Three-dimensional layered hydroxyapatite / collagenous fiber as well as preparation method and application thereof

The three-dimensional structure is formed in the fibers through gas foaming technology, which solves the precipitation and agglomeration problems in HAp fibers, achieves uniform dispersion and biocompatibility of HAp fibers, and improves the plasticity and biocompatibility of bone repair materials.

CN119015503APending Publication Date: 2024-11-26HANGZHOU ZHONGKE PHYSICOCHEMICAL BIOMEDICAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411146598.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing HAp fibers are prone to precipitation and agglomeration during spinning, resulting in uneven distribution and difficulty in preparing three-dimensional bone repair materials with excellent plasticity properties. The transformation of two-dimensional fibers into three-dimensional structures and poor results.

Method used

Using gas foaming technology, crosslinked fibers are soaked in aqueous phosphoric acid solution to generate carbon dioxide, and the expanded fibers are in a three-dimensional structure. At the same time, hydroxyapatite nanoparticles grow along the fibers to avoid accumulation and agglomeration, and immerse in collagen solution to improve porosity. and biocompatibility.

Benefits of technology

The uniform dispersion of HAp in the fiber and the formation of three-dimensional structures are achieved, providing better cell-to-cell interactions and bone repair performance, with excellent biocompatibility and degradability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119015503A_ABST
    Figure CN119015503A_ABST
Patent Text Reader

Abstract

The invention provides a three-dimensional layered hydroxyapatite / collagenous fiber as well as a preparation method and application thereof, and relates to the technical field of medical materials. Firstly, coaxial electrostatic spinning is carried out, a core layer is composed of high polymer materials and metal hydroxides, and the high polymer materials are gelatin, chitosan and polyvinyl alcohol; the shell layer is composed of polyvinylpyrrolidone and a foaming agent, then gas foaming is utilized, coaxial fibers are soaked in a phosphoric acid aqueous solution, carbon dioxide is generated to expand the fibers from two-dimensional fibers to three-dimensional fibers, meanwhile, hydroxyapatite nano-particles can continuously grow along the fibers, then the fibers are soaked in a collagen solution, and finally freeze drying is conducted to obtain the hydroxyapatite / collagen composite material. The three-dimensional layered hydroxyapatite / collagen fiber is obtained. The prepared three-dimensional layered hydroxyapatite / collagenous fiber is soft in structure, can provide filling for bone defect parts, has good biocompatibility, and has great potential in clinical application as a bone repair filling material in the future.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of medical materials, and in particular to a three-dimensional layered hydroxyapatite / collagen fiber and a preparation method and application thereof. Background Art

[0002] Bone tissue engineering is a promising therapeutic strategy for bone repair and regeneration. It aims to reconstruct bone tissue with the help of tissue engineering components - cells, growth stimulation signals and scaffolds. Tissue scaffolds provide a microenvironment for cell attachment, proliferation, differentiation and new tissue formation, and should be porous to facilitate the effective delivery of nutrients and oxygen, and be biocompatible and degradable. Scaffolds should also mimic the composition, structure, morphology and bioactivity of bone extracellular matrix (ECM) to regulate cell behavior. ECM is a typical organic-inorganic nanocomposite material, mainly composed of collagen fibers containing embedded hydroxyapatite (HAp) nanoparticles. About 70% of natural bone mineral is composed of HAp. HAp-based ceramic materials have been widely used in clinical practice due to their significant osteoconductivity and ability to serve as precursors for bone calcium phosphate formation.

[0003] However, these ceramic materials are brittle, have poor compressibility and are difficult to shape during surgery, making it difficult for them to play their role in implants that need to be soft and plastic.

[0004] Fibrous scaffolds have attracted extensive attention due to their structure similar to that of bone matrix. HAp-doped electrostatic coaxial fibers are considered to be the simplest and most promising materials for bone tissue engineering. Although HAp-doped fibers are soft and plastic relative to ceramic materials, HAp is prone to precipitation during the spinning process, and HAp is unevenly distributed in the fibers and easily agglomerated, which affects its effect. In addition, electrospun fibers are limited to two-dimensional (2D) membranes. The three-dimensionality and higher porosity of tissue scaffolds can provide a better environment for cell-cell interactions, cell migration, and cell morphogenesis. In order to overcome this shortcoming of electrospinning, some methods have been developed, such as multilayer electrospinning, post-treatment of two-dimensional membranes, and the use of three-dimensional templates or liquid collectors. However, the three-dimensional fiber structures prepared by these methods are relatively loose, and the preparation process is complicated.

[0005] Therefore, how to solve the problem of HAp agglomeration in fibers and transform two-dimensional fibers into three-dimensional fibers using a simple method to obtain bone repair materials with excellent plasticity remains a great challenge. Summary of the invention

[0006] The purpose of the present invention is to provide a three-dimensional layered hydroxyapatite / collagen fiber and a preparation method and application thereof. The preparation method of the present invention is simple, and the hydroxyapatite is evenly dispersed in the fiber.

[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0008] The present invention provides a method for preparing three-dimensional layered hydroxyapatite / collagen fibers, comprising the following steps: mixing a gelatin solution, a chitosan solution, a polyvinyl alcohol solution and a metal hydroxide to obtain a core layer spinning precursor solution;

[0009] Dispersing a foaming agent into a polyvinyl pyrrolidone solution to obtain a shell spinning precursor solution; the foaming agent is a nano carbonate and / or a nano bicarbonate;

[0010] Coaxially electrospinning the core layer spinning precursor solution and the shell layer spinning precursor solution to obtain coaxial fibers;

[0011] cross-linking the coaxial fibers with formaldehyde vapor to obtain cross-linked fibers;

[0012] The cross-linked fiber is immersed in a phosphoric acid aqueous solution, and the foaming agent in the shell layer of the cross-linked fiber reacts with the phosphoric acid to generate gas to expand the fiber into a three-dimensional structure. After the expansion is complete, the reaction is continued to react so that the metal hydroxide in the core layer reacts with the phosphoric acid to generate hydroxyapatite, and the fiber after the reaction is taken out and freeze-dried to obtain a three-dimensional layered hydroxyapatite fiber;

[0013] The three-dimensional layered hydroxyapatite fibers are immersed in a collagen solution, taken out, and freeze-dried to obtain the three-dimensional layered hydroxyapatite / collagen fibers.

[0014] Preferably, the mass concentration of the gelatin solution is 5-20%;

[0015] The mass concentration of the chitosan solution is 1-10%;

[0016] The mass concentration of the polyvinyl alcohol solution is 1 to 15%;

[0017] The volume ratio of the gelatin solution, the chitosan solution and the polyvinyl alcohol solution is 1:0.5-1:0.1-1.

[0018] Preferably, the metal hydroxide includes one or more of calcium hydroxide, strontium hydroxide and magnesium hydroxide; the mass content of the metal hydroxide in the core layer spinning precursor solution is 1-10%.

[0019] Preferably, the mass concentration of the polyvinyl pyrrolidone solution is 5-10%.

[0020] Preferably, the nano carbonate includes one or more of nano sodium carbonate, nano magnesium carbonate, nano calcium carbonate and nano strontium carbonate; the nano bicarbonate includes nano sodium bicarbonate; and the mass content of the foaming agent in the shell spinning precursor solution is 1-10%.

[0021] Preferably, the conditions for the coaxial electrospinning include: a spinning voltage of 15 to 30 kV, an injection rate of a core layer spinning precursor solution of 0.3 to 2 mL / h, and an injection rate of a shell layer spinning precursor solution of 0.5 to 2 mL / h.

[0022] Preferably, the mass concentration of the phosphoric acid aqueous solution is 0.5-5%.

[0023] Preferably, the temperature of the continued reaction is 40-70° C. and the time is 1-3 hours.

[0024] The present invention provides three-dimensional layered hydroxyapatite / collagen fibers prepared by the preparation method described in the above scheme, including three-dimensional layered hydroxyapatite fibers and collagen wrapped on the surface of the three-dimensional layered hydroxyapatite fibers; the three-dimensional layered hydroxyapatite fibers include a core layer and a shell layer, the core layer is a gelatin-chitosan-polyvinyl alcohol crosslinked product and hydroxyapatite; the shell layer is polyvinyl pyrrolidone.

[0025] The present invention provides the use of the three-dimensional layered hydroxyapatite / collagen fibers described in the above scheme in preparing bone repair filling materials.

[0026] The invention provides a method for preparing three-dimensional layered hydroxyapatite / collagen fibers, comprising the following steps: mixing a gelatin solution, a chitosan solution, a polyvinyl alcohol solution and a metal hydroxide to obtain a core layer spinning precursor solution; dispersing a foaming agent in a polyvinyl pyrrolidone solution to obtain a shell layer spinning precursor solution; the foaming agent is nano carbonate and / or nano bicarbonate; coaxially electrospinning the core layer spinning precursor solution and the shell layer spinning precursor solution to obtain coaxial fibers; cross-linking the coaxial fibers with formaldehyde vapor to obtain cross-linked fibers; immersing the cross-linked fibers in a phosphoric acid aqueous solution, wherein the foaming agent in the shell layer of the cross-linked fibers reacts with phosphoric acid to generate gas to expand the fibers into a three-dimensional structure, and after the expansion is complete, continuing the reaction to react the metal hydroxide in the core layer with phosphoric acid to generate hydroxyapatite, taking out the reacted fibers, freeze-drying them, and obtaining three-dimensional layered hydroxyapatite fibers; immersing the three-dimensional layered hydroxyapatite fibers in a collagen solution, taking them out, and freeze-drying them to obtain the three-dimensional layered hydroxyapatite / collagen fibers.

[0027] The present invention utilizes gas foaming technology to immerse the cross-linked fibers in a phosphoric acid aqueous solution, generating carbon dioxide to expand the fibers from two-dimensional to three-dimensional fibers, while hydroxyapatite nanoparticles will continue to grow along the fibers, avoiding the accumulation and agglomeration of hydroxyapatite. The present invention fills collagen in the pores of the three-dimensional fibers, can mimic the main components of bone materials, and has excellent biocompatibility, degradability, and bone repair performance.

[0028] The preparation method provided by the present invention is simple, and three-dimensional layered hydroxyapatite / collagen fibers with controllable thickness and porosity can be prepared. Specifically, the porosity of the three-dimensional layered hydroxyapatite / collagen fibers can be controlled by controlling the amount of the foaming agent, and the thickness of the core layer and the shell layer can be controlled by controlling the amount of the core layer spinning precursor solution and the shell layer spinning precursor solution. The three-dimensional fiber prepared by the present invention has a highly continuous layered fiber structure, which is different from the previously reported layered structure formed by stacking. The three-dimensionality and higher porosity of the fiber of the present invention can provide a better environment for cell-to-cell interaction, cell migration and cell morphogenesis. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The figure is a flow chart of the preparation of three-dimensional layered hydroxyapatite / collagen fibers of the present invention;

[0030] Figure 2 The shape diagrams of the fibers of Example 1, Example 2 and Comparative Example 1;

[0031] Figure 3 is a scanning electron microscope image of the cross-section of the fiber of Example 2;

[0032] Figure 4 This is a transmission electron microscope image of the fiber of Example 2;

[0033] Figure 5 is the XRD pattern of the fiber of Example 2;

[0034] Figure 6 The cytotoxicity test results of Example 2 and Comparative Examples 1-2 are shown;

[0035] Figure 7 The cell morphology photos of Example 2 and Comparative Examples 1-2;

[0036] Figure 8 The ALP staining results of Example 2 and Comparative Example 2;

[0037] Fig. 9 The ARS staining results of Example 2 and Comparative Example 2 are shown. DETAILED DESCRIPTION

[0038] like Figure 1 As shown, the present invention provides a method for preparing three-dimensional layered hydroxyapatite / collagen fibers, comprising the following steps: mixing a gelatin solution, a chitosan solution, a polyvinyl alcohol solution and a metal hydroxide to obtain a core layer spinning precursor solution;

[0039] Dispersing a foaming agent into a polyvinyl pyrrolidone solution to obtain a shell spinning precursor solution; the foaming agent is a nano carbonate and / or a nano bicarbonate;

[0040] Coaxially electrospinning the core layer spinning precursor solution and the shell layer spinning precursor solution to obtain coaxial fibers;

[0041] cross-linking the coaxial fibers with formaldehyde vapor to obtain cross-linked fibers;

[0042] The cross-linked fiber is immersed in a phosphoric acid aqueous solution, and the foaming agent in the shell layer of the cross-linked fiber reacts with the phosphoric acid to generate gas to expand the fiber into a three-dimensional structure. After the expansion is complete, the reaction is continued to react so that the metal hydroxide in the core layer reacts with the phosphoric acid to generate hydroxyapatite, and the fiber after the reaction is taken out and freeze-dried to obtain a three-dimensional layered hydroxyapatite fiber;

[0043] The three-dimensional layered hydroxyapatite fibers are immersed in a collagen solution, taken out, and freeze-dried to obtain the three-dimensional layered hydroxyapatite / collagen fibers.

[0044] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known in the art.

[0045] The invention mixes gelatin solution, chitosan solution, polyvinyl alcohol solution and metal hydroxide to obtain a core layer spinning precursor solution.

[0046] In the present invention, the preparation of the gelatin solution preferably includes: mixing gelatin and water, swelling for 30 minutes, heating at 50°C to dissolve, and obtaining the gelatin solution. In the present invention, the mass concentration of the gelatin solution is preferably 5-20%, more preferably 10-15%.

[0047] In the present invention, the chitosan solution is preferably obtained by dissolving chitosan in acetic acid solution; the mass concentration of the acetic acid solution is preferably 1-5%; the mass concentration of the chitosan solution is preferably 1-10%, more preferably 3-7%.

[0048] In the present invention, the polyvinyl alcohol solution is preferably obtained by dissolving polyvinyl alcohol in water; the dissolution temperature is preferably 80° C. The mass concentration of the polyvinyl alcohol solution is preferably 1 to 15%, more preferably 5 to 10%.

[0049] In the present invention, the volume ratio of the gelatin solution, the chitosan solution and the polyvinyl alcohol solution is preferably 1:0.5 to 1:0.1 to 1, more preferably 1:0.8 to 1:0.4 to 0.6, and further preferably 1:1:0.5.

[0050] In the present invention, the metal hydroxide preferably includes one or more of calcium hydroxide, strontium hydroxide and magnesium hydroxide, more preferably calcium hydroxide; the mass content of the metal hydroxide in the core layer spinning precursor solution is preferably 1-10%, more preferably 4-7%.

[0051] In the present invention, the mixing of gelatin solution, chitosan solution, polyvinyl alcohol solution and metal hydroxide preferably includes: firstly mixing gelatin solution, chitosan solution and polyvinyl alcohol solution, keeping warm at 40-60°C, then adding metal hydroxide to the obtained mixed solution, ultrasonically dispersing, and obtaining a core layer spinning precursor solution.

[0052] The invention disperses the foaming agent into the polyvinyl pyrrolidone solution to obtain the shell spinning precursor solution.

[0053] In the present invention, the foaming agent is nano carbonate and / or nano bicarbonate; the nano carbonate preferably includes one or more of nano sodium carbonate, nano magnesium carbonate, nano calcium carbonate and nano strontium carbonate; the nano bicarbonate preferably includes nano sodium bicarbonate; the mass content of the foaming agent in the shell spinning precursor solution is preferably 1-10%, more preferably 3-7%.

[0054] In the present invention, the polyvinyl pyrrolidone solution is preferably obtained by dissolving polyvinyl pyrrolidone in water; the mass concentration of the polyvinyl pyrrolidone solution is preferably 5-10%, more preferably 6-9%.

[0055] The present invention has no special requirements on the dispersion method of the foaming agent, and it only needs to be able to evenly disperse the foaming agent into the polyvinyl pyrrolidone solution, such as ultrasonic dispersion.

[0056] After obtaining the core layer spinning precursor solution and the shell layer spinning precursor solution, the present invention performs coaxial electrostatic spinning on the core layer spinning precursor solution and the shell layer spinning precursor solution to obtain coaxial fibers.

[0057] In the present invention, the conditions of the coaxial electrospinning include: the spinning voltage is preferably 15-30 kV, more preferably 20-25 kV; the core layer spinning precursor injection rate is preferably 0.3-2 mL / h, more preferably 0.5-1.5 mL / h; the shell layer spinning precursor injection rate is preferably 0.5-2 mL / h, more preferably 1-1.5 mL / h. In the present invention, the diameter of the coaxial fiber is preferably 800 nm-5 μm, the core layer diameter is preferably 400 nm-3 μm; the thickness of the fiber membrane formed by the coaxial electrospinning is preferably 1-5 mm.

[0058] In the present invention, the coaxial fibers obtained after coaxial electrospinning exist on the receiver in the form of fiber cloth. The present invention preferably cuts the fiber cloth and then performs a series of subsequent steps such as cross-linking.

[0059] After obtaining the coaxial fibers, the present invention cross-links the coaxial fibers with formaldehyde vapor to obtain cross-linked fibers.

[0060] In the present invention, the formaldehyde vapor is preferably generated from a formaldehyde aqueous solution, the mass of formaldehyde in the formaldehyde aqueous solution is preferably 0.1-0.5% of the mass of water, more preferably 0.2-0.4% (hereinafter referred to as formaldehyde density). The present invention utilizes formaldehyde vapor to promote crosslinking of gelatin, chitosan and polyvinyl alcohol.

[0061] After obtaining the cross-linked fibers, the present invention immerses the cross-linked fibers in a phosphoric acid aqueous solution.

[0062] In the present invention, the mass concentration of the phosphoric acid aqueous solution is preferably 0.5-5%, more preferably 1-4%. The present invention has no special requirements for the amount of the phosphoric acid aqueous solution, as long as it can immerse the cross-linked fibers. After the cross-linked fibers are placed in the phosphoric acid aqueous solution, the foaming agent in the cross-linked fiber shell reacts with the phosphoric acid to generate gas, causing the fibers to expand into a three-dimensional structure.

[0063] After the expansion is complete, the present invention continues the reaction so that the metal hydroxide in the core layer reacts with phosphoric acid to generate hydroxyapatite.

[0064] In the present invention, the temperature of the continued reaction is preferably 40 to 70° C., more preferably 50 to 60° C.; the time of the continued reaction is preferably 1 to 3 hours, more preferably 1.5 to 2.5 hours.

[0065] After the reaction is completed, the present invention takes out the reacted fibers and freeze-dries them to obtain three-dimensional layered hydroxyapatite fibers.

[0066] The present invention utilizes gas foaming technology to immerse the cross-linked fibers in a phosphoric acid aqueous solution to generate carbon dioxide to expand the fibers from two dimensions to three dimensions. At the same time, hydroxyapatite nanoparticles will continue to grow along the fibers, thereby avoiding the accumulation and agglomeration of hydroxyapatite.

[0067] After obtaining the three-dimensional layered hydroxyapatite fibers, the present invention immerses the three-dimensional layered hydroxyapatite fibers in a collagen solution, takes them out, and freeze-dries them to obtain the three-dimensional layered hydroxyapatite / collagen fibers.

[0068] In the present invention, the mass concentration of the collagen solution is preferably 5-50%, more preferably 10-40%, and further preferably 20-30%. In the present invention, the immersion time is preferably 0.5-1h. The present invention can mimic the main components of bone materials by immersing collagen in the pores, and has excellent biocompatibility, degradability and bone repair performance.

[0069] The present invention provides three-dimensional layered hydroxyapatite / collagen fibers prepared by the preparation method described in the above scheme, including three-dimensional layered hydroxyapatite fibers and collagen wrapped on the surface of the three-dimensional layered hydroxyapatite fibers; the three-dimensional layered hydroxyapatite fibers include a core layer and a shell layer, the core layer is a gelatin-chitosan-polyvinyl alcohol crosslinked product and hydroxyapatite; the shell layer is polyvinyl pyrrolidone.

[0070] The three-dimensional layered hydroxyapatite / collagen fiber prepared by the invention has good biocompatibility and can promote the extracellular mineralization of osteoblasts.

[0071] The present invention provides the use of the three-dimensional layered hydroxyapatite / collagen fibers described in the above scheme in preparing bone repair filling materials.

[0072] The three-dimensional layered hydroxyapatite / collagen fiber structure prepared by the present invention is soft, can provide filling for bone defect sites, and has good biocompatibility, and has great potential in clinical applications as bone repair filling materials in the future.

[0073] The three-dimensional layered hydroxyapatite / collagen fibers provided by the present invention and their preparation method and application are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0074] Example 1

[0075] (1) Add gelatin into deionized water, swell for 30 minutes, and heat at 50°C to dissolve to obtain a 15% gelatin solution.

[0076] (2) Add chitosan into 5% acetic acid solution and stir to dissolve to obtain a 5% chitosan solution.

[0077] (3) Add polyvinyl alcohol (PVA) into deionized water and stir to dissolve at 80° C. to obtain a 10% polyvinyl alcohol solution.

[0078] (4) The solutions obtained in steps (1), (2) and (3) are mixed uniformly in a certain volume ratio and kept warm at 50° C. The volume ratio of the gelatin solution, the chitosan solution and the polyvinyl alcohol solution is 1:1:0.5.

[0079] (5) adding calcium hydroxide to the mixed solution of step (4), and dispersing by ultrasonic to obtain a core layer spinning precursor solution, wherein the mass fraction of calcium hydroxide is 5%.

[0080] (6) Add polyvinyl pyrrolidone (PVP) into deionized water and stir to dissolve to obtain a 10% PVP solution.

[0081] (7) Adding nano sodium carbonate to the PVP solution obtained in step (6), and dispersing by ultrasonication to obtain a shell spinning precursor solution, wherein the concentration of nano sodium carbonate is 3%.

[0082] (8) The core layer spinning precursor solution obtained in step (5) and the shell layer spinning precursor solution obtained in step (7) are respectively added into syringes for coaxial electrospinning, and the obtained fiber membrane has a thickness of 1 mm. Then it is cut into 5 cm×5 cm squares. The spinning voltage is 30 kV, the core layer syringe speed is 1 mL / h, and the shell layer syringe speed is 1 mL / h.

[0083] (9) The coaxial fibers obtained in step (8) are cross-linked with formaldehyde vapor, wherein the formaldehyde density is 0.5%.

[0084] (10) The cross-linked fibers obtained in step (9) are immersed in a 3% phosphoric acid aqueous solution, and after the fibers are fully expanded, the reaction is continued at 60° C. for 2 h, and the fibers are taken out and freeze-dried.

[0085] (11) Soaking the fibers obtained in step (10) in a 20% collagen solution, taking them out and freeze-drying them to obtain three-dimensional layered hydroxyapatite / collagen fibers in the shape of Figure 2 shown.

[0086] Example 2

[0087] The only difference from Example 1 is that the concentration of nano sodium carbonate in step (7) is replaced by "7%" from "3%". The specific steps are as follows:

[0088] (1) Add gelatin into deionized water, swell for 30 minutes, and heat at 50°C to dissolve to obtain a 15% gelatin solution.

[0089] (2) Add chitosan into 5% acetic acid solution and stir to dissolve to obtain a 5% chitosan solution.

[0090] (3) Add polyvinyl alcohol (PVA) into deionized water and stir to dissolve at 80° C. to obtain a 10% polyvinyl alcohol solution.

[0091] (4) The solutions obtained in steps (1), (2) and (3) are mixed uniformly in a certain volume ratio and kept warm at 50° C. The volume ratio of the gelatin solution, the chitosan solution and the polyvinyl alcohol solution is 1:1:0.5.

[0092] (5) adding calcium hydroxide to the mixed solution of step (4), and dispersing by ultrasonic to obtain a core layer spinning precursor solution, wherein the mass fraction of calcium hydroxide is 5%.

[0093] (6) Add polyvinyl pyrrolidone (PVP) into deionized water and stir to dissolve to obtain a 10% PVP solution.

[0094] (7) Adding nano sodium carbonate to the PVP solution obtained in step (6), and dispersing by ultrasonication to obtain a shell spinning precursor solution, wherein the concentration of nano sodium carbonate is 7%.

[0095] (8) The core layer spinning precursor solution obtained in step (5) and the shell layer spinning precursor solution obtained in step (7) are respectively added into syringes for coaxial electrospinning, and the obtained fiber membrane has a thickness of 1 mm. Then it is cut into 5 cm×5 cm squares. The spinning voltage is 30 kV, the core layer syringe speed is 1 mL / h, and the shell layer syringe speed is 1 mL / h.

[0096] (9) The coaxial fibers obtained in step (8) are cross-linked with formaldehyde vapor, wherein the formaldehyde density is 0.5%.

[0097] (10) The cross-linked fibers obtained in step (9) are immersed in a 3% phosphoric acid aqueous solution, and after the fibers are fully expanded, the reaction is continued at 60° C. for 2 h, and the fibers are taken out and freeze-dried.

[0098] (11) Soaking the fibers obtained in step (10) in a 20% collagen solution and then freeze-drying them to obtain three-dimensional layered hydroxyapatite / collagen fibers in the shape of Figure 2 shown.

[0099] Comparative Example 1

[0100] The difference from Example 1 is that nano sodium carbonate is omitted, and the specific steps are as follows:

[0101] (1) Add gelatin into deionized water, swell for 30 minutes, and heat at 50°C to dissolve to obtain a 15% gelatin solution.

[0102] (2) Add chitosan into 5% acetic acid solution and stir to dissolve to obtain a 5% chitosan solution.

[0103] (3) Add polyvinyl alcohol (PVA) into deionized water and stir to dissolve at 80° C. to obtain a 10% polyvinyl alcohol solution.

[0104] (4) The solutions obtained in steps (1), (2) and (3) are mixed uniformly in a certain volume ratio and kept warm at 50° C. The volume ratio of the gelatin solution, the chitosan solution and the polyvinyl alcohol solution is 1:1:0.5.

[0105] (5) adding calcium hydroxide to the mixed solution of step (4), and dispersing by ultrasonic to obtain a core layer spinning precursor solution, wherein the mass fraction of calcium hydroxide is 5%.

[0106] (6) Add polyvinyl pyrrolidone (PVP) into deionized water and stir to dissolve to obtain a 10% PVP solution.

[0107] (7) The core layer spinning precursor solution obtained in step (5) and the shell layer spinning precursor solution obtained in step (6) are respectively added into syringes for coaxial electrospinning, and the spinning thickness is 1 mm. Then, the spinning is cut into 5 cm×5 cm squares. The spinning voltage is 30 kV, the core layer syringe speed is 1 mL / h, and the shell layer syringe speed is 1 mL / h.

[0108] (8) The coaxial fibers obtained in step (7) are cross-linked with formaldehyde vapor, wherein the formaldehyde density is 0.5%.

[0109] (9) Immerse the cross-linked fibers obtained in step (8) in a phosphoric acid aqueous solution, wait for the fibers to swell completely, continue to react at 60° C. for 2 h, take out, and freeze-dry.

[0110] (10) Soaking the fibers obtained in step (9) in a 20% collagen solution, taking them out, and then freeze-drying them to obtain hydroxyapatite / collagen fibers in the shape of Figure 2 Obviously, the hydroxyapatite / collagen fibers obtained in Comparative Example 1 are two-dimensional flat and cannot expand.

[0111] Comparative Example 2

[0112] The difference from Example 2 is that calcium hydroxide is omitted and hydroxyapatite is not formed. The specific steps are as follows:

[0113] (1) Add gelatin into deionized water, swell for 30 minutes, and heat at 50°C to dissolve to obtain a 15% gelatin solution.

[0114] (2) Add chitosan into 5% acetic acid solution and stir to dissolve to obtain a 5% chitosan solution.

[0115] (3) Add polyvinyl alcohol (PVA) into deionized water and stir to dissolve at 80° C. to obtain a 10% polyvinyl alcohol solution.

[0116] (4) The solutions obtained in steps (1), (2) and (3) are mixed uniformly in a certain volume ratio, kept warm at 50° C., wherein the volume ratio of the gelatin solution, the chitosan solution and the polyvinyl alcohol solution is 1:1:0.5, to obtain a core layer spinning precursor solution.

[0117] (5) Add polyvinyl pyrrolidone (PVP) into deionized water, stir and dissolve, and obtain a 10% PVP spinning solution.

[0118] (6) Adding nano sodium carbonate to the PVP solution obtained in step (5), and dispersing by ultrasonication to obtain a shell spinning precursor solution, wherein the concentration of nano sodium carbonate is 7%.

[0119] (7) The core layer spinning precursor solution obtained in step (4) and the shell layer spinning precursor solution obtained in step (6) are respectively added into syringes for coaxial electrospinning, and the spinning thickness is 1 mm. Then, the spinning is cut into 5 cm×5 cm squares. The spinning voltage is 30 kV, the core layer syringe speed is 1 mL / h, and the shell layer syringe speed is 1 mL / h.

[0120] (8) The fiber obtained in step (7) is cross-linked with formaldehyde vapor, wherein the formaldehyde density is 0.5%.

[0121] (9) Immerse the fiber obtained in step (8) in a phosphoric acid aqueous solution, wait for the fiber to swell completely, continue to react at 60° C. for 2 h, take out, and freeze-dry.

[0122] (10) Soak the fibers obtained in step (9) in a 20% collagen solution, take them out and freeze-dry them.

[0123] Structural characterization and performance testing

[0124] (1) Structural characterization

[0125] The hydroxyapatite / collagen fibers prepared in Example 2 were observed by scanning electron microscopy. Figure 3 As shown, the diameter is about 2 microns and the outer layer is uniform. The hydroxyapatite / collagen fibers prepared in Example 2 were further observed by transmission electron microscopy and characterized by XRD. Figure 4 and Figure 5 . Figure 4 This indicates that the fibers contain nanoparticles and are evenly distributed on the fibers. Figure 5 This indicates that the nanoparticles are hydroxyapatite.

[0126] (2) Cytotoxicity assay

[0127] Preparation of extract: The extract was prepared according to the national standard GB / T 16886.12-2005. The samples of Example 2, Comparative Example 1 and Comparative Example 2 were added to the cell culture medium at an extraction ratio of 0.2 g / mL, and then cultured in a 37°C incubator for 24 hours. The obtained extract was refrigerated at 4°C for later use. The extract was added to a 96-well plate, 2,000 cells were inoculated in each well, 10% fetal bovine serum (FBS) was added to each well, and cultured at 37°C in 5% CO2 for 7 days. Using Incucyte TM The Zoom system observed the effects of the extract on L929 cells in real time. Figure 6 and Figure 7 As shown, Figure 6 The cytotoxicity test results of Example 2 and Comparative Examples 1-2 indicate the survival rates of L929 cells cultured in the extract for 1, 3 and 6 days. Figure 7The cell morphology photos of Example 2 and Comparative Examples 1-2 are specifically the cell morphology of L929 cells cultured in the extract for 1, 3 and 6 days.

[0128] from Figures 6-7 It can be seen that the relative cell survival rate of the samples prepared in Example 2 and Comparative Examples 1-2 is comparable to that of the control group (no extract was added, and the cells were grown in normal cell culture medium), and the cells were healthy spindle or star-shaped, indicating no cytotoxicity.

[0129] (3) Alkaline phosphatase (ALP) assay

[0130] Alkaline phosphatase (ALP) was used to evaluate the osteogenic differentiation of MC3T3-E1 cells by bone hemostatic materials. ALP is a glycoprotein on the cell membrane of osteoblasts and a marker of early osteogenic differentiation.

[0131] Specifically, the ALP activity of MC3T3-E1 of Example 2 and Comparative Example 2 was measured on the 4th day and the 7th day, respectively. Briefly, the cells were lysed with a cell lysis buffer, and the supernatant of the lysis after centrifugation was collected. Then, an alkaline phosphatase detection kit was used for detection. The total protein content was determined using a BCA protein detection kit. The relative ALP activity was normalized to the total protein content and expressed as U / grot.

[0132] Figure 8 The ALP staining optical microscope images and ALP relative activity of MC3T3-E1 cells cultured for 7 days on the samples of Example 2 and Comparative Example 2 are shown, indicating that the sample of Example 8 is conducive to early osteogenic differentiation.

[0133] (4) Alizarin Red S staining

[0134] Alizarin red staining (ARS) was used to further evaluate the effects of the samples of Example 2 and Comparative Example 2 on the mineralization level of osteoblasts MC3T3-E1. Calcium deposition, as a marker of osteoblast maturation, can be enhanced during osteoblast differentiation.

[0135] Specifically, on the 4th and 7th days, the calcium-rich deposition of MC3T3-E1 cells cultured in the sample extracts prepared in Example 2 and Comparative Example 2 was evaluated by Alizarin Red staining. Briefly, the cells were washed three times with PBS and then stained with an Alizarin Red S staining kit for 30 minutes. After PBS washing, the cells were observed under an inverted microscope and photographed. 1 mL of 100 mmol / L hexadecylpyridinium chloride was added to each well, and after incubation at room temperature for 1 hour, the absorbance value was measured at 560 nm.

[0136] The results are as follows Fig. 9As shown, more mineralized nodules were observed in the sample of Example 2. This is consistent with the staining results of the ALP test. These results indicate that the sample of Example 2 can promote the extracellular mineralization of osteoblasts.

[0137] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing three-dimensional layered hydroxyapatite / collagen fibers, comprising the following steps: The gelatin solution, chitosan solution, polyvinyl alcohol solution and metal hydroxide are mixed to obtain a core layer spinning precursor solution; Dispersing a foaming agent into a polyvinyl pyrrolidone solution to obtain a shell spinning precursor solution; the foaming agent is a nanocarbonate and / or nanobicarbonate; Coaxially electrospinning the core layer spinning precursor solution and the shell layer spinning precursor solution to obtain coaxial fibers; cross-linking the coaxial fibers with formaldehyde vapor to obtain cross-linked fibers; The cross-linked fiber is immersed in a phosphoric acid aqueous solution, and the foaming agent in the shell layer of the cross-linked fiber reacts with the phosphoric acid to generate gas, causing the fiber to expand into a three-dimensional structure. After the expansion is complete, the reaction is continued to cause the metal hydroxide in the core layer to react with the phosphoric acid to generate hydroxyapatite. The reacted fiber is removed and freeze-dried to obtain a three-dimensional layered hydroxyapatite fiber. The three-dimensional layered hydroxyapatite fibers are immersed in a collagen solution, taken out, and freeze-dried to obtain the three-dimensional layered hydroxyapatite / collagen fibers.

2. The preparation method according to claim 1, characterized in that The mass concentration of the gelatin solution is 5-20%; The mass concentration of the chitosan solution is 1 to 10%; The mass concentration of the polyvinyl alcohol solution is 1 to 15%; The volume ratio of the gelatin solution, the chitosan solution and the polyvinyl alcohol solution is 1:0.5-1:0.1-1.

3. The preparation method according to claim 1 or 2, characterized in that The metal hydroxide includes one or more of calcium hydroxide, strontium hydroxide and magnesium hydroxide; the mass content of the metal hydroxide in the core layer spinning precursor solution is 1-10%.

4. The preparation method according to claim 1, characterized in that The mass concentration of the polyvinyl pyrrolidone solution is 5-10%.

5. The preparation method according to claim 1 or 4, characterized in that The nano carbonate includes one or more of nano sodium carbonate, nano magnesium carbonate, nano calcium carbonate and nano strontium carbonate; the nano bicarbonate includes nano sodium bicarbonate; and the mass content of the foaming agent in the shell spinning precursor solution is 1-10%.

6. The preparation method according to claim 1, characterized in that The coaxial electrospinning conditions include: a spinning voltage of 15 to 30 kV, a core layer spinning precursor injection speed of 0.3 to 2 mL / h, and a shell layer spinning precursor injection speed of 0.5 to 2 mL / h.

7. The preparation method according to claim 1, characterized in that The mass concentration of the phosphoric acid aqueous solution is 0.5-5%.

8. The preparation method according to claim 1 or 7, characterized in that The temperature of the continued reaction is 40-70° C., and the time is 1-3 hours.

9. The three-dimensional layered hydroxyapatite / collagen fibers prepared by the preparation method according to any one of claims 1 to 8 comprise three-dimensional layered hydroxyapatite fibers and collagen wrapped on the surface of the three-dimensional layered hydroxyapatite fibers; the three-dimensional layered hydroxyapatite fibers comprise a core layer and a shell layer, the core layer being a gelatin-chitosan-polyvinyl alcohol crosslinked product and hydroxyapatite; and the shell layer being polyvinyl pyrrolidone.

10. Use of the three-dimensional layered hydroxyapatite / collagen fibers according to claim 9 in preparing bone repair filling materials.