Coated modified anhydrous lithium hydroxide and preparation method thereof

By covering the polymer layer on the surface of anhydrous lithium hydroxide, the dust and absorption performance problems of lithium hydroxide modified products are solved, and its safety and application range is improved, and efficient carbon dioxide absorption performance is ensured.

CN119016035AActive Publication Date: 2024-11-26HUBEI INST OF AEROSPACE CHEMOTECHNOLOGY
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411140939.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-26
Estimated Expiration
2044-08-20

Smart Images

  • Figure CN119016035A_ABST
    Figure CN119016035A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lithium hydroxide, and particularly discloses coated modified anhydrous lithium hydroxide and a preparation method thereof. Comprising the following steps: weighing an internal matrix and an external coating modifier; the internal matrix is anhydrous lithium hydroxide, and the external coating modifier is one of polyaspartic acid, polyacrylamide or polyacrylic acid; an external coating modifier is dissolved in deionized water, and a coating modifier solution is prepared; coating the matrix by using a coating modifier solution to obtain wet-coated modified anhydrous lithium hydroxide; and drying the wet coated modified anhydrous lithium hydroxide to prepare the coated modified anhydrous lithium hydroxide. The surface of anhydrous lithium hydroxide is coated with a physical coating layer, the operation is simple, the particle hardness can be increased, the dust diffusion caused by collision and friction on the particle surface is effectively reduced, and the problem of dust raising is solved. The content and the absorption performance of the effective absorbent can be ensured, the use safety of the lithium hydroxide absorbent is improved, and the requirements of multiple fields on anhydrous hydroxide products are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium hydroxide, and in particular to coated modified anhydrous lithium hydroxide and a preparation method thereof. Background Art

[0002] Lithium hydroxide is an efficient carbon dioxide absorbent, which has the characteristics of fast carbon dioxide absorption speed, large adsorption capacity per unit mass, and easy handling of reaction products. Since lithium hydroxide is a strong alkaline substance, it is easy to generate corrosive dust during use, which irritates the human body. Therefore, in order to improve and solve the dust problem of lithium hydroxide products, technicians in this field have modified lithium hydroxide. The invention patent CN102020294B discloses dust-free lithium hydroxide monohydrate and its preparation method, and provides an undried dust-free lithium hydroxide monohydrate wet product. Due to its high water content, there is no dust during use, but the product will agglomerate if it is placed for a long time. It is necessary to wrap an anti-caking agent on the surface of lithium hydroxide to prevent agglomeration during long-term storage.

[0003] Invention patents such as CN104163442B and CN102786069B ensure that there is no dust and irritating odor during use by wrapping surfactants on the surface of lithium hydroxide monohydrate. However, lithium hydroxide monohydrate contains crystal water, which reduces the content of effective absorbent lithium hydroxide. The lithium hydroxide content can only reach 55-57%, while reducing the specific surface area of ​​lithium hydroxide.

[0004] Invention patents such as CN112216834B and CN112299452A spray liquid alkanes, alkane derivatives, etc. on the surface of lithium hydroxide and obtain anhydrous lithium hydroxide after drying. Although this method can reduce irritating dust, substances such as alkanes have low boiling points. Due to the exothermic reaction during the absorption process, they may volatilize during the use of the product, and the gas permeability is poor, which reduces the absorption performance and quality of lithium hydroxide.

[0005] In summary, the existing lithium hydroxide has the problems of dust flying and high irritation when used, while the modified product has the problems of high water content, low effective absorbent content, volatilization of modifier, and poor gas permeability. Summary of the invention

[0006] In view of the problems existing in the prior art, an object of the present invention is to provide a method for preparing a coated modified anhydrous lithium hydroxide, which is used to prepare the coated modified anhydrous lithium hydroxide of the present invention. A physical coating layer is coated on the surface of the anhydrous lithium hydroxide, which is simple to operate, can increase the hardness of the particles, effectively reduce the diffusion of dust generated by collision and friction on the particle surface, and solve the dust problem.

[0007] The second purpose of the present invention is to provide a coated modified anhydrous lithium hydroxide, which can not only increase the particle hardness and solve the dust problem, but also ensure the effective absorbent content and absorption performance, improve the safety of lithium hydroxide absorbent, expand the scope of application, improve the performance, and meet the requirements of anhydrous lithium hydroxide treatment products in multiple fields.

[0008] The first technical solution adopted by the present invention is: a method for preparing coated modified anhydrous lithium hydroxide, comprising the following steps:

[0009] Step 1: weighing an internal matrix and an external coating modifier; the internal matrix is ​​anhydrous lithium hydroxide, and the external coating modifier is one of polyaspartic acid, polyacrylamide or polyacrylic acid;

[0010] Step 2: dissolving the external coating modifier in deionized water to prepare a coating modifier solution;

[0011] Step 3: coating the inner matrix with the coating modifier solution to obtain wet-coated modified anhydrous lithium hydroxide;

[0012] Step 4: Drying the wet coated modified anhydrous lithium hydroxide to obtain coated modified anhydrous lithium hydroxide.

[0013] Preferably, the anhydrous lithium hydroxide in step 1 is in granular form.

[0014] Preferably, the molecular weight range of the polyaspartic acid is 2000-20000; the molecular weight range of the polyacrylamide is 20000-100000; and the molecular weight range of the polyacrylic acid is 500-5000.

[0015] Preferably, the mass concentration of the external coating modifier in the coating modifier solution in step 2 is 0.1% to 8%.

[0016] Preferably, the mass ratio of the external coating modifier to the internal matrix is ​​0.1% to 2.0%.

[0017] Preferably, the coating method in step 3 comprises: adding the internal matrix into the coating modifier solution;

[0018] Alternatively, the coating modifier solution is uniformly sprayed on the surface of the inner matrix.

[0019] Preferably, the drying conditions in step 4 are: temperature 90-150° C., time 4-12 h.

[0020] The second technical solution adopted by the present invention is: a coated modified anhydrous lithium hydroxide, comprising an internal matrix and an external coating modifier; the mass ratio of the external coating modifier to the internal matrix is ​​0.1% to 2.0%;

[0021] The internal matrix is ​​anhydrous lithium hydroxide;

[0022] The external coating modifier is one of polyaspartic acid, polyacrylamide or polyacrylic acid.

[0023] Preferably, the molecular weight range of the polyaspartic acid is 2000-20000; the molecular weight range of the polyacrylamide is 20000-100000; and the molecular weight range of the polyacrylic acid is 500-5000.

[0024] Preferably, the molecular weight of the polyaspartic acid is one of 4000, 6000-8000 and 10000-12000; the molecular weight of the polyacrylamide is 20000-100000; and the molecular weight of the polyacrylic acid is one of 1000 and 3000.

[0025] Beneficial effects of the above technical solution:

[0026] (1) The coated modified anhydrous lithium hydroxide provided by the present invention has no crystal water in the molecule, is not easily adsorbed on the tube wall of the device, and is not easy to agglomerate and fail. The number of replacement and cleaning times can be reduced, raw materials are saved, and costs are reduced. In addition, the coated modifier effectively reduces the diffusion of dust generated by collision and friction on the particle surface, solving the dust problem. The modifier content is low, the lithium hydroxide content is high, the specific surface area is large, the absorption performance is good, and the charge amount is low. The coated modified anhydrous lithium hydroxide can basically maintain the carbon dioxide absorption efficiency of the uncoated anhydrous lithium hydroxide, and does not affect the performance of the product.

[0027] (2) The preparation method of the coated modified anhydrous lithium hydroxide provided by the present invention is to coat a physical coating layer on the surface of the anhydrous lithium hydroxide, which is simple to operate, can increase the hardness of the particles, effectively reduce the dust diffusion caused by collision and friction on the particle surface, solve the dust problem, and protect the health of users. The modifier used in the present invention contains active group structures such as amino and carboxyl groups, which have extremely strong chelating, dispersing, and adsorption effects, and is a good coating material. The modifier material is porous and has strong gas permeability, and will not affect the absorption performance of lithium hydroxide. At the same time, the modifier has a high boiling point, is green, non-toxic, and pollution-free, and will not volatilize during the use of the product, avoiding harm to human health. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a static absorption curve of carbon dioxide for the coated modified anhydrous lithium hydroxide provided in Example 1 of the present invention. DETAILED DESCRIPTION

[0029] The following is a further detailed description of the implementation methods of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than an exhaustive list of all the embodiments. It should be noted that the embodiments and features in the embodiments of the present application can be combined with each other without conflict.

[0030] The terms "first", "second", etc. (if any) in the specification and claims are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way are interchangeable where appropriate so that the embodiments described herein can be implemented in an order other than that illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product, or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products, or devices.

[0031] It should be understood that the term "and / or" used in this article is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0032] The polyaspartic acid with a molecular weight of 4000 and 6000-8000 is recorded as polyaspartic acid 4000 and polyaspartic acid 6000-8000 respectively; the polyacrylamide with a molecular weight of 20000-100000 is recorded as polyacrylamide 20000-100000; the polyacrylic acid with a molecular weight of 1000 and 3000 is recorded as polyacrylic acid 1000 and polyacrylic acid 3000 respectively.

[0033] Example 1

[0034] The coated modified anhydrous lithium hydroxide of the present invention comprises an anhydrous lithium hydroxide matrix and an external coating modifier coated on the surface of the anhydrous lithium hydroxide matrix, wherein the material of the external coating modifier is polyaspartic acid 4000.

[0035] The preparation method of the coated modified anhydrous lithium hydroxide of this embodiment comprises the following steps:

[0036] (1) Dissolve polyaspartic acid 4000 in deionized water and stir manually for 3 min to prepare 200 g of a 3% solution;

[0037] (2) Weigh 50 g of anhydrous lithium hydroxide particles, pour into the solution obtained in step (1), shake the container to mix for 10 seconds, and filter to obtain wet particles with a modifier attached to the surface;

[0038] (3) The wet anhydrous lithium hydroxide particles obtained in step (2) are placed in a drying oven for drying (temperature of 140° C., drying time of 12 h) to obtain coated modified anhydrous lithium hydroxide.

[0039] The particle hardness test showed that the average hardness of the coated modified anhydrous lithium hydroxide particles prepared in this embodiment was 20.81N. The carbon dioxide static absorption performance test showed that the carbon dioxide static absorption rate was 65.4% after 20 minutes. During the experiment, there was no dust.

[0040] Example 2

[0041] The invention discloses a coated modified anhydrous lithium hydroxide, an anhydrous lithium hydroxide matrix and a coating modifier coated on the surface of the anhydrous lithium hydroxide matrix, wherein the coating modifier material is polyaspartic acid 4000.

[0042] The preparation method of the coated modified anhydrous lithium hydroxide of this embodiment comprises the following steps:

[0043] (1) Dissolve polyaspartic acid 4000 in deionized water and stir manually for 3 min to prepare 200 g of a 4% solution;

[0044] (2) Weigh 50 g of anhydrous lithium hydroxide particles, pour into the solution obtained in step (1), shake the container to mix for 10 seconds, and filter to obtain wet particles with a modifier attached to the surface;

[0045] (3) The wet anhydrous lithium hydroxide particles obtained in step (2) are placed in a drying oven for drying (temperature of 140° C., drying time of 12 h) to obtain coated modified anhydrous lithium hydroxide.

[0046] The particle hardness test shows that the average hardness of the coated modified anhydrous lithium hydroxide particles prepared in this embodiment is 23.23N; the carbon dioxide static absorption performance test shows that the carbon dioxide static absorption rate is 64.9% after 20 minutes; and there is no dust during the experiment.

[0047] Example 3

[0048] The invention discloses a coated modified anhydrous lithium hydroxide, an anhydrous lithium hydroxide matrix and a coating modifier coated on the surface of the anhydrous lithium hydroxide matrix, wherein the coating modifier material is polyaspartic acid 4000.

[0049] The preparation method of the coated modified anhydrous lithium hydroxide of this embodiment comprises the following steps:

[0050] (1) Dissolve polyaspartic acid 4000 in deionized water and stir manually for 3 min to prepare 200 g of a 5% solution;

[0051] (2) Weigh 50 g of anhydrous lithium hydroxide particles, pour into the solution obtained in step (1), shake the container to mix for 10 seconds, and filter to obtain wet particles with a modifier attached to the surface;

[0052] (3) The wet anhydrous lithium hydroxide particles obtained in step (2) are placed in a drying oven for drying (temperature of 140° C., drying time of 12 h) to obtain coated modified anhydrous lithium hydroxide.

[0053] The particle hardness test shows that the average hardness of the coated modified anhydrous lithium hydroxide particles prepared in this embodiment is 27.63N; the carbon dioxide static absorption performance test shows that the carbon dioxide static absorption rate is 60.2% after 20 minutes; and there is no dust during the experiment.

[0054] Example 4

[0055] The invention discloses a coated modified anhydrous lithium hydroxide, an anhydrous lithium hydroxide matrix and a coating modifier coated on the surface of the anhydrous lithium hydroxide matrix, wherein the coating modifier material is polyaspartic acid 6000-8000.

[0056] The preparation method of the coated modified anhydrous lithium hydroxide of this embodiment comprises the following steps:

[0057] (1) Dissolve polyaspartic acid 6000-8000 in deionized water and stir manually for 3 minutes to prepare 200 g of a 4% solution;

[0058] (2) Weigh 50 g of anhydrous lithium hydroxide particles, pour into the solution obtained in step (1), shake the container to mix for 10 seconds, and filter to obtain wet particles with a modifier attached to the surface;

[0059] (3) The wet anhydrous lithium hydroxide particles obtained in step (2) are placed in a drying oven for drying (temperature of 140° C., drying time of 12 h) to obtain coated modified anhydrous lithium hydroxide.

[0060] The particle hardness test shows that the average hardness of the coated modified anhydrous lithium hydroxide particles prepared in this embodiment is 29.52N; the carbon dioxide static absorption performance test shows that the carbon dioxide static absorption rate is 60.7% after 20 minutes; and there is no dust during the experiment.

[0061] Example 5

[0062] The invention discloses a coated modified anhydrous lithium hydroxide, an anhydrous lithium hydroxide matrix and a coating modifier coated on the surface of the anhydrous lithium hydroxide matrix, wherein the coating modifier material is polyacrylamide 20000-100000.

[0063] The preparation method of the coated modified anhydrous lithium hydroxide of this embodiment comprises the following steps:

[0064] (1) Dissolve polyacrylamide 20000-100000 in deionized water and stir manually for 3 min to prepare 200 g of a 2% solution;

[0065] (2) Weigh 50 g of anhydrous lithium hydroxide particles, pour into the solution obtained in step (1), shake the container to mix for 10 seconds, and filter to obtain wet particles with a modifier attached to the surface;

[0066] (3) The wet anhydrous lithium hydroxide particles obtained in step (2) are placed in a drying oven for drying (temperature of 140° C., drying time of 12 h) to obtain coated modified anhydrous lithium hydroxide.

[0067] The particle hardness test showed that the average hardness of the coated modified anhydrous lithium hydroxide particles prepared in this embodiment was 24.97N. The carbon dioxide static absorption performance test showed that the carbon dioxide static absorption rate was 59.4% after 20 minutes. During the experiment, there was no dust phenomenon.

[0068] Example 6

[0069] The invention discloses a coated modified anhydrous lithium hydroxide, an anhydrous lithium hydroxide matrix and a coating modifier coated on the surface of the anhydrous lithium hydroxide matrix, wherein the coating modifier material is polyacrylic acid 3000.

[0070] The preparation method of the coated modified anhydrous lithium hydroxide of this embodiment comprises the following steps:

[0071] (1) Dissolve polyacrylic acid 3000 in deionized water and stir manually for 3 min to prepare 200 g of a 3% solution;

[0072] (2) Weigh 50 g of anhydrous lithium hydroxide particles, pour into the solution obtained in step (1), shake the container to mix for 10 seconds, and filter to obtain wet particles with a modifier attached to the surface;

[0073] (3) The wet anhydrous lithium hydroxide particles obtained in step (2) are placed in a drying oven for drying (temperature of 140° C., drying time of 12 h) to obtain coated modified anhydrous lithium hydroxide.

[0074] The particle hardness test shows that the average hardness of the coated modified anhydrous lithium hydroxide particles prepared in this embodiment is 28.35N; the carbon dioxide static absorption performance test shows that the carbon dioxide static absorption rate is 59.1% after 20 minutes; and there is no dust during the experiment.

[0075] Example 7

[0076] The invention discloses a coated modified anhydrous lithium hydroxide, an anhydrous lithium hydroxide matrix and a coating modifier coated on the surface of the anhydrous lithium hydroxide matrix, wherein the coating modifier material is polyacrylic acid 1000.

[0077] The preparation method of the coated modified anhydrous lithium hydroxide of this embodiment comprises the following steps:

[0078] (1) Dissolve polyacrylic acid 1000 in deionized water and stir manually for 3 min to prepare 200 g of a 4% solution;

[0079] (2) Weigh 50 g of anhydrous lithium hydroxide particles, pour into the solution obtained in step (1), shake the container to mix for 10 seconds, and filter to obtain wet particles with a modifier attached to the surface;

[0080] (3) The wet anhydrous lithium hydroxide particles obtained in step (2) are placed in a drying oven for drying (temperature of 140° C., drying time of 12 h) to obtain coated modified anhydrous lithium hydroxide.

[0081] The particle hardness test shows that the average hardness of the coated modified anhydrous lithium hydroxide particles prepared in this embodiment is 27.7N; the carbon dioxide static absorption performance test shows that the carbon dioxide static absorption rate is 61.7% after 20 minutes; and there is no dust during the experiment.

[0082] Comparative Example

[0083] The anhydrous lithium hydroxide of this comparative example has no coating modifier, and its preparation method comprises the following steps:

[0084] (1) Weigh 50 g of anhydrous lithium hydroxide particles;

[0085] (2) The anhydrous lithium hydroxide particles obtained in step (1) are placed in a drying oven for drying (temperature of 140° C., drying time of 12 h) to obtain anhydrous lithium hydroxide.

[0086] The particle hardness test showed that the average hardness of the anhydrous lithium hydroxide particles prepared in this comparative example was 15.42N. The carbon dioxide static absorption performance test showed that the carbon dioxide static absorption rate was 68.3% after 20 minutes. During the experiment, dusting was obvious.

[0087] Through the experimental results of Examples 1 to 7 and Comparative Examples, and Figure 1 It can be seen from the static absorption curve of carbon dioxide of the coated modified anhydrous lithium hydroxide provided in Example 1 that the coated modified anhydrous lithium hydroxide provided by the present invention effectively reduces the dust diffusion caused by collision and friction on the particle surface, and solves the dust problem. The modifier content is low, the lithium hydroxide content is high, the specific surface area is large, the absorption performance is good, and the charge amount is low. The coated modified anhydrous lithium hydroxide can basically maintain the carbon dioxide absorption efficiency of the uncoated anhydrous lithium hydroxide without affecting the use performance of the product. The preparation method of the coated modified anhydrous lithium hydroxide provided by the present invention is simple to operate, and the modifier used contains active group structures such as amino and carboxyl groups, which have extremely strong chelating, dispersion, adsorption and other effects, and are very good coating materials. The modifier material has porosity and strong gas permeability, and will not affect the absorption performance of lithium hydroxide. At the same time, the modifier has a high boiling point, is green, non-toxic and pollution-free, and will not volatilize during the use of the product to avoid harm to human health.

[0088] Effect evaluation

[0089] The application effect of coated modified anhydrous lithium hydroxide was evaluated, and the coated modified anhydrous lithium hydroxide was used in a semi-enclosed self-oxygen protective breathing device as a carbon dioxide absorbent produced by human breathing. The dust rate test result of the coated modified anhydrous lithium hydroxide used was 0.8%. After wearing and using the human breathing simulation device for 10 minutes, the maximum carbon dioxide concentration in the device hood was 1.8%. When the uncoated modified anhydrous lithium hydroxide was used, the dust rate test result was 4.7%. After wearing and using the human breathing simulation device for 10 minutes, the maximum carbon dioxide concentration in the device hood was 1.6%. It can be seen that the absorption rate of the anhydrous lithium hydroxide after coating and modification remains basically unchanged, and the dust rate is significantly improved.

[0090] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made on the basis of the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.

Claims

1. A method for preparing coated modified anhydrous lithium hydroxide, characterized in that: The following steps are involved: Step 1: weighing an internal matrix and an external coating modifier; the internal matrix is ​​anhydrous lithium hydroxide, and the external coating modifier is one of polyaspartic acid, polyacrylamide or polyacrylic acid; Step 2: dissolving the external coating modifier in deionized water to prepare a coating modifier solution; Step 3: coating the inner matrix with the coating modifier solution to obtain wet-coated modified anhydrous lithium hydroxide; Step 4: Drying the wet coated modified anhydrous lithium hydroxide to obtain coated modified anhydrous lithium hydroxide.

2. The method for preparing coated modified anhydrous lithium hydroxide according to claim 1, characterized in that: The anhydrous lithium hydroxide described in step 1 is in granular form.

3. The method for preparing coated modified anhydrous lithium hydroxide according to claim 1, characterized in that: The molecular weight range of the polyaspartic acid is 2000-20000; the molecular weight range of the polyacrylamide is 20000-100000; and the molecular weight range of the polyacrylic acid is 500-5000.

4. The method for preparing coated modified anhydrous lithium hydroxide according to claim 1, characterized in that: The mass concentration of the external coating modifier in the coating modifier solution in step 2 is 0.1% to 8%.

5. The method for preparing coated modified anhydrous lithium hydroxide according to claim 1, characterized in that: The mass ratio of the external coating modifier to the internal matrix is ​​0.1% to 2.0%.

6. The method for preparing coated modified anhydrous lithium hydroxide according to claim 1, characterized in that: The coating method in step 3 includes: adding the internal matrix to the coating modifier solution; Alternatively, the coating modifier solution is uniformly sprayed on the surface of the inner matrix.

7. The method for preparing coated modified anhydrous lithium hydroxide according to claim 1, characterized in that: The drying conditions in step 4 are: temperature 90-150° C., time 4-12 hours.

8. A coated modified anhydrous lithium hydroxide prepared by the preparation method according to any one of claims 1 to 8, characterized in that: It comprises an internal matrix and an external coating modifier; the mass ratio of the external coating modifier to the internal matrix is ​​0.1% to 2.0%; The internal matrix is ​​granular anhydrous lithium hydroxide; The external coating modifier is one of polyaspartic acid, polyacrylamide or polyacrylic acid.

9. The coated modified anhydrous lithium hydroxide according to claim 8, characterized in that: The molecular weight range of the polyaspartic acid is 2000-20000; the molecular weight range of the polyacrylamide is 20000-100000; and the molecular weight range of the polyacrylic acid is 500-5000.

10. The coated modified anhydrous lithium hydroxide according to claim 8, characterized in that: The molecular weight of the polyaspartic acid is one of 4000, 6000-8000 and 10000-12000; the molecular weight of the polyacrylamide is 20000-100000; and the molecular weight of the polyacrylic acid is one of 1000 and 3000.

Citation Information

Patent Citations

  • Dust-free grade lithium hydroxide monohydrate and preparation method

    CN104163442A

  • Method for preparing modified anhydrous lithium hydroxide through spray coating

    CN112216834A

  • Coated modified anhydrous lithium hydroxide and preparation method thereof

    CN112299452A

  • Dust-free lithium hydroxide monohydrate as well as preparation method and application thereof

    CN117776226A

  • High-strength lithium hydroxide absorbent and preparation method thereof

    CN118320607A