Heterojunction photocatalyst and preparation method thereof

By combining Al-SrTiO3 and SrNbO3 and introducing RhCrOx and CoOOH cocatalysts, the heterojunction structure is optimized, and the problem of insufficient activity and stability of the photocatalyst under visible light is solved, and efficient photoenergy utilization and water decomposition reactions are achieved.

CN119016114APending Publication Date: 2024-11-26扬州市常发新能源科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411303712.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the catalytic reaction of existing photocatalysts, the photogenerated electron-grade holes are easy to recombinate and the light energy utilization rate is low. In particular, the wide band gap of strontium titanate (SrTiO3) leads to poor absorption of visible light, and intrinsic semiconductor light The photogenerated carrier recombination rate of catalytic materials is high.

Method used

Al-SrTiO3 and SrNbO3 are combined to form a heterojunction photocatalyst, and RhCrOx and CoOOH are introduced as cocatalysts. By optimizing energy band arrangement and local electric field effect, the recombination rate of photogenerated electrons and holes is slowed down, and their separation and transmission are promoted. Improve the activity and stability of the water decomposition reaction.

Benefits of technology

Effectively broaden the light absorption range, improve photocatalytic efficiency, and improve the water decomposition activity and stability of the photocatalyst under visible light, solving the problems of insufficient photocatalyst activity and poor stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016114A_ABST
    Figure CN119016114A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of photocatalytic materials, and particularly provides a heterojunction photocatalyst and a preparation method thereof.The preparation method comprises the steps that an Al source compound is evenly mixed with SrTiO3 and SrCl2 in proportion, heat treatment is conducted at a certain temperature, then a large amount of water is washed, redundant SrCl2 is removed, and Al-SrTiO3 is obtained after drying; the preparation method comprises the following steps: uniformly mixing SrCO3 and Nb2O5 in proportion, and carrying out heat treatment at a certain temperature to obtain a Sr5Nb4O15 precursor; the obtained Al-SrTiO3 and Sr5Nb4O15 precursor and Nb powder are evenly mixed according to a proper molar ratio, the mixture is continuously kept at the temperature for a certain time in the Ar atmosphere, the Al-SrTiO3 / SrNbO3 heterojunction photocatalyst is obtained, RhCrOx and CoOOH are supported as cocatalysts, the molar ratio of the Al-SrTiO3 to the SrNbO3 is (0.5-3): 1, and the prepared photocatalyst can achieve pure water decomposition under visible light and has good catalytic activity and stability; and the preparation method has the characteristics of simple process, mild conditions and low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of photocatalytic materials, and in particular to a heterojunction photocatalyst and a preparation method thereof. Background Art

[0002] With the continuous increase of the world's population and the rapid development of modern industry, energy shortage and environmental pollution are two major problems facing human society today. Semiconductor photocatalysts use light energy to trigger specific redox reactions and play a catalytic role. They have important application prospects in the fields of energy and environmental remediation, such as photocatalytic decomposition of water to produce hydrogen and reduction of CO 2 , degradation of organic pollutants, etc. Finding efficient photocatalysts is a core issue in the field of photocatalysis. 3 ) As an n-type semiconductor with a typical perovskite structure, it has attracted widespread attention due to its high activity, chemical stability and non-toxic properties. However, the problem of low light utilization caused by its wide band gap (about 3.2eV) still needs to be solved. In addition, intrinsic semiconductor photocatalytic materials inevitably have the characteristic of high recombination rate of photogenerated carriers. In order to improve the above problems, researchers have done a lot of work to improve them from the aspects of ion doping, precious metal deposition, and construction of composite materials. The Domen research group at the University of Tokyo in Japan found that a single Al 3+ The introduction of ions can regulate oxygen defects. Although it cannot achieve visible light response, it can greatly enhance its photocatalytic water decomposition activity within the ultraviolet light response range.

[0003] Strontium niobate (SrNbO 3 ) is a kind of electron with degenerate Fermi level and large carrier density (~10 22 cm -3 ) metal oxides, which exhibit strong plasma resonance (LSPR) absorption in the visible light region. Unlike general photocatalytic semiconductor materials, SrNbO 3 The generation of intermediate carriers and the catalytic reaction can occur simultaneously without the need for charge transfer. As the only intrinsic plasma photocatalytic material (IPP) currently developed, the known means to effectively improve its photocatalytic activity are still very limited. Summary of the invention

[0004] In view of this, the present invention proposes a heterojunction photocatalyst and a preparation method thereof, aiming to solve the problems in the prior art that photogenerated electron-level holes in the catalytic reaction of the photocatalyst are easy to recombine and the light energy utilization rate is low.

[0005] The technical solution of the present invention is achieved as follows: The present invention provides a heterojunction photocatalyst, which is composed of Al-SrTiO 3 and SrNbO3 Combination formation, loaded with RhCrO x and CoOOH as co-catalysts.

[0006] In the above embodiments, SrTiO 3 It has good photocatalytic performance, but its band gap is wide (about 3.2 eV), which limits its absorption of visible light. 3 Oxygen defects can be introduced to improve the ultraviolet light response activity, but it still cannot effectively respond to visible light. 3 As a photocatalytic material with plasma resonance effect, it can absorb visible light and generate a strong local electric field inside the material. The combination of the two can effectively broaden the light absorption range and improve the photocatalytic efficiency. The heterojunction structure slows down the recombination rate of photogenerated electrons and holes by optimizing the energy band arrangement, while promoting the separation and transmission of photogenerated carriers. SrNbO 3 The plasmon resonance effect further improves the material's responsiveness to visible light.

[0007] RhO x As an excellent hydrogen evolution reaction (HER) catalyst, it can effectively promote the hydrogen evolution reaction in water decomposition; while CoOOH has good catalytic activity in the oxygen evolution reaction (OER). The synergistic effect of these two co-catalysts can promote the anode and cathode reactions of the water decomposition reaction respectively, thereby improving the overall efficiency of photocatalysis. RhCrO x The introduction of and CoOOH not only improves the utilization efficiency of photogenerated electrons and holes in the photocatalytic reaction, but also further enhances the activity and stability of the heterojunction material in the water decomposition reaction.

[0008] In some embodiments, Al-SrTiO 3 With SrNbO 3 The molar ratio is (0.5-3):1.

[0009] In the above embodiments, the appropriate molar ratio can ensure the structural stability and synergistic effect of the heterojunction material. 3 When the ratio of SrNbO 3 The energy band matching of the photocatalyst is optimal, which promotes the separation and transfer of photogenerated electrons and holes. The appropriate molar ratio can optimize the energy band alignment, further improve the photogenerated carrier separation efficiency of the photocatalyst, reduce the recombination of carriers, and thus improve the photocatalytic activity.

[0010] In some embodiments, RhCrO x and CoOOH loadings are respectively 3 and SrNbO 30.01wt%-0.5wt% of the total molar amount.

[0011] In the above embodiment, an appropriate amount of RhCrO x CoOOH and CoOOH help to improve the activity of the photocatalytic reaction, but too much co-catalyst loading will lead to excessive coverage of the material surface, affecting the absorption of light and the reaction. Controlling the loading of the co-catalyst within an appropriate range can effectively increase the reaction rate, ensure the effective use of photogenerated carriers, and at the same time not hinder the absorption of light by the photocatalytic material.

[0012] In a second aspect, the present invention further provides a method for preparing a heterojunction photocatalyst, comprising the following steps:

[0013] (1) uniformly mixing the aluminum-containing compound and strontium titanate nanoparticles by ball milling for 3-12 hours;

[0014] (2) The mixture obtained in step (1) is mixed with excess SrCl 2 After grinding and mixing, the mixture is transferred to a muffle furnace for heat treatment;

[0015] (3) Wash and dry the sample after heat treatment in step (2) to remove excess SrCl 2 , the obtained product is Al-SrTiO 3 Nanoparticles;

[0016] (4) SrCO 3 With Nb 2 O 5 The nanoparticles are uniformly ball-milled and mixed for 3-12 h;

[0017] (5) The mixture obtained in step (4) is transferred to a muffle furnace for heat treatment to obtain Sr 5 Nb 4 O 15 Precursor powder;

[0018] (6) uniformly mixing the nanoparticles obtained in step (3) and the powder obtained in step (5) with Nb powder by ball milling for 3-12 hours;

[0019] (7) The mixture obtained in step (6) is transferred to a tube furnace and subjected to heat treatment under an Ar atmosphere to obtain Al-SrTiO 3 / SrNbO 3 Heterojunction photocatalyst nanoparticles;

[0020] (8) Loading the nanoparticles obtained in step (7) with RhCrO x and CoOOH to obtain RhCrO x / Al-SrTiO 3 / SrNbO 3 / CoOOH heterojunction photocatalytic materials.

[0021] In some embodiments, the aluminum-containing compound in step (1) is one or a mixture of any of aluminum oxide, aluminum nitrate, aluminum acetate, aluminum carbonate or aluminum chloride.

[0022] In some embodiments, the heat treatment temperature in step (2) is 900-1200° C. and the time is 6-12 hours.

[0023] In some embodiments, the heat treatment temperature in step (5) is 800-1200° C. and the time is 8-15 hours.

[0024] In some embodiments, the heat treatment temperature in step (7) is 1000-1400° C. and the time is 15-30 hours.

[0025] In some embodiments, the Al-SrTiO obtained in step (7) 3 / SrNbO 3 The size of nanoparticles is 200-500 nanometers.

[0026] In some embodiments, in step (8), RhCrO is loaded x Specifically, the steps include: mixing the nanoparticles obtained in step (7) with NaRhCl in a mass ratio of 0.01wt% to 0.5wt% of the nanoparticles obtained in step (7); 6 With Cr(NO 3 ) 3 Evenly ball-mill and mix for 1-3 hours, keep warm at 300-700℃ for 3-6 hours, and the obtained product is RhCrO x / Al-SrTiO 3 / SrNbO 3 Nanoparticles.

[0027] In some embodiments, the step (8) of loading CoOOH specifically comprises the following steps: x / Al-SrTiO 3 / SrNbO 3 Evenly dispersed in water, the obtained RhCrO x / Al-SrTiO 3 / SrNbO 3 The mass ratio is 0.01wt%-0.5wt% Co(NO 3 ) 2 , and then kept under 300W xenon lamp for 1-5 hours, filtered, washed and dried, and the final product was RhCrO x / Al-SrTiO 3 / SrNbO3 / CoOOH nanocomposite photocatalytic materials.

[0028] By rationally designing Al-SrTiO 3 / SrNbO 3 Heterojunction structure and the introduction of RhCrO x With the help of CoOOH as a co-catalyst, the photogenerated electrons and holes were effectively separated and transported, the light energy utilization rate in the photocatalytic reaction was improved, and the problems of insufficient activity and poor stability of photocatalysts in the prior art were solved. This optimized photocatalyst has good water splitting activity and stability under visible light and has broad application prospects.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] The present invention provides an Al-SrTiO 3 / SrNbO 3 Heterojunction photocatalyst and preparation method thereof, the catalyst is La, Al double metal ion co-doped SrTiO 3 , compared with single Al-SrTiO 3 and SrNbO 3 Has a more stable structure; RhCrO prepared by the present invention x / Al-SrTiO 3 / SrNbO 3 / CoOOH heterojunction material can realize pure water decomposition under visible light and has good catalytic activity and stability in photocatalytic reactions. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0032] Figure 1 The Al-SrTiO prepared in Example 1 of the present invention 3 / SrNbO 3 SEM images of

[0033] Figure 2 The Al-SrTiO prepared in Example 2 of the present invention 3 UV-visible absorption spectrum;

[0034] Figure 3 The SrNbO prepared in Example 2 of the present invention 3UV-visible absorption spectrum;

[0035] Figure 4 The Al-SrTiO prepared in Example 2 of the present invention 3 / SrNbO 3 UV-visible absorption spectrum;

[0036] Figure 5 RhCrO prepared in Example 2 of the present invention x / Al-SrTiO 3 / SrNbO 3 / CoOOH and single RhCrO x / Al-SrTiO 3 / CoOOH and RhCrO x / SrNbO 3 / CoOOH photocatalytic water decomposition activity comparison chart. DETAILED DESCRIPTION

[0037] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the embodiments of the present invention belong. If the definitions set forth in this section are contrary to or otherwise inconsistent with the definitions set forth in the patents, patent applications, published patent applications, and other publications incorporated herein by reference, the definitions listed in this section take precedence over the definitions incorporated herein by reference.

[0039] Unless otherwise specified, the methods used in the following examples are all conventional methods. Unless otherwise specified, the materials, reagents and instruments used are all conventional materials, reagents and instruments in the art, and can be obtained by those skilled in the art through commercial channels.

[0040] When an amount, concentration or other value or parameter is expressed as a range, a preferred range or a range defined by a series of upper preferred values ​​and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including the range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described herein, unless otherwise stated, the range is intended to include its end values ​​and all integers and fractions within the range. In the present specification and claims, range definitions can be combined and / or interchanged, and if not otherwise stated, these ranges include all subranges contained therein.

[0041] Example 1

[0042] A kind of Al-SrTiO 3 / SrNbO 3 The preparation method of the heterojunction photocatalyst comprises the following steps:

[0043] Weigh 0.0032 mol of aluminum nitrate and 0.08 mol of SrTiO 3 , mixed and ground in an agate mortar for 1 h, the ground mixture was placed in a ball mill and ball milled at 3000 rpm for 6 h, and then SrCl 2 Continue ball milling for 1 hour. The ball-milled mixture is separated by sieving and placed in a muffle furnace at 900°C for 10 hours. After taking it out, it is filtered and washed with 2L of deionized water, and then the material is placed in a drying oven at 60°C overnight to obtain Al-SrTiO 3 Nanocatalyst material: Take 0.06 mol of SrCO 3 and 0.024 mol Nb 2 O 5 , mixed and ground in an agate mortar for 1 hour, the ground mixture was placed in a ball mill, ball milled at 3000 rpm for 6 hours, the ball milled mixture was sieved and separated, and placed in a muffle furnace and kept at 900 ° C for 10 hours to obtain Sr 5 Nb 4 O 15 Precursor powder; take 0.4 mol of Al-SrTiO 3 Nanocatalyst and 0.02 mol Sr 5 Nb 4 O 15and 0.04 mol of Nb powder, mixed and ground in an agate mortar for 1 h, the ground mixture was placed in a ball mill, ball milled at 3000 speed for 6 h, and placed in a tube furnace, and kept at 1200 ° C for 20 h under Ar atmosphere to obtain Al-SrTiO 3 / SrNbO 3 Nanocatalyst material: 0.5 g Al-SrTiO 3 / SrNbO 3 Nanoparticles, add 2.5 mg of NaRhCl 6 and 2.5 mg of Cr(NO 3 ) 3 , ball milled for 1 hour, calcined at 600°C in air for 3 hours, dispersed in 100 ml of water, and added 2.5 mg Co(NO 3 ) 2 , after irradiation with 300W xenon lamp for 3 hours, filtered, washed and dried to obtain RhCrO x / Al-SrTiO 3 / SrNbO 3 / CoOOH heterojunction photocatalyst.

[0044] Prepare RhCrO x / Al-SrTiO 3 / SrNbO 3 SEM images of the / CoOOH heterojunction photocatalyst Figure 1 As shown, the prepared Al-SrTiO3 / SrNbO3 nanoparticles have a size of 200-500 nanometers.

[0045] Example 2

[0046] A kind of Al-SrTiO 3 / SrNbO 3 The preparation method of the heterojunction photocatalyst comprises the following steps:

[0047] Weigh 0.0032 mol of aluminum nitrate and 0.08 mol of SrTiO 3 , mixed and ground in an agate mortar for 1 h, the ground mixture was placed in a ball mill and ball milled at 3000 rpm for 10 h, and then SrCl 2 Continue ball milling for 1 hour. The ball-milled mixture is separated by sieving and placed in a muffle furnace at 1100°C for 12 hours. After taking it out, it is filtered and washed with 2L of deionized water, and then the material is placed in a drying oven at 60°C overnight to obtain Al-SrTiO 3 Nanocatalyst material: Take 0.1 mol of SrCO 3 and 0.04 mol Nb 2 O5 , mixed and ground in an agate mortar for 1 hour, the ground mixture was placed in a ball mill, ball milled at 3000 rpm for 10 hours, the ball milled mixture was sieved and separated, and placed in a muffle furnace and kept at 900 ° C for 10 hours to obtain Sr 5 Nb 4 O 15 Precursor powder; take 0.4 mol of Al-SrTiO 3 Nanocatalyst and 0.08 mol Sr 5 Nb 4 O 15 and 0.04 mol of Nb powder, mixed and ground in an agate mortar for 1 h, the ground mixture was placed in a ball mill, ball milled at 3000 speed for 6 h, and placed in a tube furnace, and kept at 1300 ° C for 30 h under Ar atmosphere to obtain Al-SrTiO 3 / SrNbO 3 Nanocatalyst material: 0.5 g Al-SrTiO 3 / SrNbO 3 Nanoparticles, add 1.0 mg of NaRhCl 6 and 1.5 mg of Cr(NO 3 ) 3 , ball milled for 3 hours, calcined at 700°C in air for 5 hours, dispersed in 100 ml of water, and added 1.5 mg Co(NO 3 ) 2 , after irradiation with 300W xenon lamp for 4 hours, filtered, washed and dried to obtain RhCrO x / Al-SrTiO 3 / SrNbO 3 / CoOOH heterojunction photocatalyst.

[0048] like Figure 2 , Figure 3 , Figure 4 The Al-SrTiO 3 、SrNbO 3 and Al-SrTiO 3 / SrNbO 3 UV-visible absorption spectrum of Al-SrTiO 3 The absorption edge of SrNbO is 380 nm. 3 It shows obvious plasma resonance absorption peaks in the range of 300-600nm; Al-SrTiO 3 / SrNbO 3 The absorbance range is 250-700nm.

[0049] The RhCrOx / Al-SrTiO 3 / SrNbO 3 / CoOOH heterojunction photocatalyst is used for photocatalytic pure water decomposition. Its photocatalytic water decomposition performance is tested in pure water irradiated with visible spectrum. The catalyst dosage is 100mg, pure water is 100ml, the light source is a 300W xenon lamp, and a 420nm wavelength cutoff filter is configured, which makes the wavelength of the irradiation light source spectrum greater than 420nm, which represents visible light. Figure 3 As shown, RhCrO x / Al-SrTiO 3 / SrNbO 3 The hydrogen evolution rate of the / CoOOH heterojunction photocatalyst is 2358μmol / h / g, the oxygen evolution rate is 1233μmol / h / g, and the hydrogen-oxygen ratio is close to 2:1.

[0050] Example 3

[0051] A kind of Al-SrTiO 3 / SrNbO 3 The preparation method of the heterojunction photocatalyst comprises the following steps:

[0052] Weigh 0.0032 mol of aluminum nitrate and 0.08 mol of SrTiO 3 , mixed and ground in an agate mortar for 1 h, the ground mixture was placed in a ball mill and ball milled at 3000 rpm for 10 h, and then SrCl 2 Continue ball milling for 1 hour. The ball-milled mixture is separated by sieving and placed in a muffle furnace at 1100°C for 12 hours. After taking it out, it is filtered and washed with 2L of deionized water, and then the material is placed in a drying oven at 60°C overnight to obtain Al-SrTiO 3 Nanocatalyst material: Take 0.1 mol of SrCO 3 and 0.04 mol Nb 2 O 5 , mixed and ground in an agate mortar for 1 hour, the ground mixture was placed in a ball mill, ball milled at 3000 rpm for 10 hours, the ball milled mixture was sieved and separated, and placed in a muffle furnace and kept at 900 ° C for 10 hours to obtain Sr 5 Nb 4 O 15 Precursor powder: Take 0.05 mol of Al-SrTiO 3 Nanocatalyst and 0.02 mol Sr 5 Nb 4 O 15and 0.04 mol of Nb powder, mixed and ground in an agate mortar for 1 h, the ground mixture was placed in a ball mill, ball milled at 3000 speed for 6 h, and placed in a tube furnace, and kept at 1300 ° C for 30 h under Ar atmosphere to obtain Al-SrTiO 3 / SrNbO 3 Nanocatalyst material: 0.5 g Al-SrTiO 3 / SrNbO 3 Nanoparticles, add 1.5 mg of NaRhCl 6 and 1.0 mg of Cr(NO 3 ) 3 , ball milled for 3 hours, calcined at 700°C in air for 5 hours, dispersed in 100 ml of water, and added 1.5 mg Co(NO 3 ) 2 , after irradiation with 300W xenon lamp for 4 hours, filtered, washed and dried to obtain RhCrO x / Al-SrTiO 3 / SrNbO 3 / CoOOH heterojunction photocatalyst.

[0053] The RhCrO x / Al-SrTiO 3 / SrNbO 3 / CoOOH heterojunction photocatalyst was used for photocatalytic pure water decomposition. Its photocatalytic water decomposition performance was tested in pure water irradiated with visible spectrum. The catalyst dosage was 100 mg, pure water was 100 ml, the light source was a 300W xenon lamp, and a 420nm wavelength cutoff filter was configured, which made the wavelength of the irradiation light source spectrum greater than 420nm, which represents visible light. x / Al-SrTiO 3 / SrNbO 3 The hydrogen evolution rate of the / CoOOH heterojunction photocatalyst is 2349μmol / h / g, the oxygen evolution rate is 1213μmol / h / g, and the hydrogen-oxygen ratio is close to 2:1.

[0054] Example 4

[0055] A kind of Al-SrTiO 3 / SrNbO 3 The preparation method of the heterojunction photocatalyst comprises the following steps:

[0056] Weigh 0.0032 mol of aluminum nitrate and 0.08 mol of SrTiO 3, mixed and ground in an agate mortar for 1 h, the ground mixture was placed in a ball mill and ball milled at 3000 rpm for 10 h, and then SrCl 2 Continue ball milling for 1 hour. The ball-milled mixture is separated by sieving and placed in a muffle furnace at 1100°C for 12 hours. After taking it out, it is filtered and washed with 2L of deionized water, and then the material is placed in a drying oven at 60°C overnight to obtain Al-SrTiO 3 Nanocatalyst material: Take 0.1 mol of SrCO 3 and 0.04 mol Nb 2 O 5 , mixed and ground in an agate mortar for 1 hour, the ground mixture was placed in a ball mill, ball milled at 3000 rpm for 10 hours, the ball milled mixture was sieved and separated, and placed in a muffle furnace and kept at 900 ° C for 10 hours to obtain Sr 5 Nb 4 O 15 Precursor powder: Take 0.3 mol of Al-SrTiO 3 Nanocatalyst and 0.02 mol Sr 5 Nb 4 O 15 and 0.04 mol of Nb powder, mixed and ground in an agate mortar for 1 h, the ground mixture was placed in a ball mill, ball milled at 3000 speed for 6 h, and placed in a tube furnace, and kept at 1300 ° C for 30 h under Ar atmosphere to obtain Al-SrTiO 3 / SrNbO 3 Nanocatalyst material: 0.5 g Al-SrTiO 3 / SrNbO 3 Nanoparticles, add 0.5 mg of NaRhCl 6 and 0.5 mg of Cr(NO 3 ) 3 , ball milled for 3 hours, calcined at 700°C in air for 5 hours, dispersed in 100 ml of water, and added 1.5 mg Co(NO 3 ) 2 , after irradiation with 300W xenon lamp for 4 hours, filtered, washed and dried to obtain RhCrO x / Al-SrTiO 3 / SrNbO 3 / CoOOH heterojunction photocatalyst.

[0057] The RhCrO x / Al-SrTiO 3 / SrNbO 3 / CoOOH heterojunction photocatalyst was used for photocatalytic pure water decomposition. Its photocatalytic water decomposition performance was tested in pure water irradiated with visible spectrum. The catalyst dosage was 100 mg, pure water was 100 ml, the light source was a 300W xenon lamp, and a 420nm wavelength cutoff filter was configured, which made the wavelength of the irradiation light source spectrum greater than 420nm, which represents visible light. x / Al-SrTiO 3 / SrNbO 3 The hydrogen evolution rate of the / CoOOH heterojunction photocatalyst is 2367μmol / h / g, the oxygen evolution rate is 1226μmol / h / g, and the hydrogen-oxygen ratio is close to 2:1.

[0058] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A heterojunction photocatalyst, It is characterized in that The photocatalyst is Al-SrTiO 3 and SrNbO 3 Combination formation, loaded with RhCrO x and CoOOH as co-catalysts.

2. The heterojunction photocatalyst according to claim 1, It is characterized in that Al-SrTiO 3 With SrNbO 3 The molar ratio is (0.5-3):

1.

3. The heterojunction photocatalyst according to claim 1, It is characterized in that The RhCrO x The loading amounts of MgO and CoOOH were 0.01wt%-0.5wt%, respectively.

4. A method for preparing a heterojunction photocatalyst according to any one of claims 1 to 3, It is characterized in that The steps include: (1) uniformly mixing the aluminum-containing compound and strontium titanate nanoparticles by ball milling; (2) The mixture obtained in step (1) is mixed with excess SrCl 2 After grinding and mixing, the mixture is transferred to a muffle furnace for heat treatment; (3) Wash and dry the sample after heat treatment in step (2) to remove excess SrCl 2 , the obtained product is Al-SrTiO 3 Nanoparticles; (4) SrCO 3 With Nb 2 O 5 Nanoparticles are evenly mixed by ball milling; (5) The mixture obtained in step (4) is transferred to a muffle furnace for heat treatment to obtain Sr 5 Nb 4 O 15 Precursor powder; (6) uniformly mixing the nanoparticles obtained in step (3) and the powder obtained in step (5) with Nb powder by ball milling; (7) The mixture obtained in step (6) is transferred to a tube furnace and subjected to heat treatment under an Ar atmosphere to obtain Al-SrTiO 3 / SrNbO 3 Heterojunction photocatalyst nanoparticles; (8) Loading the nanoparticles obtained in step (7) with RhCrO x and CoOOH to obtain RhCrO x / Al-SrTiO 3 / SrNbO 3 / CoOOH heterojunction photocatalytic materials.

5. The method for preparing the heterojunction photocatalyst according to claim 4, It is characterized in that The aluminum-containing compound described in step (1) is one or a mixture of any of aluminum oxide, aluminum nitrate, aluminum acetate, aluminum carbonate or aluminum chloride.

6. The method for preparing the heterojunction photocatalyst according to claim 4, It is characterized in that In step (2), the heat treatment temperature is 900-1200° C. and the time is 6-12 hours.

7. The method for preparing the heterojunction photocatalyst according to claim 4, It is characterized in that In step (5), the heat treatment temperature is 800-1200° C. and the time is 8-15 hours.

8. The method for preparing the heterojunction photocatalyst according to claim 4, It is characterized in that In step (7), the heat treatment temperature is 1000-1400° C. and the time is 15-30 hours.

9. The method for preparing the heterojunction photocatalyst according to claim 4, It is characterized in that In step (8), RhCrO is loaded x Specifically, the steps include: mixing the nanoparticles obtained in step (7) with NaRhCl in a mass ratio of 0.01wt% to 0.5wt% of the nanoparticles obtained in step (7); 6 With Cr(NO 3 ) 3 Evenly ball-mill and mix, keep warm at 300-700℃ for 3-6 hours, and the obtained product is RhCrO x / Al-SrTiO 3 / SrNbO 3 Nanoparticles.

10. The method for preparing the heterojunction photocatalyst according to claim 9, It is characterized in that The step (8) of loading CoOOH specifically includes the following steps: The obtained RhCrO x / Al-SrTiO 3 / SrNbO 3 Evenly dispersed in water, the obtained RhCrO x / Al-SrTiO 3 / SrNbO 3 The mass ratio is 0.01wt%-0.5wt% Co(NO 3 ) 2 , and then kept under 300W xenon lamp for 1-5 hours, filtered, washed and dried, and the final product was RhCrO x / Al-SrTiO 3 / SrNbO 3 / CoOOH nanocomposite photocatalytic materials.