Method for producing LGPS-based solid electrolyte and method for producing all-solid-state battery

By using organic solvents containing a specific amount of sulfur to remove impurities in lithium-ion secondary batteries, the problem of low ion conductivity caused by unreacted residues is solved, and a high purity and high performance LGPS-based solid electrolyte is achieved. The manufacturing of all solid state batteries is suitable for applications.

CN119013738APending Publication Date: 2024-11-22MITSUBISHI GAS CHEM CO INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380033606.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-21
Filing Date
2023-04-17
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

When the existing lithium-ion secondary batteries use organic solvents to synthesize Li3PS4 solid electrolytes, unreacted Li2S and intermediate Li4P2S7 are easily retained, resulting in low ionic conductivity and difficulty in separation, affecting battery performance.

Method used

The Li3PS4 powder is stirred and filtered with an organic solvent containing a specific amount of sulfur to remove impurities and improve the purity and ionic conductivity of the electrolyte. The specific steps include adding 0.1 to 1.75 mass% sulfur solvent to the Li3PS4 powder, stirring and filtering, and Vacuum drying is carried out in an inactive gas environment to form a high-purity LGPS-based solid electrolyte.

Benefits of technology

This method significantly improves the purity and ionic conductivity of Li3PS4, achieves good electrochemical performance, is suitable for the manufacturing of all-solid-state batteries, and improves the safety and performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013738A_ABST
    Figure CN119013738A_ABST
Patent Text Reader

Abstract

The present invention relates to a method for producing an LGPS-based solid electrolyte, which is characterized by comprising: a step for preparing a Li3PS4 powder or for preparing a Li3PS4 powder from at least Li2S and P2S5; and a step in which a solvent containing 0.1-1.75 mass% of sulfur in the organic solvent is added to the Li3PS4 powder, and impurities in the Li3PS4 powder are removed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing an LGPS solid electrolyte and a method for manufacturing an all-solid-state battery. It should be noted that the LGPS solid electrolyte refers to a solid electrolyte having a specific crystal structure containing Li, P and S, for example, a solid electrolyte containing Li, M (M is one or more elements selected from Ge, Si and Sn), P and S. Background Art

[0002] In recent years, the demand for lithium-ion secondary batteries has been increasing in applications such as portable information terminals, portable electronic devices, electric vehicles, hybrid electric vehicles, and stationary power storage systems. However, current lithium-ion secondary batteries use flammable organic solvents as electrolytes and require a sturdy outer packaging to prevent the organic solvent from leaking. In addition, in portable computers, etc., there are restrictions on the device structure, such as the need to take precautions against the risk of electrolyte leakage.

[0003] In addition, as the use of stationary lithium-ion secondary batteries expands to mobile objects such as automobiles and airplanes, they are required to have larger capacities. Under such circumstances, safety tends to be more important than before, and great efforts are also devoted to the development of all-solid-state lithium-ion secondary batteries that do not use harmful substances such as organic solvents.

[0004] For example, as a solid electrolyte in an all-solid-state lithium ion secondary battery, use of oxides, phosphoric acid compounds, organic polymers, sulfides, and the like has been studied.

[0005] Among these solid electrolytes, sulfides have the characteristics of high ion conductivity and easy formation of interfaces between solids due to their softness. The development of solid electrolytes that are stable as active materials and highly practical has been progressing.

[0006] As a conventional method for manufacturing Li3PS4 as a sulfide solid electrolyte, a synthesis method using a planetary ball mill and an organic solvent can be cited. However, unreacted Li2S is easily left in the synthesized Li3PS4, and because Li2S is a solid, there are few solvents that can dissolve it. For example, although alcohol is a solvent that can dissolve Li2S, it also decomposes Li3PS4 (Patent Document 1), making it difficult to separate Li3PS4 from Li2S. In addition, although the compound Li4P2S7 that exists as an intermediate can be separated in the filtration process in the synthesis using an organic solvent, a small amount still remains in Li3PS4.

[0007] Prior Art Literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2020-027781 Summary of the invention

[0010] Problems to be solved by the invention

[0011] Under such circumstances, it is necessary to provide a method for producing an LGPS-based solid electrolyte having excellent productivity and good ion conductivity.

[0012] Technical means to solve problems

[0013] Therefore, the inventors have conducted in-depth research in view of the above problems and found that once unreacted Li2S and intermediate Li4P2S7 remain as impurities in Li3PS4, they will become the cause of low ion conductivity when manufacturing LGPS solid electrolytes. In addition, the inventors have also obtained an unexpected understanding that by removing impurities from Li3PS4 powder using an organic solvent containing a specific amount of sulfur, LGPS solid electrolytes with good ion conductivity can be manufactured.

[0014] That is, the present invention includes the following aspects.

[0015] <1> A method for producing a LGPS-based solid electrolyte, characterized in that it comprises a step of preparing Li3PS4 powder, or preparing Li3PS4 powder from at least Li2S and P2S5; and

[0016] A step of adding a solvent containing 0.1 to 1.75 mass % of sulfur in an organic solvent to the above-mentioned Li3PS4 powder to remove impurities in the above-mentioned Li3PS4 powder.

[0017] <2> According to the above <1> The manufacturing method, wherein the impurities include unreacted Li2S or intermediate Li4P2S7.

[0018] <3> According to the above <1> or <2> In the production method, the organic solvent is at least one selected from tetrahydrofuran, acetonitrile, ethyl acetate and methyl acetate.

[0019] <4> According to the above <1> ~ <3> The manufacturing method described in any one of the above, wherein the step of removing the above-mentioned impurities includes the steps of stirring the above-mentioned Li3PS4 powder and the above-mentioned solvent and filtering the obtained mixture.

[0020] <5> According to the above <4> In the manufacturing method, the process of removing the impurities further comprises the step of vacuum drying the filter residue after filtering the mixture.

[0021] <6> According to the above <1> ~ <5> The production method described in any one of the preceding claims, wherein the Li3PS4 is β-Li3PS4.

[0022] <7> According to the above <1> ~ <6> Any one of the manufacturing methods described above includes a step of manufacturing a Sn-type LGPS solid electrolyte by sintering a mixture obtained by using Li3PS4 powder from which the above-mentioned impurities have been removed and Li4SnS4 prepared from Li2S and SnS2 under an inert gas environment.

[0023] <8> According to the above <1> ~ <7> The manufacturing method described in any one of the above, wherein the LGPS-based solid electrolyte has a X-ray diffraction (CuKα: ), there are peaks at least at the positions of 2θ=19.90°±0.50°, 20.20°±0.50°, 26.70°±0.50° and 29.20°±0.50°.

[0024] <9> According to the above <1> ~ <8> The manufacturing method described in any one of the above-mentioned claims, wherein the above-mentioned LGPS-based solid electrolyte contains the following crystal structure as a main body, the crystal structure having an octahedron O composed of Li element and S element, a tetrahedron T1 composed of one or more elements selected from P and Sn and the S element, and a tetrahedron T2 composed of the P element and the S element, and the above-mentioned tetrahedron T1 shares edges with the above-mentioned octahedron O and the above-mentioned tetrahedron T2 shares vertices with the above-mentioned octahedron O.

[0025] <10> A method for manufacturing an all-solid-state battery, comprising: <1> ~ <9> A step of pressure-molding the LGPS solid electrolyte obtained by any one of the production methods.

[0026] Effects of the Invention

[0027] According to the present invention, a method for producing an LGPS solid electrolyte having good ionic conductivity by improving the purity of Li3PS4, which is a raw material of the LGPS solid electrolyte, can be provided. Moreover, the production method may also be applied to mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 A schematic diagram of the crystal structure of an LGPS-based solid electrolyte according to one embodiment of the present invention.

[0029] Figure 2 A schematic cross-sectional view of an all-solid-state battery according to one embodiment of the present invention.

[0030] Figure 3A figure showing the X-ray diffraction measurement results of the Li3PS4 powder obtained after the impurity removal process in each example and comparative example. However, the impurity removal process was not performed in Comparative Example 1.

[0031] Figure 4 A figure showing the 31 P solid NMR results of the Li3PS4 powder obtained after the impurity removal process in Example 1 and Example 2 and the Li3PS4 powder obtained without the impurity removal process in Comparative Example 1.

[0032] Figure 5 A figure showing the 31 P solid NMR results of the filter residue obtained by filtration and the powder after concentration of the filtrate in the impurity removal process of Example 1 and the Li3PS4 powder obtained without the impurity removal process in Comparative Example 1.

[0033] Figure 6 A figure showing the measurement results of the ionic conductivity of the solid electrolytes obtained in Examples 1 to 3 and Comparative Examples 1 to 2. Detailed implementation mode

[0034] Hereinafter, the manufacturing method of the LGPS-based solid electrolyte of the present invention will be specifically described. It should be noted that the materials, compositions, etc. described below are not limitations on the present invention, and various changes can be made within the scope of the gist of the present invention.

[0035] <Manufacturing method of LGPS-based solid electrolyte>

[0036] The manufacturing method of the LGPS-based solid electrolyte of the present invention includes a step of preparing Li3PS4 powder, or preparing Li3PS4 powder at least from Li2S and P2S5; and a step of adding a solvent containing 0.1 to 1.75% by mass of sulfur in an organic solvent to the above Li3PS4 powder to remove impurities in the above Li3PS4 powder.

[0037] The Li3PS4 used in the present invention preferably has a peak at 420 ± 10 cm ﹣1 in Raman spectroscopy measurement.

[0038] The above LGPS-based solid electrolyte in X-ray diffraction (CuKα: ) has peaks at least at positions of 2θ = 19.90° ± 0.50°, 20.20° ± 0.50°, 26.70° ± 0.50° and 29.20° ± 0.50°.

[0039] In addition, the above LGPS-based solid electrolyte is as Figure 1As shown, it preferably contains the following crystal structure as the main body. This crystal structure has an octahedron O composed of Li and S elements, a tetrahedron T1 composed of one or more elements selected from P and Sn and S elements, and a tetrahedron T2 composed of P and S elements. The tetrahedron T1 shares an edge with the octahedron O, and the tetrahedron T2 shares a vertex with the octahedron O.

[0040] <Preparation of Li3PS4>

[0041] Li3PS4 used in the present invention can be any of α, β, and γ types, but β-LPS is more preferred. The reason is that it can exist relatively stably in the LGPS synthesis system.

[0042] Li3PS4 in the present invention can be a commercially available product, or Li3PS4 can be manufactured by mechanically grinding sulfides represented by Li2S and P2S5 using a planetary ball mill, or it can also be synthesized from sulfides represented by Li2S and P2S5 in an inert gas environment such as argon.

[0043] If an example of the manufacturing method of Li3PS4 is given, it is by weighing Li2S and P2S5 according to a molar ratio of Li2S:P2S5 = 3:1, adding Li2S and P2S5 to tetrahydrofuran in sequence, making the concentration of (Li2S + P2S5) 10 wt%, and mixing at room temperature for a specified time to obtain a precipitate. By subjecting the filter residue obtained by filtering the product to vacuum drying, Li3PS4 can be manufactured.

[0044] In addition, if another example of the manufacturing method of Li3PS4 is given, it is by weighing Li2S and P2S5 according to a molar ratio of Li2S:P2S5 = 1.5:1, adding Li2S and P2S5 to tetrahydrofuran in sequence, making the concentration of (Li2S + P2S5) 10 wt%, and mixing at room temperature for a specified time to obtain a homogeneous solution. It should be noted that at this time, depending on the purity of the raw materials and the progress of the reaction, there may be a small amount of precipitates, but it has little impact on the purity of the finally obtained Li3PS4. However, in the case where precipitates have been formed, filtration can be carried out to remove the precipitates. Further add Li2S to the obtained homogeneous solution so that the composition including all the above raw materials reaches a weight ratio of Li2S:P2S5 = 3:1, and a precipitate is obtained in a state of mixing at room temperature for a specified time. By subjecting the filter residue obtained by filtering the product to vacuum drying, Li3PS4 can be manufactured.

[0045] Li2S can be either a synthetic product or a commercial product. Since the mixing of water may cause the deterioration of other raw materials and precursors, the water content is preferably small, more preferably 300 ppm or less, and particularly preferably 50 ppm or less.

[0046] It should be noted that even if part of the above raw materials is amorphous, there will be no problem in use.

[0047] Regardless of the raw material, a small particle size is important, and the particle diameter is preferably in the range of 10 nm to 10 μm, more preferably in the range of 10 nm to 5 μm, and further preferably in the range of 100 nm to 1 μm. It should be noted that the particle size can be measured by SEM or by a particle size distribution measuring device using laser scattering. Since the particles are small, they are prone to reaction during the heat treatment process, which can inhibit the generation of by-products.

[0048] P2S5 can be used as either a synthetic product or a commercial product. Products with high purity of P2S5 are preferred because the impurities mixed into the solid electrolyte are reduced. Products with small particle size of P2S5 are preferred because the reaction speed is accelerated. The particle diameter is preferably in the range of 10nm to 100μm, more preferably in the range of 10nm to 30μm, and further preferably in the range of 100nm to 10μm.

[0049] <Impurity Removal Process>

[0050] The impurity removal step of the present invention is a step of adding a solvent containing 0.1 to 1.75% by mass of sulfur in an organic solvent to the Li3PS4 powder obtained above to remove impurities in the Li3PS4 powder. That is, the total amount of the solvent needs to contain 0.1 to 1.75% by mass, preferably 0.5 to 1.7% by mass, and more preferably 1.0 to 1.7% by mass of sulfur.

[0051] The sulfur used in the present invention is preferably high-purity sulfur, and for example, pure sulfur (purity 99.99%) manufactured by Kojundo Chemical Laboratory Co., Ltd. is particularly preferably used.

[0052] The organic solvent contained in the solvent used in the present invention preferably contains at least one selected from tetrahydrofuran, acetonitrile, ethyl acetate and methyl acetate, and more preferably contains tetrahydrofuran.

[0053] In order to prevent the raw material composition from deteriorating, it is preferred to remove oxygen and water in the organic solvent in advance. In particular, the water content is preferably 100 ppm or less, more preferably 50 ppm or less.

[0054] In the impurity removal step of the present invention, it is preferred that the Li3PS4 powder and the solvent are stirred and the obtained mixture is filtered.

[0055] The stirring method is not a specific method and can be carried out in air or in an inert gas environment. As the inert gas, nitrogen, helium, argon, etc. can be used, and the deterioration of the raw material composition is suppressed by removing both oxygen and moisture in the inert gas. The concentration of both oxygen and moisture in the inert gas is preferably 1000 ppm or less, more preferably 100 ppm or less, and particularly preferably 10 ppm or less.

[0056] The filtration method is not a specific method and can be carried out under pressure or without pressure.

[0057] In the impurity removal step of the present invention, it is preferred to further perform vacuum drying on the filter residue obtained by filtering the above mixture.

[0058] The vacuum drying method is not a specific method. The drying temperature is usually about 100 to 200 °C, and the drying time is usually about 2 to 6 hours.

[0059] In the impurity removal step of the present invention, it is preferred that the impurities include at least one of unreacted Li2S and intermediate Li4P2S7. By removing these impurities, an LGPS-based solid electrolyte with high ionic conductivity can be manufactured.

[0060] <Micronization of Li3PS4>

[0061] In a preferred embodiment of the present invention, by mixing the Li3PS4 powder from which the above impurities have been removed with an acetonitrile solvent, particles of about 1 μm can be formed. Then, by performing vacuum drying on the suspension at a temperature of 150 to 210 °C for 2 to 6 hours in a vacuum environment, micronized Li3PS4 powder from which the coordinating solvent has been removed can be obtained.

[0062] <Preparation of Li4SnS4>

[0063] A preferred embodiment of the present invention includes a step of firing a mixture obtained by using the micronized Li3PS4 powder from which the above impurities have been removed and Li4SnS4 prepared from Li2S and SnS2 in an inert gas environment to manufacture an Sn-type LGPS-based solid electrolyte.

[0064] In the present invention, Li4SnS4 preferably used can be a commercially available product or can be synthesized from sulfides represented by Li2S and SnS2 in an inert gas environment such as argon. If an example of the manufacturing method of Li4SnS4 is given, it can be prepared by weighing according to a molar ratio of Li2S∶SnS2 = 2∶1, mixing using an agate mortar; then, putting the obtained mixture into a zirconia crucible, further putting zirconia balls, completely sealing the crucible, and then assembling the crucible on a planetary ball mill to manufacture Li4SnS4 by mechanical grinding.

[0065] In a preferred embodiment of the present invention, a homogeneous solution can be prepared by dissolving the above-obtained Li4SnS4 in an alcohol solvent.

[0066] Examples of the above alcohol solvents include methanol, ethanol, 1-propanol, 1-butanol, 1-pentanol, 1-hexanol, 1-heptanol, 1-octanol, etc. Among them, at least one selected from methanol, ethanol, 1-propanol, and 1-butanol is preferred.

[0067] The dissolution is preferably carried out in an inert gas environment. As the inert gas, nitrogen, helium, argon, etc. can be used. By removing both oxygen and moisture in the inert gas, the deterioration of the raw material composition can be inhibited. The concentration of both oxygen and moisture in the inert gas is preferably 1000 ppm or less, more preferably 100 ppm or less, and particularly preferably 10 ppm or less.

[0068] In a preferred embodiment of the present invention, by dropping the above-obtained homogeneous solution into acetonitrile, Li4SnS4 particles can be precipitated in acetonitrile. Then, in a vacuum environment, the precipitated particles are dried at a temperature of 150 to 210 °C for 2 to 6 hours, and Li4SnS4 powder from which the coordination solvent has been removed can be obtained.

[0069] <Manufacture of LGPS-based solid electrolyte>

[0070] As described above, a preferred embodiment of the present invention includes a step of firing a mixture obtained by using Li3PS4 powder from which the above impurities have been removed and Li4SnS4 obtained as described above in an inert gas environment to manufacture an Sn-type LGPS-based solid electrolyte.

[0071] When obtaining the mixture, as long as the molar ratio of Li3PS4∶Li4SnS4 = 3∶1 to 2∶3, the obtained solid electrolyte will have almost only the peaks of LGPS crystals in XRD measurement, and the ionic conductivity will be relatively high. For example, when it is Li 9.81 Sn 0.81 P 2.19 S 12In this case, the mixture is mixed in a molar ratio of Li3PS4:Li4SnS4=2.7:1.

[0072] The mixing is preferably carried out under an inert gas environment. As the inert gas, nitrogen, helium, argon, etc. can be used. By removing both oxygen and water in the inert gas, the raw material composition can be inhibited from deteriorating. The concentrations of both oxygen and water in the inert gas are preferably 1000 ppm or less, more preferably 100 ppm or less, and particularly preferably 10 ppm or less.

[0073] In a preferred embodiment of the present invention, the LGPS solid electrolyte is obtained by heating the obtained mixture at a temperature of 300 to 700°C. The heating temperature is preferably in the range of 350 to 650°C, more preferably in the range of 400 to 600°C. When the temperature is lower than 300°C, it is difficult to generate the desired crystals; on the other hand, when the temperature is higher than 700°C, crystals other than the target may also be generated, resulting in a decrease in ionic conductivity.

[0074] Although the heating time varies to some extent depending on the heating temperature, a range of 0.1 to 24 hours is generally sufficient to achieve crystallization. Heating for a long time at a high temperature beyond the above range is not preferred because it may cause deterioration of the LGPS solid electrolyte.

[0075] The heating can be carried out in a vacuum or inert gas environment, preferably in an inert gas environment. As the inert gas, nitrogen, helium, argon, etc. can be used, among which argon is preferred. It is preferred that the oxygen and water content are low.

[0076] The LGPS solid electrolyte of the present invention obtained as described above can be formed into a desired molded body by various means and used in various applications represented by all-solid-state batteries described below. The molding method is not particularly limited. For example, the same method as the molding method of each layer constituting the all-solid-state battery described in the all-solid-state battery described later can be used.

[0077] <All-solid-state battery>

[0078] The LGPS-based solid electrolyte of the present invention can be used as, for example, a solid electrolyte for an all-solid-state battery. In addition, according to another embodiment of the present invention, an all-solid-state battery containing the above-mentioned solid electrolyte for an all-solid-state battery can also be provided.

[0079] Here, the "all-solid-state battery" in this embodiment refers to an all-solid-state lithium-ion secondary battery. Figure 2Schematic cross-sectional view of an all-solid-state battery according to an embodiment of the present invention. The all-solid-state battery 10 has a structure in which a solid electrolyte layer 2 is arranged between a positive electrode layer 1 and a negative electrode layer 3. The all-solid-state battery 10 can be used in various devices represented by mobile phones, personal computers, and automobiles.

[0080] The LGPS solid electrolyte of the present invention can be contained as a solid electrolyte in any one or more of the positive electrode layer 1, the negative electrode layer 3 and the solid electrolyte layer 2. When the LGPS solid electrolyte of the present invention is contained in the positive electrode layer 1 or the negative electrode layer 3, the LGPS solid electrolyte of the present invention is used in combination with a known positive electrode active material or negative electrode active material for a lithium ion secondary battery. The amount ratio of the LGPS solid electrolyte of the present invention contained in the positive electrode layer 1 or the negative electrode layer 3 is not particularly limited.

[0081] When the solid electrolyte layer 2 includes the LGPS solid electrolyte of the present invention, the solid electrolyte layer 2 may be composed of the LGPS solid electrolyte of the present invention alone, or may be combined with an oxide solid electrolyte (e.g., Li7La3Zr2O 12 ), sulfide-based solid electrolytes (such as Li2S-P2S5) and other hydrogenated coordination compound solid electrolytes (such as LiBH4, 3LiBH4-LiI), etc. can be used in appropriate combinations.

[0082] Although the all-solid-state battery is obtained by molding and stacking the above-mentioned layers, there are no particular restrictions on the molding method and stacking method of each layer.

[0083] For example, there are methods in which a solid electrolyte and / or electrode active material is dispersed in a solvent to form a slurry, the slurry is applied using a scraper or spin coating device, and then the slurry is rolled to form a film; a gas phase method in which vacuum evaporation, ion plating, sputtering, laser ablation, etc. are used for film formation and lamination; a pressure molding method in which powder is formed by hot pressing or cold pressing without heating, and the formed body is then laminated, etc.

[0084] The LGPS solid electrolyte of the present invention is relatively soft, so it is particularly preferred to prepare an all-solid-state battery by molding and stacking each layer by a pressure molding method. As a pressure molding method, there are hot pressing methods with heating and cold pressing methods without heating, but even cold pressing is sufficient to achieve molding.

[0085] It should be noted that the present invention includes a molded body obtained by pressure molding the LGPS-based solid electrolyte of the present invention. The molded body is suitable for use as an all-solid-state battery. In addition, the present invention also includes a method for manufacturing an all-solid-state battery including a step of pressure molding the LGPS-based solid electrolyte of the present invention.

[0086] Example

[0087] Hereinafter, the embodiments of the present invention will be described more specifically by way of examples, but the embodiments of the present invention are not limited to these examples.

[0088] (Example 1)

[0089] (Manufacture of β-Li3PS4)

[0090] In a glove box under an argon atmosphere, Li2S (manufactured by Sigma Aldrich, purity: 99.8%) and P2S5 (manufactured by Sigma Aldrich, purity: 99%) were weighed in a molar ratio of Li2S:P2S5 = 3:1. Then, tetrahydrofuran (manufactured by Wako Pure Chemical Industries, Ltd., ultra-dehydrated grade) was added thereto, and Li2S and P2S5 were added in sequence such that the concentration of (Li2S + P2S5) reached 10% by weight, and stirring was carried out at 200 rpm under an argon stream and reflux was carried out for 24 hours. The filter residue obtained by filtering it was vacuum-dried at a temperature of 150 °C for 4 hours, whereby a white powder of β-Li3PS4 was obtained.

[0091] (Impurity removal process)

[0092] To 0.5 g of the β-Li3PS4 powder obtained above, 10 mL of a tetrahydrofuran (THF) solution containing 1.75% by mass of sulfur (hereinafter also referred to as "S-THF solution") was added and stirred overnight. After filtering it, it was washed 3 times with 10 mL of THF, whereby a white powder of β-Li3PS4 from which impurities were removed was obtained.

[0093] (Micronization of β-Li3PS4)

[0094] To 1 g of the β-Li3PS4 powder obtained in the above process, 20 mL of acetonitrile was added and stirred for two days. After the obtained slurry was degassed at a temperature of 50 °C under reduced pressure to remove acetonitrile, the obtained powder was dried at a temperature of 180 °C under vacuum for 4 hours to remove the coordination solvent. The solvent removal was carried out under stirring. Thereafter, a micronized β-Li3PS4 powder was obtained.

[0095] (Manufacture of Li4SnS4)

[0096] In a glove box under an argon atmosphere, Li₂S (purity: 99.8%, manufactured by Sigma Aldrich) and SnS₂ (purity: 99.9%, manufactured by High Purity Chemical Research Institute Co., Ltd.) were weighed according to the stoichiometric ratio of Li₄SnS₄ and mixed in an agate mortar for 15 minutes. 1.0 g of the obtained mixture and 15 zirconia beads (outer diameter Φ: 10 mm) were placed in a 45 mL zirconia crucible and sealed. The zirconia crucible was fixed to a planetary ball mill (manufactured by Fritsch Japan Co., Ltd.) and ball-milled at 370 rpm for 4 hours. The obtained precursor was fired at a temperature of 450 °C for 8 hours to produce the solid electrolyte Li₄SnS₄.

[0097] Subsequently, in a glove box under an argon atmosphere, 1 g of Li₄SnS₄ obtained as described above was added to 20 mL of a good solvent, methanol (ultra-dehydrated grade, boiling point: 64 °C, manufactured by Fujifilm Wako Pure Chemical Corporation), and mixed at room temperature (25 °C) for 24 hours. It should be noted that Li₄SnS₄ gradually dissolved. The insoluble matter from the Li₄SnS₄ manufacturing process contained in the obtained solution was filtered using a membrane filter (polytetrafluoroethylene (PTFE), pore size: 1.0 μm) to obtain a good solvent solution in which Li₄SnS₄ was dissolved.

[0098] Subsequently, in a glove box under an argon atmosphere, 120 mL of ultra-dehydrated acetonitrile was put into a 300 mL flask, and an acetonitrile total reflux state was formed using a distillation apparatus. 20 mL of the good solvent solution prepared as described above was added dropwise to the acetonitrile. Methanol, which is the solvent of the added alcohol solution, volatilized after the addition, causing Li₄SnS₄ particles to precipitate in the acetonitrile. After the addition of the good solvent solution was completed, the moment when the top temperature reached 81 °C (boiling point of acetonitrile: 82 °C) was set as the distillation end point.

[0099] Under a vacuum state, the obtained powder was dried at a temperature of 180 °C for 4 hours to remove the coordinating solvent and obtain Li₄SnS₄ powder.

[0100] <Manufacture of Sn-type LGPS-based solid electrolyte>

[0101] In a glove box under an argon atmosphere, the micronized β-Li₃PS₄ and Li₄SnS₄ described above were weighed according to a molar ratio of β-Li₃PS₄∶Li₄SnS₄ = 2.7∶1 and mixed in an agate mortar. The mixture was fired at a temperature of 550 °C for 2 hours under an argon atmosphere to obtain a Sn-type LGPS-based solid electrolyte (Li 9.81 Sn 0.81 P 2.19 S 12)Crystallization.

[0102] (Example 2)

[0103] A Li3PS4 crystal was produced in the same manner as in Example 1, except that a tetrahydrofuran (THF) solution containing 0.5 mass% sulfur was used in the <impurity removal step> of Example 1. 9.81 Sn 0.81 P 2.19 S 12 Crystallization.

[0104] (Example 3)

[0105] A Li3PS4 crystal was produced in the same manner as in Example 1, except that a tetrahydrofuran (THF) solution containing 0.1 mass% sulfur was used in the <impurity removal step> of Example 1. 9.81 Sn 0.81 P 2.19 S 12 Crystallization.

[0106] (Comparative Example 1)

[0107] A Li3PS4 crystal was produced in the same manner as in Example 1, except that the <impurity removal step> was not performed in Example 1. 9.81 Sn 0.81 P 2.19 S 12 Crystallization.

[0108] (Comparative Example 2)

[0109] A Li3PS4 crystal was produced in the same manner as in Example 1, except that a tetrahydrofuran (THF) solution containing 0.05 mass% sulfur was used in the <impurity removal step> of Example 1. 9.81 Sn 0.81 P 2.19 S 12 Crystallization.

[0110] <X-ray diffraction measurement>

[0111] X-ray diffraction measurements were performed on the Li3PS4 powder obtained after the impurity removal step in each example and comparative example at room temperature (25 °C) in an Ar (argon) environment using "X'Pert3 Powder" manufactured by PANalytical B.V., with CuKα radiation: ). In Comparative Example 1, the impurity removal step was not performed. The measurement results of Examples 1 to 3 and Comparative Examples 1 to 2 are shown in Figure 3 . According to Figure 3 the results, it was found that Li2S was removed by the impurity removal step in Examples 1 to 3.

[0112] < 31P solid NMR measurement>

[0113] Under the following device conditions and measurement conditions, the Li3PS4 powders obtained after the impurity removal process in Examples 1 and 2 and the Li3PS4 powder obtained without the impurity removal process in Comparative Example 1 were subjected to 31 P solid NMR measurement. The results are shown in Figure 4 .

[0114] Furthermore, the filtrate residue obtained by filtration in the impurity removal process in Example 1 and the powder after filtrate concentration, as well as the Li3PS4 powder obtained without the impurity removal process in Comparative Example 1 were subjected to the following device conditions and measurement conditions. 31 P solid NMR measurement. The results are shown in Figure 5 .

[0115] [Device conditions]

[0116] Device: JEOL ECA-500 (manufactured by JEOL Ltd.)

[0117] Probe diameter: Φ3.2mm (corresponding to non-exposure measurement in the atmosphere)

[0118] Speed: 10kHz

[0119] Rotation gas: N2 (corresponding to non-atmospheric exposure measurement)

[0120] Sampling tube: sleeve zirconia

[0121] Sample processing was carried out in a glove box.

[0122] [Measurement conditions]

[0123] Relaxation time (T1) measurement: Saturation recovery method

[0124] Delay time: T1×5

[0125] Main body measurement: Single pulse

[0126] scanning: 31 P 32

[0127] Comparison: 31 P 85% H3PO4 aqueous solution

[0128] The measurement procedure is to measure the relaxation time, calculate T1, set the delay time to 5 times the T1 value, and perform a single pulse measurement. The obtained peaks are separated by the Lorentz function to obtain the integral value of each peak. Based on the obtained integral value, the content (mass %) of Li4P2S7 in Li3PS4 is calculated.

[0129] It should be noted that Li3PS4 has a peak in the range of 86.4±5ppm, and Li4P2S7 has a peak in the range of 89.0±5ppm.

[0130] <Lithium ion conductivity measurement>

[0131] 100 mg of the Sn-type LGPS solid electrolyte obtained as described above was used for uniaxial molding (480 MPa) to obtain a disk with a thickness of about 1 mm and a diameter of 8 mm. The lithium ion conductivity was calculated by AC impedance measurement using a four-terminal method using a lithium electrode ("SI1260IMPEDANCE / GAIN-PHASE ANALYZER" manufactured by Solartron) at intervals of 10°C in the temperature range from room temperature (25°C) to 100°C and to -20°C.

[0132] Specifically, the sample was placed in a thermostatic bath set at 25°C and kept for 30 minutes before the lithium ion conductivity was measured. The temperature of the thermostatic bath was then raised by 10°C at a time to 30°C to 90°C, and the ion conductivity was measured after the sample was kept at each temperature for 25 minutes. After the measurement at 90°C, the temperature of the thermostatic bath was lowered by 10°C at a time to 80°C to 30°C, and the sample was kept at each temperature for 40 minutes before the lithium ion conductivity was measured. Next, the sample was kept in a thermostatic bath set at 25°C for 40 minutes before the lithium ion conductivity was measured. Next, the temperature of the thermostatic bath was lowered by 10°C at a time to 20°C to -30°C, and the sample was kept at each temperature for 40 minutes before the lithium ion conductivity was measured. The measurement frequency range was set to 0.1Hz to 1MHz, and the amplitude was set to 50mV. The measurement results of lithium ion conductivity during temperature reduction are shown in Figure 6 .

[0133] AC impedance method

[0134] [Battery Cell Composition]

[0135] Evaluation battery cell: Constrained cell / Electrochemical cell improved version SSBC-2 (SUS-303)

[0136] Electrode: SUS electrode / primary pressure 120MPa, secondary pressure 480MPa

[0137] [Measurement conditions]

[0138] Analytical device: Solartron SI 1260

[0139] Measurement control software: Z Plot

[0140] Display and analysis software: Z View

[0141] Measuring method: 4-terminal method

[0142] Voltage control: DC 0V AC 50mV

[0143] Frequency: 0.1Hz~1MHz

[0144] [Table 1]

[0145] Table 1. Synthesis conditions and ionic conductivity of each sample

[0146]

[0147] *The intensity ratio of the diffraction line of Li3PS4 and the diffraction line of Li2S obtained by X-ray diffraction (XRD) was used for quantification by the RIR method. Li2S used the 111 diffraction line with the strongest peak, and Li3PS4 also used the 221 diffraction line with the strongest peak. In the RIR method, it is based on the ratio of the integrated intensity within the range of 26.7°±0.50° of 2θ in X-ray diffraction to the integrated intensity within the range of 29.2°±0.50° of 2θ. It should be noted that Examples 1 to 3 could not be calculated because the Li2S peak was not detected.

[0148] ** Used by 31 The integral value of the peak of Li3PS4 and the peak of Li4P2S7 obtained by P-NMR was calculated according to the following formula.

[0149] (Integral value of Li4P2S7) / (Integral value of Li3PS4)×100

[0150] The sulfur concentration of the S-THF solution is 1.75 mass % which is the maximum (saturated state). According to the results in Table 1, the recovery amount of Li3PS4 varies with the sulfur concentration. It is believed that this is because the sulfur concentration in Example 1 is high, so that Li3PS4 is also dissolved, and the recovery rate falls instead.

[0151] It should be noted that the recovery rate of Li3PS4 after purification of the S-THF solution in Examples 1 to 3 and Comparative Example 2 was calculated based on (mass g of β-Li3PS4 powder after drying at 150°C after purification operation) / (mass g of powder before purification operation)×100.

[0152] Figure 4 The amount of Li4P2S7 contained in the Li3PS4 powder obtained after the impurity removal process in Examples 1 and 2 is compared with the amount of Li4P2S7 contained in the Li3PS4 powder obtained without the impurity removal process in Comparative Example 1. 31 P solid NMR diagram. Figure 4The results show that the impurity Li4P2S7 can be quantitatively removed regardless of the sulfur concentration in the S-THF solution.

[0153] Figure 5 To show the filtering effect of S-THF solution 31 P solid NMR diagram. Figure 5 The results show that the impurity Li4P2S7 is dissolved in the filtrate, while Li3PS4 is also dissolved. When the sulfur concentration in the S-THF solution is high, Li3PS4 will also be dissolved, and the recovery rate of Li3PS4 will decrease. However, by reducing the sulfur concentration in the S-THF solution, the dissolution ratio of Li3PS4 will be reduced, and the recovery rate of Li3PS4 will be improved.

[0154] Explanation of symbols

[0155] 1: positive electrode layer;

[0156] 2: solid electrolyte layer;

[0157] 3: negative electrode layer;

[0158] 10: All-solid-state battery.

Claims

1. A method for producing a LGPS solid electrolyte, characterized in that: include: A process for preparing Li3PS4 powder, or at least preparing Li3PS4 powder from Li2S and P2S5; and A step of adding a solvent containing 0.1 to 1.75 mass % of sulfur in an organic solvent to the Li3PS4 powder to remove impurities in the Li3PS4 powder.

2. The manufacturing method according to claim 1, characterized in that: The impurities include unreacted Li2S or intermediate Li4P2S7.

3. The manufacturing method according to claim 1 or 2, characterized in that: The organic solvent is at least one selected from tetrahydrofuran, acetonitrile, ethyl acetate and methyl acetate.

4. The manufacturing method according to any one of claims 1 to 3, characterized in that: The process of removing the impurities includes stirring the Li3PS4 powder and the solvent and filtering the obtained mixture.

5. The manufacturing method according to claim 4, characterized in that: The process of removing the impurities also includes the step of vacuum drying the filter residue after filtering the mixture.

6. The manufacturing method according to any one of claims 1 to 5, characterized in that: The Li3PS4 is β-Li3PS4.

7. The manufacturing method according to any one of claims 1 to 6, characterized in that: The invention comprises the process of manufacturing a Sn-type LGPS solid electrolyte by sintering a mixture obtained by using Li3PS4 powder from which the impurities are removed and Li4SnS4 prepared from Li2S and SnS2 in an inert gas environment.

8. The manufacturing method according to any one of claims 1 to 7, characterized in that: The LGPS solid electrolyte has an X-ray diffraction (CuKα: ), there are peaks at least at the positions of 2θ=19.90°±0.50°, 20.20°±0.50°, 26.70°±0.50° and 29.20°±0.50°.

9. The manufacturing method according to any one of claims 1 to 8, characterized in that: The LGPS-based solid electrolyte contains the following crystal structure as a main body, which has an octahedron O composed of Li element and S element, a tetrahedron T1 composed of one or more elements selected from P and Sn and the S element, and a tetrahedron T2 composed of the P element and the S element, and the tetrahedron T1 shares edges with the octahedron O and the tetrahedron T2 shares vertices with the octahedron O.

10. A method for manufacturing an all-solid-state battery, characterized in that: The method comprises the step of pressure-molding the LGPS solid electrolyte obtained by the production method according to any one of claims 1 to 9.