can better reduce the stress generated during the processing, thereby reducing warpage and further reducing the thickness of the silicon carbide wafer.
[0051] Example 2
[0052] like Figure 1 and Figure 6 As shown, this embodiment provides a method for reducing warpage of an ultra-thin silicon carbide wafer, comprising:
[0053] S1: performing front process processing on the front side of the silicon carbide substrate of the silicon carbide wafer to form a front process film layer.
[0054] S2: forming a first reaction force film layer on the surface of the front process film layer; the stress direction generated by the first reaction force film layer is opposite to that of the front process film layer.
[0055] A second reactive force film layer 4 is manufactured on the surface of the first reactive force film layer 3 ; the stress direction generated by the second reactive force film layer 4 is the same as that of the first reactive force film layer 3 .
[0056] The first reactive film layer 3 is a silicon dioxide film layer.
[0057] The raw materials of the first reactive film layer 3 include silane, nitrogen and nitrous oxide; the sputtering parameters of the first reactive film layer 3 include: sputtering power of 50-300W, deposition temperature of 150-400°C, pressure of 500-2000mTorr, stress of 200-600Mpa, and thickness of 400nm-2000nm.
[0058] As an example, the raw materials of the first reactive film layer 3 include silane doped with nitrogen, pure nitrogen and nitrous oxide. In the mixed gas composed of silane and nitrogen, the volume ratio of silane is 5%, and the volume ratio of nitrogen is 95%. The volume flow rate of the mixed gas composed of silane and nitrogen is 350sccm, the volume flow rate of pure nitrogen is 400sccm, and the volume flow rate of nitrous oxide is 900sccm. The deposition temperature is 300°C, the sputtering power is 100W, and the pressure is 800mTorr.
[0059] Optionally, the raw materials of the first reaction force film layer 3 include silane doped with nitrogen, pure nitrogen and nitrous oxide. In the mixed gas composed of silane and nitrogen, the volume ratio of silane is 5%, and the volume ratio of nitrogen is 95%. The volume flow rate of the mixed gas composed of silane and nitrogen is 300sccm, the volume flow rate of pure nitrogen is 380sccm, and the volume flow rate of nitrous oxide is 850sccm. The deposition temperature is 350°C, the sputtering power is 200W, and the pressure is 1000mTorr. The front side of the silicon carbide substrate 1 of the silicon carbide wafer is subjected to front process processing to form a front process film layer 2, and then a first reaction force film layer 3 is sputtered on the front process film layer 2 of the silicon carbide wafer. The first reaction force film layer 3 here serves as a transition layer, which mainly plays a buffering role for the second reaction force film layer 4.
[0060] The stress regulation of the first reaction force film layer 3 is mainly adjusted by the sputtering power, gas flow, pressure, raw material gas ratio and temperature. For example, the raw material of the first reaction force film layer 3 contains a mixed gas of silane and nitrogen, wherein the volume ratio of silane is 5%, and the volume ratio of nitrogen is 95%. Pure silane is an explosive gas, so nitrogen is used to dilute silane. As an example, at 300°C, a mixed gas containing 5% silane and 95% nitrogen is used with 350sccm, 400sccm nitrogen and 1000sccm nitrous oxide, a sputtering power of 100W, a pressure of 800mTorr, and 16min can deposit a SiO2 layer with a thickness of 1200nm. 2 , SiO 2 The stress of the first reaction film layer 3 is tensile stress, which can offset the compressive stress caused by the front process film layer 2 and thinning.
[0061] If the front process film layer 2 is in tensile stress after thinning, the stress of the first reaction force film layer 3 is compressive stress, and the process conditions as described above are adopted. This indicates that the stress of the first reaction force film layer 3 will be adjusted according to the thickness of the silicon carbide ultra-thin wafer after thinning and the conditions of the front and back processes, thereby achieving the purpose of reducing the warpage of the silicon carbide ultra-thin wafer, and the final stress will be adjusted according to the final thickness after thinning and the conditions of the front and back processes.
[0062] The stress adjustment of the first reaction force film layer 3 is mainly carried out through comprehensive adjustment of sputtering power, gas flow, pressure, raw material gas ratio and temperature, and the process parameters are adjusted according to the needs of the processing production line.
[0063] The present embodiment describes that the first reaction force film layer 3 is made on the surface of the front process film layer 2, including sputtering the first reaction force film layer 3 on the surface of the front process film layer 2, and the first reaction force film layer 3 is used to buffer the second reaction force film layer 4. The sputtering parameters of the first reaction force film layer 3 include: sputtering power of 50-300W, deposition temperature of 150-400℃, pressure of 500-2000mTorr, stress of 200-600Mpa, thickness of 400nm-2000nm, and the raw materials of the first reaction force film layer 3 include silane, nitrogen and nitrous oxide. If the front process film layer 2 generates compressive stress, the first reaction force film layer 3 generates tensile stress; if the front process film layer 2 generates tensile stress, the first reaction force film layer 3 generates compressive stress. The stress generated by the first reaction force film layer 3 is opposite to the stress generated by the front process film layer 2, thereby offsetting the stress generated by the front process film layer 2 and reducing the warping of the silicon carbide wafer. The sputtering parameters of the first reactive force film layer 3 are adjusted according to the needs of the processing production line to control the sputtering process of the first reactive force film layer 3 .
[0064] Example 3
[0065] like Figure 1 and Figure 6 As shown, this embodiment provides a method for reducing warpage of an ultra-thin silicon carbide wafer, comprising:
[0066] S1: performing front process processing on the front side of the silicon carbide substrate of the silicon carbide wafer to form a front process film layer.
[0067] S2: forming a first reaction force film layer on the surface of the front process film layer; the stress direction generated by the first reaction force film layer is opposite to that of the front process film layer.
[0068] A second reactive force film layer 4 is manufactured on the surface of the first reactive force film layer 3 ; the stress direction generated by the second reactive force film layer 4 is the same as that of the first reactive force film layer 3 .
[0069] The second reactive film layer 4 is a silicon nitride film layer.
[0070] A second reactive film layer 4 is fabricated on the surface of the first reactive film layer 3. The second reactive film layer 4 is fabricated by sputtering, and the raw material of the second reactive film layer 4 is silicon nitride. The second reactive film layer 4 can generate stress, and the direction of the stress is opposite to the direction of the stress generated by the front process film layer 2 and thinning, thereby offsetting the stress generated by the front process film layer 2 and thinning. The second reactive film layer 4 can also isolate external water vapor, thereby ensuring the quality of the silicon carbide wafer.
[0071] The raw material of the second reactive film layer 4 includes silicon nitride Si 3 N 4 The stress of the second reaction force film layer 4 is comprehensively adjusted by sputtering power, gas flow, pressure, raw material gas ratio and temperature. For example, the raw material of the second reaction force film layer 4 is a mixed gas containing 5% silane and 95% nitrogen, pure nitrogen and ammonia. In the mixed gas composed of silane and nitrogen, silane is diluted with nitrogen, and the volume ratio of silane is 5%. Pure silane is an explosive gas, so nitrogen needs to be mixed with silane. The sputtering power of the second reaction force film layer 4 is 50-300W, the deposition temperature is 150-400℃, the pressure is 500-2000mTorr, the stress is 200-600Mpa, and the thickness is 400nm-2000nm.
[0072] As an example, the raw materials of the second reaction force film layer are a mixed gas containing 5% silane and 95% nitrogen, pure nitrogen and ammonia, wherein the volume flow rate of the mixed gas composed of silane and nitrogen is 280sccm, the volume flow rate of pure nitrogen is 450sccm, the volume flow rate of ammonia is 10sccm, the sputtering power is 100W, the deposition temperature is 280°C, and the pressure is 850mTorr.
[0073] Optionally, the raw materials of the second reactive film layer are a mixed gas containing 5% silane and 95% nitrogen, pure nitrogen and ammonia, wherein the volume flow rate of the mixed gas composed of silane and nitrogen is 300sccm, the volume flow rate of pure nitrogen is 480sccm, the volume flow rate of ammonia is 11sccm, the sputtering power is 110W, the deposition temperature is 300°C, and the pressure is 1000mTorr.
[0074] As an example, the volume flow rate of the mixed gas containing silane and nitrogen is 300sccm, the volume flow rate of pure nitrogen is 500sccm, the volume flow rate of ammonia is 11sccm, the sputtering power is 100W, the deposition temperature is 300℃, the pressure is 800mTorr, and a Si layer with a thickness of 1000nm can be deposited in 25min. 3 N 4 .Si 3 N 4It is tensile stress, and the stress magnitude is 88.5MPa. Here, the stress of the second reaction force film layer 4 is tensile stress, which can offset the compressive stress generated by the front process film layer and thinning. If it is tensile stress after thinning, the stress of the second reaction force film layer 4 is compressive stress. The stress magnitude of the second reaction force film layer 4 can be adjusted according to the thickness of the silicon carbide ultra-thin wafer after thinning and the conditions of the front and back processes, so as to achieve the purpose of reducing the warpage of the silicon carbide ultra-thin wafer.
[0075] The second reaction force film layer 4 can further adjust the stress, and has excellent water-proof and gas-proof performance. If the first reaction force film layer 3 itself can adjust the warping stress, the thickness of the second reaction force film layer 4 only needs to be 100±50nm to isolate water vapor. If the second reaction force film layer 4 needs to further adjust the stress, the thickness corresponding to the actual stress shall prevail, and the final thickness of the second reaction force film layer 4 needs to be 100±50nm. By adding the second reaction force film layer 4, not only can the stress be adjusted secondary, but by adjusting the thickness of the second reaction force film layer 4, it can have better adhesion and water-proof and gas-proof performance at the same time, so that water vapor can be isolated while reducing the warping of the silicon carbide ultra-thin wafer, protecting the device with the silicon carbide ultra-thin wafer.
[0076] The second reaction force film layer 4 is made on the surface of the first reaction force film layer 3 as described in this embodiment, including sputtering the second reaction force film layer 4 on the surface of the first reaction force film layer 3, and the second reaction force film layer 4 is used to adjust the warping stress and isolate water vapor. The second reaction force film layer 4 can be combined with the first reaction force film layer 3 to further adjust the stress. The second reaction force film layer 4 can also isolate water vapor to protect devices with silicon carbide ultra-thin wafers. If the front process film layer 2 generates compressive stress, the second reaction force film layer 4 generates tensile stress; if the front process film layer 2 generates tensile stress, the second reaction force film layer 4 generates compressive stress. The stress generated by the second reaction force film layer 4 is opposite to the stress generated by the front process film layer 2, thereby offsetting the stress generated by the front process film layer 2 and reducing the warping of the silicon carbide wafer. The sputtering parameters of the second reaction force film layer 4 are adjusted according to the needs of the processing production line to control the sputtering process of the second reaction force film layer 4.
[0077] Example 4
[0078] like Figure 1 and Figure 6 As shown, this embodiment provides a method for reducing warpage of an ultra-thin silicon carbide wafer, comprising:
[0079] S1: performing front process processing on the front side of the silicon carbide substrate of the silicon carbide wafer to form a front process film layer.
[0080] S2: forming a first reaction force film layer on the surface of the front process film layer; the stress direction generated by the first reaction force film layer is opposite to that of the front process film layer.
[0081] The step of manufacturing the first reactive force film layer 3 on the surface of the front process film layer 2 comprises:
[0082] A first reactive force film layer 3 is sputtered on the surface of the front process film layer 2 , and the first reactive force film layer 3 is used for buffering the second reactive force film layer 4 .
[0083] The sputtering parameters of the first reactive force film layer 3 include: sputtering power of 50-300 W, deposition temperature of 150-400° C., pressure of 500-2000 mTorr, stress of 200-600 Mpa, and thickness of 400 nm-2000 nm.
[0084] The raw materials of the first reactive film layer 3 include silane, nitrogen and nitrous oxide.
[0085] The method of manufacturing the second reactive film layer 4 on the surface of the first reactive film layer 3 includes:
[0086] A second reactive force film layer 4 is sputtered on the surface of the first reactive force film layer 3 , and the second reactive force film layer 4 is used to adjust the warping stress and isolate water vapor.
[0087] The above method is used to prepare SiO 2 The first reaction force film layer 3, and the main raw material is Si 3 N 4 The second reaction force film layer 4 does not need to be removed in the subsequent back process, and the first reaction force film layer 3 and the second reaction force film layer 4 remain on the device surface. The two reaction force film layers act on the front of the silicon carbide wafer, and form a pair of balanced forces with the stress generated during the processing of the silicon carbide wafer, thereby fully reducing the warping. For ultra-thin wafers with a thickness of less than 150um, the warping is controlled within 2mm. If the warping is ≥4mm, the back process cannot be carried out. The degree of warping is particularly important for the back processing technology of silicon carbide ultra-thin wafers, which can ensure that the silicon carbide ultra-thin wafers complete the full process of device manufacturing.
[0088] The stress directions generated by the first reaction force film layer 3 and the second reaction force film layer 4 are the same, and the stress directions generated by the first reaction force film layer 3 and the front process film layer 2 are opposite. For example, if the front process film layer 2 generates compressive stress, the first reaction force film layer 3 and the second reaction force film layer 4 generate tensile stress. The combination of the first reaction force film layer 3 and the second reaction force film layer 4 can better offset the stress generated by the front process film layer 2 and thinning, thereby reducing the warpage of the silicon carbide ultra-thin wafer.
[0089] A first reaction force film layer 3 whose main component is silicon dioxide is sputtered on the surface of the front process film layer 2, and a second reaction force film layer 4 whose main component is silicon nitride is sputtered on the surface of the first reaction force film layer 3. The stress generated by the first reaction force film layer 3 and the second reaction force film layer 4 is opposite to the stress generated by the front process film layer 2, which can better offset the stress generated by the front process film layer 2 and thinning, thereby reducing the warpage of the silicon carbide ultra-thin wafer.
[0090] The front side process is performed on the front side of the silicon carbide substrate of the silicon carbide wafer to form a front side process film layer, including:
[0091] S11: depositing a metal electrode on the front side of the silicon carbide substrate.
[0092] S12: removing metal from areas other than the metal electrode.
[0093] S13: Connecting electrode leads to the metal electrodes.
[0094] A metal electrode is deposited on the front of the silicon carbide substrate 1 of the silicon carbide wafer, and the area where no metal is needed is removed by photolithography, so that only the electrode area on the surface of the silicon carbide substrate 1 has metal, and other areas have no metal. After the silicon carbide wafer is processed, it is packaged and the electrode lead is connected to the metal electrode.
[0095] After the second reactive force film layer is formed on the surface of the first reactive force film layer, the method further comprises:
[0096] S41: If the silicon carbide wafer is used for a diode, the first reactive force film layer and the second reactive force film layer corresponding to the front electrode are removed.
[0097] S42: If the silicon carbide wafer is used for a MOS tube, the first reaction force film layer and the second reaction force film layer corresponding to the gate, the source and the Kelvin electrode are removed.
[0098] Step S41 and step S42 are in parallel relationship. Figure 3-Figure 5 As shown, the silicon carbide wafer is photolithographically and etched. If the silicon carbide wafer is used for a diode, the front electrode is exposed, that is, the front electrode is not covered with the first reactive film layer 3 and the second reactive film layer 4, and the other areas are covered with the first reactive film layer 3 and the second reactive film layer 4. If the silicon carbide wafer is used for a MOS tube, the gate, source and Kelvin electrode are exposed, that is, the gate, source and Kelvin electrode are not covered with the first reactive film layer 3 and the second reactive film layer 4, and the other areas are covered with the first reactive film layer 3 and the second reactive film layer 4.
[0099] In this embodiment, the front side of the silicon carbide substrate 1 of the silicon carbide wafer is subjected to front processing to form a front process film layer 2, including depositing a metal electrode on the front side of the silicon carbide substrate 1, removing metal in the area outside the metal electrode, and connecting an electrode lead to the metal electrode. According to the device corresponding to the silicon carbide wafer, a portion of the first reaction force film layer 3 and the second reaction force film layer 4 are removed to expose the corresponding area. If the silicon carbide wafer is used for a diode, the first reaction force film layer 3 and the second reaction force film layer 4 corresponding to the front electrode are removed. If the silicon carbide wafer is used for a MOS tube, the first reaction force film layer 3 and the second reaction force film layer 4 corresponding to the gate, source and Kelvin electrode are removed.
[0100] Example 5
[0101] The present embodiment provides a semiconductor structure, which is obtained by processing the method for reducing the warpage of silicon carbide ultra-thin wafers described in any one of Embodiments 1 to 5, and the semiconductor structure includes a silicon carbide substrate 1, and a front process film layer 2 is arranged on the front side of the silicon carbide substrate 1; a first reaction force film layer 3 is arranged on the side of the front process film layer 2 away from the silicon carbide substrate 1, and a second reaction force film layer 4 is arranged on the side of the first reaction force film layer 3 away from the front process film layer 2.
[0102] The first reactive film layer 3 is made of silicon dioxide, and the second reactive film layer 4 is made of silicon nitride.
[0103] The semiconductor structure further includes an exposure area, which penetrates the first reactive film layer 3 and the second reactive film layer 4; the exposure area corresponds to the front electrode, or the exposure area corresponds to the gate, source and Kelvin electrode.
[0104] like Figure 4-Figure 5 As shown, the front electrode exposure area 5, or the gate exposure area 7, the source exposure area 11 and the Kelvin exposure area 9 of the semiconductor structure are photolithographically processed and etched. The front electrode exposure area 5 is provided with a front electrode lead 6, the gate exposure area 7 is provided with a gate lead 8, the source exposure area 11 is provided with a source lead 12, and the Kelvin exposure area 9 is provided with a Kelvin lead 10. If it is a diode, only the front electrode needs to be exposed. If it is a MOS, the gate, source and Kelvin electrode need to be exposed. Other areas are covered by the reactive film layer. The exposure area corresponds to the packaging wire bonding area, that is, it corresponds to the position of the hole punched on the front of the semiconductor structure in the last step of the aforementioned silicon carbide front process. The number of leads is not limited here, only the schematic diagram of the exposure area is shown, and the size of the exposure area is determined by the packaging conditions corresponding to the product specifications. The etching gas is CF4, CHF 3 , SF 6 Combination of Si-based etching gas and Ar gas.
[0105] Unless otherwise specifically stated, the relative arrangement, numerical expressions and numerical values of the parts and steps set forth in these embodiments do not limit the scope of the application. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a restriction. Therefore, other examples of exemplary embodiments can have different values. It should be noted that similar reference numerals and letters represent similar items in the following drawings, and therefore, once a certain item is defined in an accompanying drawing, it does not need to be further discussed in the subsequent accompanying drawings.
[0106] It should be understood that spatially relative terms are intended to encompass different orientations of the device in use or operation in addition to the orientation depicted in the figures. For example, if the device in the figures is inverted, a device described as "above" or "above" other devices or structures would then be positioned "below" or "below" the other devices or structures. Thus, the exemplary term "above" can include both the orientations of "above" and "below." The device may also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatially relative descriptions used herein should be interpreted accordingly.
[0107] In addition, it should be noted that the use of terms such as "first" and "second" to limit components is only for the convenience of distinguishing the corresponding components. Unless otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of this application.
[0108] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for reducing warpage of an ultra-thin silicon carbide wafer, characterized in that: include: Performing front process processing on the front side of the silicon carbide substrate of the silicon carbide wafer to form a front process film layer; Making a first reaction force film layer on the surface of the front process film layer; The first reaction force film layer and the front process film layer generate stress in opposite directions.
2. The method for reducing warpage of an ultra-thin silicon carbide wafer according to claim 1, characterized in that: A second reactive force film layer is formed on the surface of the first reactive force film layer; the stress direction generated by the second reactive force film layer is the same as that of the first reactive force film layer.
3. The method for reducing warpage of an ultra-thin silicon carbide wafer according to claim 1, characterized in that: The first reactive film layer is a silicon dioxide film layer.
4. The method for reducing warpage of an ultra-thin silicon carbide wafer according to claim 3, characterized in that: The raw materials of the first reactive force film layer include silane, nitrogen and nitrous oxide; the sputtering parameters of the first reactive force film layer include: sputtering power of 50-300W, deposition temperature of 150-400°C, pressure of 500-2000mTorr, stress of 200-600Mpa, and thickness of 400nm-2000nm.
5. The method for reducing warpage of an ultra-thin silicon carbide wafer according to claim 2, characterized in that: The second reactive force film layer is a silicon nitride film layer.
6. The method for reducing warpage of an ultra-thin silicon carbide wafer according to claim 5, characterized in that: The raw materials of the second reactive film layer include silane, nitrogen and ammonia. The sputtering parameters of the second reactive film layer include: sputtering power of 50-300W, deposition temperature of 150-400°C, pressure of 500-2000mTorr, stress of 200-600Mpa, and thickness of 400nm-2000nm.
7. The method for reducing warpage of an ultra-thin silicon carbide wafer according to claim 1, characterized in that: The front side process is performed on the front side of the silicon carbide substrate of the silicon carbide wafer to form a front side process film layer, including: depositing a metal electrode on the front side of the silicon carbide substrate; removing metal from areas outside the metal electrode; An electrode lead is connected to the metal electrode.
8. The method for reducing warpage of an ultra-thin silicon carbide wafer according to claim 1, characterized in that: After the second reactive force film layer is formed on the surface of the first reactive force film layer, the method further comprises: If the silicon carbide wafer is used for a diode, the first reactive force film layer and the second reactive force film layer corresponding to the front electrode are removed.
9. The method for reducing warpage of an ultra-thin silicon carbide wafer according to claim 1, characterized in that: After the second reactive force film layer is formed on the surface of the first reactive force film layer, the method further comprises: If the silicon carbide wafer is used for a MOS tube, the first reactive force film layer and the second reactive force film layer corresponding to the gate, the source and the Kelvin electrode are removed.
Citation Information
Cited By
Manufacturing method of thin film solar cell with low warping degree
CN121419379A