Preparation method of air environment-friendly polymer-based solid-state lithium battery electrolyte

By using composite technology of materials such as active polymers, skeleton support polymers and lithium salts in lithium batteries, the problem of difficult preparation of lithium battery electrolytes in air environments and low conductivity at room temperature is solved, and high-efficiency lithium battery electrolytes are achieved Preparation and stability performance.

CN119009105APending Publication Date: 2024-11-22LUDONG UNIVERSITY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411383810.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Liquid electrolytes in traditional lithium batteries are prone to leakage, posing safety hazards, and polymer-based solid electrolytes are difficult to prepare in air environments and have low ionic conductivity at room temperature.

Method used

Using composite materials such as active polymers, skeleton support polymers and lithium salts, air-environmentally friendly polymer-based solid lithium battery electrolytes are prepared by stirring and casting, increasing the content of amorphous reagents to improve room temperature ionic conductivity and mechanical strength. .

Benefits of technology

It has achieved simplified preparation process in an air environment, improved room temperature ionic conductivity and mechanical properties, and inhibited the growth of lithium dendrites, which is suitable for large-scale production and application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009105A_ABST
    Figure CN119009105A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a polymer-based solid electrolyte which can be processed in an air environment and can be applied to a solid-state lithium battery. The polymer electrolyte designed by the invention is prepared by compounding an ion transport active polymer, a skeleton support polymer, a lithium salt and an amorphization reagent. The preparation method comprises the following steps: firstly, respectively preparing active polymer-based electrolyte slurry and skeleton-supported polymer-based electrolyte slurry, then adding lithium salt into the active polymer-based electrolyte slurry to increase the content of Li < + > in the polymer solid electrolyte, and then adding an amorphizing reagent through compounding to reduce the crystallinity of the polymer solid electrolyte. And then mixing and uniformly stirring the two polymer slurries, and preparing a membrane by a tape casting method, so that the room-temperature conductivity of the membrane can be effectively improved. The polymer-based solid electrolyte prepared by the invention has the advantages of better ionic conductivity, good tensile mechanical property and the like, and the preparation mode in an air environment can greatly simplify the process and shorten the preparation period.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of solid-state lithium batteries, and more specifically, to a method for preparing an air-friendly polymer-based solid-state lithium battery electrolyte. Background Art

[0002] Lithium metal batteries have extremely high theoretical energy density (>500 Wh / kg), extremely low electrochemical reaction potential (-3.04V) and small mass density (0.534 g / cm³). However, the liquid electrolyte used in traditional lithium batteries has leakage problems, which can easily cause explosions and pose great safety risks. Solid electrolytes are expected to become the most promising electrolytes for automotive power lithium batteries and lithium-ion batteries due to their high mechanical strength, excellent thermal stability and chemical stability. Therefore, inventing a solid electrolyte suitable for large-scale production has become a new direction for the power application of lithium batteries and lithium-ion batteries.

[0003] Currently, solid electrolytes for lithium batteries are divided into inorganic ceramic electrolytes (ICE) and organic polymer electrolytes (SPE). ICE has the disadvantages of large interfacial resistance and great brittleness, while SPE has excellent flexibility. Therefore, based on the advantages of SPE, our research group invented a polymer-based solid-state lithium battery electrolyte that still has high ionic conductivity at room temperature.

[0004] The working temperature of SPE is generally 50-70℃, and it has the disadvantage of low ionic conductivity at room temperature. In order to improve its intrinsic and room temperature ionic conductivity, people have developed many methods, one of the most suitable methods is to add fillers. Compared with ICE, there is no Li+ in SPE, so some lithium salts must be added to it to provide lithium ions to improve its ionic conductivity. However, salts containing Li+ are usually not stably stored in the air, and they will decompose due to continuous contact with water and oxygen in the air environment. Therefore, we invented an electrolyte system that inhibits the contact of lithium salts with water and oxygen and allows lithium salts to exist stably, realizing the preparation of polymer-based solid electrolytes with high performance at room temperature in an air environment, which is of great significance to further promote the development of solid-state lithium batteries. Summary of the invention

[0005] The present invention provides a method for preparing an air-friendly polymer-based solid-state lithium battery electrolyte, in order to overcome the problem that polymer-based solid-state electrolytes are difficult to prepare in an air environment and have low ionic conductivity at room temperature. The solid-state electrolyte of the invention can effectively inhibit the growth of lithium dendrites and significantly improve the room-temperature ionic conductivity. The preparation process of the polymer-based solid-state electrolyte applied in the present invention is simple, which is conducive to large-scale production.

[0006] To achieve the above purpose, the present invention adopts the following technical solutions:

[0007] An air-friendly polymer-based solid-state lithium battery electrolyte is composited with an active polymer, a skeleton-supported polymer, a lithium salt, and an amorphizing agent. The mass ratio of the active polymer to the skeleton-supported polymer is (0.0-2.0):(0.0-2.0). The mass ratio of the lithium salt to the active polymer is 1:3, and the mass fraction of the amorphizing agent in the active polymer electrolyte system is (20.0-30.0) wt.%.

[0008] On the one hand, the present invention application can provide a method for preparing the above-mentioned polymer-based solid-state lithium battery electrolyte, comprising the following steps:

[0009] S1. Preparation of ion transport active polymer-based electrolyte slurry: Add active polymer, lithium salt and amorphization agent into a polar aprotic solvent and fully dissolve them by stirring.

[0010] S2. Preparation of skeleton-supported polymer-based electrolyte slurry: adding skeleton-supported polymer into polar aprotic solvent and fully dissolving it by stirring.

[0011] S3. Mixing of air-friendly polymer-based solid-state lithium battery electrolyte slurry: Pour the slurry obtained in step S2 into the beaker of step S1, rinse the beaker in step S2 with an appropriate amount of backbone polymer polar aprotic solvent in batches, and pour it into the beaker of step S1, and mix them evenly by stirring.

[0012] S4. Preparation of air-friendly polymer-based solid-state lithium battery electrolyte: The slurry obtained in step S3 is cast in a specific mold in an appropriate amount using a casting method, and then heated and dried at 40-80°C for 4-6 hours to obtain a film-type product of a certain thickness of the air-friendly polymer-based solid-state lithium battery electrolyte.

[0013] On the other hand, the purpose of this patent application is to construct a solid-state lithium battery, which is made of a positive electrode, the above-mentioned air-friendly polymer-based solid-state lithium battery electrolyte and a negative electrode, and the polymer-based solid-state lithium battery electrolyte membrane is located between the positive electrode and the negative electrode.

[0014] Preferably, the positive electrode sheet includes a positive electrode current collector, a positive electrode active material, a conductive agent and a binder.

[0015] Preferably, the positive electrode active material is at least one of lithium iron phosphate and lithium nickel cobalt manganese oxide ternary positive electrode materials.

[0016] Preferably, the negative electrode plate is a lithium metal plate.

[0017] Compared with the prior art, the beneficial effects of the present invention are:

[0018] (1) In the present invention, the preparation process of the polymer-based electrolyte is carried out in an air environment, and the preparation time is greatly shortened. The preparation process is simplified and the efficiency is improved;

[0019] (2) In the present invention, the mechanical strength of the polymer-based solid electrolyte is greatly improved by introducing a skeleton-supported polymer;

[0020] (3) In the present invention, the content of the amorphizing agent can reach 30 wt.%. The high content of the amorphizing agent greatly reduces the crystallinity of the polymer solid electrolyte and improves the ionic conductivity at room temperature;

[0021] (4) The present invention provides a simple and convenient experimental method for preparing polymer solid electrolytes by syringe casting. The electrolyte prepared by this method has high room temperature ionic conductivity and good flexibility;

[0022] (5) The all-solid-state lithium battery prepared in the present invention has good mechanical properties and interface stability, can effectively suppress lithium dendrites, and has good charge and discharge performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a physical picture of the solid electrolyte membrane prepared in Example 2-2 of the present invention;

[0024] Figure 2 This is an electron microscope picture of the solid electrolyte membrane prepared in Example 2-2 of the present invention;

[0025] Figure 3 XRD patterns of the solid electrolyte membranes prepared in Comparative Example 1 and Example 2-2 of the present invention;

[0026] Figure 4 The stress-strain curves of the solid electrolyte membranes prepared in some embodiments of the present invention;

[0027] Figure 5 The linear sweep voltammetry test curves of button half-cells assembled with solid electrolyte membranes in Comparative Example 1 and Example 2-2 of the present invention;

[0028] Figure 6 The cycle performance of the lithium iron phosphate solid-state lithium battery assembled with the electrolyte membrane in Example 2-2 of the present invention at room temperature. DETAILED DESCRIPTION

[0029] The embodiments of the present invention will be described in detail below with reference to examples. The examples are only used to explain the present invention and are not used to limit the scope of the present invention.

[0030] Comparative Example 1:

[0031] This comparative example provides a method for preparing an air-friendly polymer-based solid-state lithium battery electrolyte: weigh 0.8 g of polyethylene oxide and add it to a beaker containing 20 mL of acetonitrile, stirring continuously during the addition. Weigh bistrifluoromethanesulfonyl lithium in a ratio of 1:3 by mass of lithium salt to active polymer, add it to the above slurry, and stir continuously during the addition until the slurry becomes transparent. Pour it into a mold with a diameter of 20.0 mm and a depth of 3.2 mm, and then dry it at 40-80°C for 3-6 h to obtain an air-friendly polymer-based solid-state lithium battery electrolyte. The visual state of the electrolyte membrane prepared under different experimental conditions in Comparative Example 1 is shown in Table 1.

[0032] Table 1

[0033] Time (h) Temperature (℃) 3 4 5 6 40 The slurry still exists The slurry still exists The slurry still exists The slurry still exists 60 The slurry still exists Film forming and easy to remove Film forming and easy to remove Film forming and easy to remove 80 Molten Molten Molten Molten

[0034] Comparative Example 2:

[0035] This comparative example provides a method for preparing an air-friendly polymer-based solid-state lithium battery electrolyte: weigh 0.8 g of polyethylene oxide and add it to a beaker containing 20 mL of acetonitrile, stirring continuously during the addition. Weigh lithium dioxalate borate at a ratio of 1:3 of lithium salt to active polymer mass ratio, add the above slurry, and stir continuously during the addition until the slurry becomes transparent. Pour it into a mold with a diameter of 20.0 mm and a depth of 3.2 mm, and then dry it at 60°C for 4-6 h to obtain an air-friendly polymer-based solid-state lithium battery electrolyte.

[0036] Comparative Example 3:

[0037] This comparative example provides a method for preparing an air-friendly polymer-based solid-state lithium battery electrolyte: weigh 0.8 g of polyethylene oxide and add it to a beaker containing 20 mL of acetonitrile, stirring continuously during the addition. Weigh lithium trifluoromethanesulfonate at a ratio of 1:3 of lithium salt to active polymer mass ratio, add it to the above slurry, and stir continuously during the addition until the slurry becomes transparent. Pour it into a mold with a diameter of 20.0 mm and a depth of 3.2 mm, and then dry it at 60°C for 4-6 h to obtain an air-friendly polymer-based solid-state lithium battery electrolyte.

[0038] Comparative Example 4:

[0039] This comparative example provides a method for preparing an air-friendly polymer-based solid-state lithium battery electrolyte: weigh 0.8 g of polypropylene oxide, add 20 mL of acetonitrile into a beaker, and continue stirring until the slurry becomes transparent. Pour it into a mold with a diameter of 20 mm and a depth of 3.2 mm, and then dry it at 60°C for 4-6 h to obtain an air-friendly polymer-based solid-state lithium battery electrolyte.

[0040] The electrolyte membranes obtained in Comparative Examples 2, 3 and 4 could not be formed into films and could not be removed from the mold.

[0041] Comparative Example 5:

[0042] This comparative example provides a method for preparing an air-friendly polymer-based solid-state lithium battery electrolyte: weigh 0.8 g of polyvinylidene fluoride-hexafluoropropylene, add 20 mL of N-methylpyrrolidone into a beaker, and continue stirring until the slurry becomes transparent. Pour it into a mold with a diameter of 20 mm and a depth of 3.2 mm, and then dry it at 40-80 ° C for 3-6 h to obtain an air-friendly polymer-based solid-state lithium battery electrolyte. The visual state results of the solid electrolyte membrane prepared in Comparative Example 5 are shown in Table 2.

[0043] Table 2

[0044] Time (h) Temperature (℃) 3 4 5 6 40 The slurry still exists The slurry still exists The slurry still exists The slurry still exists 60 The slurry still exists The slurry still exists The slurry still exists The slurry still exists 80 The slurry still exists Film forming and easy to remove Film forming and easy to remove Film forming and easy to remove

[0045] Comparative Example 6:

[0046] This comparative example provides a method for preparing an air-friendly polymer-based solid-state lithium battery electrolyte: weigh 0.8 g of polyvinyl alcohol, add 20 mL of N-methylpyrrolidone into a beaker, and continue stirring until the slurry becomes transparent. Pour it into a mold with a diameter of 20 mm and a depth of 3.2 mm, and then dry it at 80 ° C for 4-6 h to obtain an air-friendly polymer-based solid-state lithium battery electrolyte.

[0047] The solid electrolyte membranes obtained in Comparative Examples 5 and 6 cannot work independently and need to be added with commercial electrolyte to achieve the purpose of testing, which violates the original intention of the present invention.

[0048] Embodiment 1:

[0049] A method for preparing an air-friendly polymer-based solid-state lithium battery electrolyte comprises the following steps:

[0050] S1. Preparation of ion transport active polymer-based electrolyte slurry: Weigh 0.8 g of polyethylene oxide (active polymer) and add it to a beaker containing 12 mL of acetonitrile (polar aprotic solvent), stirring continuously during the addition. Weigh lithium bis(trifluoromethanesulfonyl imide) (lithium salt) at a ratio of 1:3 of lithium salt to active polymer mass, add it to the above slurry, stirring continuously during the addition until the slurry becomes transparent.

[0051] S2. Preparation of skeleton-supported polymer-based electrolyte slurry: Weigh 0.4 g of polyvinylidene fluoride-hexafluoropropylene (skeleton-supported polymer) at a mass ratio of 2:1 between active polymer and skeleton-supported polymer, add it to a beaker, then add 4 mL of N-methylpyrrolidone (polar aprotic solvent) and continue stirring until all dissolved.

[0052] S3. Mixing of an air-friendly polymer-based solid-state lithium battery electrolyte slurry: Pour the skeleton-supported polymer slurry obtained in step S2 into the active polymer slurry obtained in step S1. Rinse the beaker in step S2 three times with 4 mL of N-methylpyrrolidone, and pour all the rinse solution into the slurry obtained in step S1. Stir the mixed slurry thoroughly until it is transparent and there is no stratification. Finally, place it in a cool and dry place to remove bubbles.

[0053] S4. Preparation of an air-friendly polymer-based solid-state lithium battery electrolyte: The operations are all carried out in a fume hood. Use a glass syringe to extract 0.6 mL of the slurry each time, pour it into a mold with a diameter of 20.0 mm and a depth of 3.2 mm, and then dry it at 60-80 °C for 3-6 h to obtain a membrane product of an air-friendly polymer-based solid-state lithium battery electrolyte.

[0054] The visual state results of the air-friendly polymer-based solid-state lithium battery electrolyte membrane prepared in Example 1 are shown in Table 3.

[0055] Table 3

[0056] Time (h) Temperature (℃) 3 4 5 6 60 The slurry still exists The slurry still exists The slurry still exists The membrane cannot fall off 80 Easy to tear Film forming and easy to remove Partially molten Partially molten

[0057] After many experiments, the optimal experimental conditions were found to be: drying temperature 80℃ and drying time 4 h.

[0058] Embodiment 2:

[0059] A method for preparing an air-friendly polymer-based solid-state lithium battery electrolyte comprises the following steps:

[0060] S1. Preparation of ion transport active polymer-based electrolyte slurry: Weigh 0.8g of polyethylene oxide and add it to a beaker containing 12 mL of acetonitrile, stirring continuously during the addition. Weigh lithium bis(trifluoromethanesulfonyl)imide at a ratio of 1:3 of lithium salt to active polymer mass ratio and add it to the above slurry, stirring continuously during the addition. Weigh succinonitrile (amorphizing agent) at a mass fraction of (0.0, 20.0, 25.0, 30.0) wt.% of the amorphizing agent in the active polymer-cured electrolyte system and add it to the above slurry, stirring continuously during the addition until the slurry becomes transparent.

[0061] S2. Preparation of skeleton-supported polymer-based electrolyte slurry: Weigh 0.8 g of polyvinylidene fluoride-hexafluoropropylene with a mass ratio of active polymer to skeleton-supported polymer of 1:1, add it to a beaker, then add 4 mL of N-methylpyrrolidone and continue stirring until it is completely dissolved.

[0062] S3. Mixing of an air-friendly polymer-based solid-state lithium battery electrolyte slurry: Pour the skeleton support polymer slurry obtained in step S2 into the active polymer slurry obtained in step S1. Rinse the beaker in step S2 three times with 4 mL of N-methylpyrrolidone, and pour all the rinse liquid into the slurry obtained in step S1. Stir the mixed slurry thoroughly until it is transparent and there is no stratification. Finally, place it in a cool and dry place to remove bubbles.

[0063] S4. Preparation of an air-friendly polymer-based solid-state lithium battery electrolyte: The operations were all carried out in a fume hood. Using a glass syringe, 0.6 mL of the slurry was drawn each time and poured into a mold with a diameter of 20.0 mm and a depth of 3.2 mm, and then dried at 80 °C for 4 h to obtain a membrane product of an air-friendly polymer-based solid-state lithium battery electrolyte.

[0064] Embodiment 3:

[0065] A method for preparing an air-friendly polymer-based solid-state lithium battery electrolyte comprises the following steps:

[0066] S1. Preparation of ion transport active polymer-based electrolyte slurry: Weigh 0.4g polyethylene oxide and add it to a beaker containing 12ml acetonitrile, stirring continuously. Weigh lithium bis(trifluoromethanesulfonyl)imide at a lithium salt to active polymer mass ratio of 1:3 and add it to the above slurry, stirring continuously. Weigh succinonitrile at a mass fraction of (0.0, 20.0, 25.0, 30.0) wt.% of the amorphizing agent in the active polymer-cured electrolyte system and add it to the above slurry, stirring continuously until the slurry becomes transparent.

[0067] S2. Preparation of skeleton-supported polymer-based electrolyte slurry: Weigh 0.8 g of skeleton-supported polymer with a mass ratio of active polymer to skeleton-supported polymer of 1:2, add it into a beaker, then add 4 mL of N-methylpyrrolidone and continue stirring until it is completely dissolved.

[0068] S3. Mixing of an air-friendly polymer-based solid-state lithium battery electrolyte slurry: Pour the skeleton support polymer slurry obtained in step S2 into the active polymer slurry obtained in step S1. Rinse the beaker in step S2 three times with 4 mL of N-methylpyrrolidone, and pour all the rinse liquid into the slurry obtained in step S1. Stir the mixed slurry thoroughly until it is transparent and there is no stratification. Finally, place it in a cool and dry place to stand and remove bubbles.

[0069] S4. Preparation of an air-friendly polymer-based solid-state lithium battery electrolyte: All operations were performed in a fume hood. Using a glass syringe, 0.6 mL of the slurry was drawn each time and poured into a mold with a diameter of 20.0 mm and a depth of 3.2 mm, and then dried at 80 °C for 4 h to obtain an air-friendly polymer-based solid-state lithium battery electrolyte.

[0070] Embodiment 4:

[0071] A method for preparing an air-friendly polymer-based solid-state lithium battery electrolyte comprises the following steps:

[0072] S1. Preparation of ion transport active polymer-based electrolyte slurry: Weigh 0.8 g of polyacrylonitrile and add it to a beaker containing 12 mL of N,N-dimethylformamide, stirring continuously during the addition. Weigh lithium bis(trifluoromethanesulfonyl)imide at a ratio of 1:3 of lithium salt to active polymer mass ratio, add it to the above slurry, and stir continuously during the addition until the slurry becomes transparent. Weigh adiponitrile and 1,3,5-pentanetricarbonitrile respectively at a mass fraction of 20.0 wt.% of the amorphizing agent in the active polymer-cured electrolyte system, add them to the above slurry, and stir continuously during the addition until the slurry becomes transparent.

[0073] S2. Preparation of skeleton-supported polymer-based electrolyte slurry: Weigh 0.8 g of polyvinylidene fluoride with a mass ratio of active polymer to skeleton-supported polymer of 1:1, add it to a beaker, then add 4 mL of N-methylpyrrolidone and continue stirring until it is completely dissolved.

[0074] S3. Mixing of an air-friendly polymer-based solid-state lithium battery electrolyte slurry: Pour the skeleton support polymer slurry obtained in step S2 into the active polymer slurry obtained in step S1. Rinse the beaker in step S2 three times with 4 mL of N-methylpyrrolidone, and pour all the rinse liquid into the slurry obtained in step S1. Stir the mixed slurry thoroughly until it is transparent and there is no stratification. Finally, place it in a cool and dry place to remove bubbles.

[0075] S4. Preparation of an air-friendly polymer-based solid-state lithium battery electrolyte: The operations were all carried out in a fume hood. Using a glass syringe, 0.6 mL of the slurry was drawn each time and poured into a mold with a diameter of 20.0 mm and a depth of 3.2 mm, and then dried at 80 °C for 4 h to obtain a membrane product of an air-friendly polymer-based solid-state lithium battery electrolyte.

[0076] After multiple experiments, the film formation probability of Example 4 using different amorphization agents was extremely low, and the resulting solid electrolyte membrane had poor flexibility, was easily broken, and could not work normally at room temperature.

[0077] Result characterization and performance testing:

[0078] (1) Figure 1 This is a photo of the air-friendly polymer-based solid-state lithium battery electrolyte membrane prepared in Example 2-2. The solid-state electrolyte membrane is circular with a diameter of 17.0 mm, a thickness of 0.07 mm, and a flat surface. It has good toughness, is bendable, and has a low thickness.

[0079] (2) Electrochemical impedance spectroscopy and ionic conductivity calculation

[0080] The stainless steel sheet|solid electrolyte|stainless steel sheet button cell was assembled in air and the electrochemical impedance was measured at 25°C. The present invention adopts CHI660e electrochemical workstation with a frequency range of 10 6 ~0.1Hz, voltage amplitude is 10 mV. The calculation results are shown in Table 4 by the formula σ=L / (R·S) (σ is ionic conductivity, L is electrolyte thickness, R is electrolyte impedance, S is the effective contact area between electrolyte and stainless steel sheet).

[0081] Table 4

[0082] sample Mass fraction of amorphization agent (wt.%) Electrochemical impedance at 25°C (Ω) Thickness of electrolyte (cm) Ionic conductivity (S / cm) Example 1 0 240 0.007 <![CDATA[1.42×10 -5 ]]> Example 2-1 0 1034 0.007 <![CDATA[3.29×10 -6 ]]> Example 2-2 20 13 0.007 <![CDATA[2.61×10 -4 ]]> Example 2-3 25 165 0.007 <![CDATA[2.06×10 -5 ]]> Embodiment 2-4 30 73 0.007 <![CDATA[4.65×10 -5 ]]> Example 3-1 0 3556 0.007 <![CDATA[9.56×10 -7 ]]> Example 3-2 20 176 0.007 <![CDATA[1.93×10 -5 ]]> Example 3-3 25 140 0.007 <![CDATA[2.43×10 -5 ]]> Embodiment 3-4 30 68 0.007 <![CDATA[4.99×10 -5 ]]> Comparative Example 1 0 1328 0.01 <![CDATA[3.66×10 -6 ]]> Comparative Example 3 0 5482 0.01 <![CDATA[8.85×10 -7 ]]>

[0083] Figure 2 The scanning electron microscope photographs of the electrolyte membrane prepared in Example 2-2 from different viewing angles. Figure 2 From the microscopic morphology of the electrolyte membrane surface shown in a, it can be seen that the surface of the prepared air-friendly polymer-based solid-state lithium battery electrolyte is flat, and there are still irregular crystal parts on the surface due to solidification and crystallization. Figure 2 b The magnified photo of the electrolyte membrane surface shows that there are holes between different crystal regions. Figure 2 c The cross-sectional photo of the electrolyte membrane shows that the thickness of the solid electrolyte is 70 μm. Figure 2d In the enlarged photo of the cross-section area of ​​the electrolyte membrane slice, it can be observed that the holes in the solid electrolyte are irregular holes and run through the entire solid electrolyte film. The existence of holes is conducive to the high-speed shuttle of lithium ions in them, keeping the ion flow unimpeded. In addition, there are a large number of through holes in the solid electrolyte of the present invention, which is more beneficial to the transmission of lithium ions.

[0084] Figure 3 The XRD spectra of the air-friendly polymer-based solid lithium battery electrolyte of Comparative Example 1 and Example 2-2 are shown. No amorphizing agent was added in Comparative Example 1, and the crystallinity of the electrolyte membrane was calculated to be 78%. After the amorphizing agent was added in Example 2-2, the crystallinity of the solid electrolyte membrane was 11%. This indicates that after the amorphizing agent was added, the crystallinity of the air-friendly polymer solid electrolyte was significantly reduced, and the reduction in crystallinity ensures the good performance of the solid electrolyte at room temperature.

[0085] Figure 4 The stress-strain curves of air-friendly polymer-based solid-state lithium battery electrolytes in some embodiments are shown in the figure. As can be seen from the figure, the content of the skeleton-supported polymer greatly affects the mechanical properties of the solid electrolyte membrane. The larger the proportion of the skeleton-supported polymer, the better the mechanical properties. The addition of an amorphizing agent reduces the crystallinity of the solid electrolyte membrane, and the reduction in mechanical properties also reflects this feature. While ensuring high ionic conductivity, the solid electrolyte membrane also takes into account certain mechanical properties.

[0086] Figure 5 This is the electrochemical window test of the button half-cell assembled with the electrolyte membrane in Comparative Example 1 and Example 2-2. The stainless steel sheet|solid electrolyte|lithium sheet button cell was assembled in an argon atmosphere glove box and the linear sweep voltammetry test was performed by an electrochemical workstation. The voltage range of the linear sweep voltammetry test was 3-6 V and the scan rate was 1 mV / S. Figure 5 It can be seen that the electrochemical window of Example 2-2 is about 4.86 V, which is greater than the electrochemical window of the comparative example of 4.75 V. This indicates that the prepared air-friendly polymer-based solid-state lithium battery electrolyte has a higher electrochemical window, and the high electrochemical window has the ability to match high-voltage positive electrode materials.

[0087] Figure 6The cycle performance of the lithium iron phosphate solid-state lithium battery assembled with the electrolyte membrane in Example 2-2 at room temperature. The lithium iron phosphate | solid electrolyte | lithium sheet button battery was assembled in an argon atmosphere glove box, and the charge and discharge cycle test was carried out using the Blue Electric Battery Test System. As can be seen from the figure, the lithium iron phosphate button battery with an air-friendly polymer-based solid electrolyte still has a capacity retention rate of 85.5% after 50 cycles at room temperature and 0.1C; the coulomb efficiency is maintained at around 100%, indicating that the charge and discharge process is very stable. However, Comparative Examples 1 and 2 do not work at room temperature. It shows that the air-friendly polymer-based solid-state lithium battery electrolyte prepared by the present invention ensures the stable cycle of the battery at room temperature and a longer battery life.

[0088] The air environment-friendly polymer-based solid lithium battery electrolyte prepared by the present invention has the advantages of good room temperature ionic conductivity and good mechanical properties. The processing method prepared in an air environment can shorten the production cycle, simplify the processing technology, and has low preparation cost, which is more conducive to large-scale production. The solid electrolyte membrane prepared by the present invention can replace commercial diaphragms, and can be directly applied to lithium batteries and lithium ion batteries without adding electrolyte, and can effectively inhibit the growth of lithium dendrites, improve the poor interface contact problem between electrode materials and electrolytes, and has broad application prospects.

[0089] The specific comparisons and implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific comparison and implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing an air-friendly polymer-based solid-state lithium battery electrolyte, wherein the air-friendly polymer-based solid-state lithium battery electrolyte is prepared by compounding an ion-transmitting active polymer, a skeleton-supporting polymer, a lithium salt and an amorphizing agent; wherein the mass ratio of the active polymer to the skeleton-supporting polymer is (0.0-2.0):(0.0-2.0); the mass ratio of the lithium salt to the active polymer is 1:3, and the mass fraction of the amorphizing agent in the active polymer solid electrolyte system is (20.0-30.0) wt.%.

2. The method for preparing an air-friendly polymer-based solid-state lithium battery electrolyte according to claim 1, characterized in that: The preparation method comprises the following steps: S1. Preparation of ion transport active polymer-based electrolyte slurry: adding active polymer, lithium salt and amorphization agent into a polar aprotic solvent and fully dissolving them by stirring; S2. Preparation of skeleton-supported polymer-based electrolyte slurry: adding skeleton-supported polymer to polar aprotic solvent and fully dissolving it by stirring; S3, mixing of air-friendly polymer-based solid-state lithium battery electrolyte slurry: pouring the slurry obtained in step S2 into the beaker of step S1, rinsing the beaker in step S2 with an appropriate amount of backbone polymer polar aprotic solvent in batches, and pouring it into the beaker of step S1, and mixing it evenly by stirring; S4. Preparation of air-friendly polymer-based solid-state lithium battery electrolyte: The slurry obtained in step S3 is cast in a specific mold in an appropriate amount using a casting method, and then heated and dried at 40-80°C for 4-6 hours to obtain a film-type product of a certain thickness of the air-friendly polymer-based solid-state lithium battery electrolyte.

3. According to claim 1, the ion transport active polymer can be one of polyethylene oxide (PEO), polypropylene oxide (PPO), polyacrylonitrile (PAN) and their grafted polymers; the skeleton support polymer can be one of strong skeleton structure polymers such as polyvinylidene fluoride (PVDF), polyvinyl alcohol (PVA), fluorinated polymer PVDF-HFP, etc.; the lithium salt can be one of organic anion lithium salts such as lithium bis(trifluoromethanesulfonyl)imide, etc.; the amorphization reagent can be one of reagents such as adiponitrile, succinonitrile, 1,3,5-pentanetricarbonitrile, etc.

4. According to claim 2, the mass ratio of the active polymer to the skeleton supporting polymer is (2.0﹕0.0), (2.0﹕1.0), (1.0﹕1.0), (1.0﹕2.0), (0.0﹕2.0); the mass ratio of lithium salt to active polymer is 1:3, and the mass fraction of the amorphization agent in the active polymer electrolyte system is (0.0, 20.0, 25.0, 30.0) wt.%.

5. The method for preparing an air-friendly polymer-based solid electrolyte according to claim 2 or claim 4, characterized in that: The solvent used to dissolve the ion transport active polymer and the skeleton support polymer in steps S1 and S2 is one of polar aprotic solvents such as acetonitrile, N-methylpyrrolidone, N,N-dimethylformamide, etc.

6. The appropriate amount according to step S4 in claim 2 is 0.6 mL; the specific mold is a polytetrafluoroethylene mold with a diameter of 20.0 mm and a depth of 3.2 mm.

7. An air-friendly polymer-based solid-state lithium battery, characterized in that: The solid-state lithium battery is composed of a positive electrode, the air-friendly polymer-based solid-state lithium battery electrolyte described in claim 1, and a negative electrode; the air-friendly polymer-based solid-state lithium battery electrolyte is located between the positive electrode and the negative electrode, and no electrolyte is used.

8. The solid-state lithium battery according to claim 7, characterized in that: The positive electrode sheet is composed of a current collector, a positive electrode material, a conductive agent and a binder; the positive electrode material uses one of the ternary positive electrode materials of lithium iron phosphate or lithium nickel cobalt manganese oxide; the negative electrode sheet uses a round lithium sheet with a diameter of 16.0 mm and a thickness of 0.6 mm.

Citation Information

Patent Citations

  • Polymer-based composite solid electrolyte as well as preparation method and application thereof

    CN113206292A

  • Quick-charge type solid electrolyte, all-solid-state battery and preparation method of positive electrode material

    CN118248938A