High-strength microstructure preparation device and microstructure preparation method

By forming a periodic tapered microstructure on the copper interface and using nano-copper paste to sinter interconnect, the problem of insufficient connection strength between nano-copper solder and dielectric material in three-dimensional packaging is solved, and efficient and low-cost copper interface interconnection is achieved. , simplifies the process flow and improves the shear strength.

CN119016881AInactive Publication Date: 2024-11-2610TH RES INST OF CETC

Patent Information

Application Number
CN202411535206.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-31
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The connection strength between nano-copper solder and dielectric material-copper in three-dimensional packaging is insufficient, the traditional process is complex and costly, and cannot meet the high reliability requirements under high temperature conditions.

Method used

Using a high-intensity microstructure preparation device, a femtosecond laser is used to generate an ultra-short pulse beam, and a spot beam is formed through beam shaping and zooming systems, forming a uniform periodic conical microstructure on the copper interface, and sintering is performed using nano-copper slurry. simplify the process flow and reduce costs.

Benefits of technology

It significantly improves the shear strength of the copper interface, breaks through the bottleneck of traditional processes, realizes efficient interconnection under low temperature and low pressure conditions, reduces costs, and does not require pickling, activation, and electroplating steps, simplifying the process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016881A_ABST
    Figure CN119016881A_ABST
Patent Text Reader

Abstract

The invention discloses a high-strength microstructure preparation device and a microstructure preparation method, and belongs to the technical field of electronic packaging interconnection. Femtosecond-magnitude ultrafast pulse light beams generated by a femtosecond laser are utilized to generate Bessel light beams through a light beam shaping unit and a light velocity zooming system; the periodic conical micro-nano structure is prepared on the copper surface by controlling the motion trail of a three-dimensional motion platform, and then two copper interfaces with the periodic conical micro-nano structure are coated with nano copper paste and then sintered to enhance the interconnection effect. The shear strength of the copper interface can be greatly improved, and interconnection is achieved under the low-temperature and low-pressure conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electronic packaging interconnection, and in particular relates to a high-strength microstructure preparation device and a microstructure preparation method. Background Art

[0002] With the rapid development of new generation information technologies such as mobile Internet, microelectronic devices are developing towards integration, miniaturization, multifunctionality and high reliability. Moore's Law, which has lasted for more than half a century, is challenged by the triple limits of physics, power consumption and manufacturing process. In order to meet these challenges, the industry and academia have proposed three-dimensional integration technology - replacing large chips that are taped out at one time with several small chips stacked and packaged for interconnection to replace large chips. As three-dimensional integrated circuits continue to improve integration density and circuit operating speed, the operating temperature of chips is also increasing, so higher requirements are placed on the reliability and service performance of packaging, which in turn leads to some changes in the corresponding interconnection methods and interconnection materials. In recent years, nano copper solder has the ability to resist electromigration, high specific heat capacity, low cost, good thermal and electrical conductivity, and can well meet the reliability requirements of three-dimensional integrated packaging. However, the connection strength between nano copper solder and dielectric material-copper in three-dimensional packaging faces new challenges.

[0003] In recent years, a team from the School of Materials Science and Engineering at Shanghai Jiao Tong University has used chemical deposition methods to grow cone array structures on copper substrates, with the highest shear strength of 45.7 MPa. This method can improve the shear strength of the copper interface compared to traditional processes, but the process is relatively complicated and the cone array structure is difficult to control.

[0004] A team from the Department of Mechanical Engineering at Tsinghua University used ultrafast lasers to deposit thin films of nanoparticles on substrates, saving the bonding process time, but the minimum bonding pressure required was still as high as 20 MPa, which affected the life of the device.

[0005] Wang Haozhe's team used tin-silver-copper eutectic solder to weld on a copper substrate coated with graphene. Through in-situ surface modification, the shear strength reached a maximum of 40MPa, but the effect was still not ideal. Summary of the invention

[0006] The purpose of the present invention is to provide a high-strength microstructure preparation device and a microstructure preparation method to overcome the defects of the prior art, provide means and tools for research in the field of packaging interconnection, and meet the actual needs of scientific research and industrial production.

[0007] The object of the present invention is achieved through the following technical solutions: A high-strength microstructure preparation device, the device is used to prepare an interconnected microstructure of a three-dimensional package copper interface, the device comprising: A laser for generating an ultrashort pulse beam; A beam shaping unit, the beam shaping unit is used to receive and process the ultrashort pulse beam to obtain a shaped laser beam; A motion platform, which is used to control the position of the processed sample; The beam zoom system is used to compress the shaped laser beam into a spot beam and emit it to a specified position above the motion platform.

[0008] On the other hand, the present invention further provides a method for preparing a high-strength microstructure, which is implemented based on the above-mentioned high-strength microstructure preparation device, and the method comprises: An ultrashort pulse beam is generated by a laser, and a shaped laser beam is obtained by a beam shaping unit. The shaped laser beam is compressed into a spot beam by a beam zoom system, and then emitted and focused on the copper surface interface. Manipulate the motion platform to perform mesh scanning on the copper interface; By adjusting the laser processing parameters, a uniform periodic cone microstructure is formed on the copper interface not covered by the mask. The two cone-shaped microstructures to be interconnected are sintered to obtain an interconnected microstructure.

[0009] Furthermore, the method further comprises: The energy, wavelength, power density and pulse width of the ultrashort pulse beam emitted by the laser are set according to the desired interconnected microstructure features.

[0010] Furthermore, the laser processing parameters include one or more of repetition frequency, laser energy, scanning speed and scanning interval.

[0011] Furthermore, before sintering the interconnection, the two cone-shaped microstructures were cleaned with alcohol in an ultrasonic cleaner.

[0012] Furthermore, the sintering interconnection of the two conical microstructures to be interconnected specifically includes: The copper interfaces where the two conical microstructures are located are placed into an alignment mold, the alignment molds are interlocked, and a layer of coated nano-copper slurry is evenly applied between the copper interfaces and then sintered.

[0013] The beneficial effects of the present invention are: (1) The present invention combines ultrafast laser micro-nano manufacturing technology with electronic packaging interconnection technology. First, a regular periodic conical microstructure is formed on the copper surface using ultrafast laser micro-nano manufacturing technology. Then, two ultrafast laser-treated copper surfaces are sintered and interconnected using a coated nano-copper paste to form a better micro-filling-micro-inlay structure, which can greatly improve the shear strength of the copper interface.

[0014] (2) The present invention breaks through the bottleneck of copper interface bonding under the traditional three-dimensional packaging process and greatly improves the shear strength of copper interface interconnection.

[0015] (3) The present invention can realize interconnection under low temperature and low pressure conditions, thus reducing costs, and does not require pickling, activation, or electroplating, and the steps are simple. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 is a structural block diagram of a high-strength microstructure preparation device provided by an embodiment of the present invention; Figure 2 is a schematic diagram of a uniform periodic conical microstructure on a copper surface achieved by an embodiment of the present invention; Figure 3 is a schematic diagram of an embodiment of the present invention after the alignment mold and the processed sample are assembled; Figure 4 It is a schematic diagram of an experimental interconnection process according to an embodiment of the present invention.

[0017] Reference numerals: 1-Femtosecond laser, 2-Beam shaping unit, 3-Beam zoom system, 4-Mask, 5-Processing sample, 6-Three-dimensional motion platform, 7-Alignment mold, 8-Nano copper paste, 9-Copper pillar interface, 10-Carrying substrate. DETAILED DESCRIPTION

[0018] The following describes the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the following embodiments and features in the embodiments can be combined with each other without conflict.

[0019] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative work shall fall within the scope of protection of the present invention.

[0020] A team from the School of Materials Science and Engineering at Shanghai Jiao Tong University has used chemical deposition to grow a cone array structure on a copper substrate with a maximum shear strength of 45.7 MPa. This method can improve the shear strength of the copper interface compared to traditional processes, but the process is relatively complex and the cone array structure is difficult to control.

[0021] A team from the Department of Mechanical Engineering at Tsinghua University used ultrafast lasers to deposit thin films of nanoparticles on substrates, saving the bonding process time, but the minimum bonding pressure required was still as high as 20 MPa, which affected the life of the device.

[0022] Wang Haozhe's team used tin-silver-copper eutectic solder to weld on a copper substrate coated with graphene. Through in-situ surface modification, the shear strength reached a maximum of 40MPa, but the effect was still not ideal.

[0023] In order to solve the above technical problems, the following embodiments of a high-strength microstructure preparation device and a microstructure preparation method of the present invention are proposed.

[0024] Example 1 In order to solve the problem that the copper interface has low shear strength and cannot be used more efficiently under high temperature conditions, this embodiment provides a high-strength microstructure preparation device, referring to Figure 1 ,like Figure 1 The figure shows a structural block diagram of a high-strength microstructure preparation device provided in this embodiment. The device specifically includes a femtosecond laser 1, a beam shaping unit 2, a beam zoom system 3 and a three-dimensional motion platform 6.

[0025] The optical path is as follows: a femtosecond laser 1 generates an ultrashort pulse beam; the beam is processed by a beam shaping unit 2 to obtain a shaped laser beam with a long focal depth and a small diameter; then the beam is compressed into a spot beam by a beam zoom system 3, and the beam is emitted and focused on a processed sample 5 covered by a mask 4, wherein the processed sample 5 is fixed on a three-dimensional motion platform 6.

[0026] Example 2 This embodiment provides a high-strength microstructure preparation method based on the high-strength microstructure preparation device provided in the above embodiment, which specifically includes the following steps: 1) First, the beam of the femtosecond laser is introduced into the optical path through a reflector, and processed by the beam shaping unit to obtain a shaped laser beam with a long focal depth and small diameter. Then, the beam zoom system is used to compress the beam into a spot beam, and the beam is emitted and focused on the processed sample covered by the mask.

[0027] 2) The laser is vertically injected and focused on the copper interface surface. The motion platform is controlled by a computer to scan the copper interface in a "#"-shaped grid.

[0028] 3) By changing different laser processing parameters such as repetition frequency, laser energy, scanning speed, scanning interval and other parameters, a uniform periodic conical micro-nano structure is formed on the copper interface not covered by the mask. Figure 2 ,like Figure 2 Shown is a schematic diagram of the uniform periodic conical microstructure on the copper surface achieved in this embodiment.

[0029] 4) Reference Figure 3 and Figure 4 ,like Figure 3 The figure shows a schematic diagram of the embodiment after the alignment mold and the processed sample are assembled. Figure 4 The figure shows a schematic diagram of an experimental interconnection process of this embodiment. The copper pillar interface 9 with periodic conical micro-nano structures on the surface after two femtosecond laser treatment is first cleaned with alcohol in an ultrasonic cleaning machine for 3 minutes to remove the debris generated by laser processing, and then the sample is placed in the alignment mold 7, the two alignment molds 7 are buckled, and a layer of coated nano copper paste 8 (benzimidazole, copper acetate monohydrate, ascorbic acid, ethylene glycol mixed by centrifugation) is evenly applied between the interfaces and then sintered (sintering temperature 250°C, sintering time 1h, sintering pressure 3MPa), and the supporting substrate 10 is prepared from silicon. This embodiment combines ultrafast laser micro-nano manufacturing technology with electronic packaging interconnection technology. First, a regular periodic conical microstructure is formed on the copper surface using ultrafast laser micro-nano manufacturing technology. Then, two ultrafast laser-treated copper surfaces are sintered and interconnected using coated nano-copper slurry to form a better micro-filling-micro-inlay structure, which can greatly improve the shear strength of the copper interface.

[0030] By combining ultrafast laser micro-nano manufacturing technology with packaging interconnection technology, the two interfaces treated by femtosecond lasers are sintered and interconnected with nano-copper paste, which can greatly improve the shear strength of the copper interface to more than 60 MPa. Compared with the existing welding methods, the method proposed in this embodiment can simply and efficiently achieve the welding performance of the interface.

[0031] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A high-strength microstructure preparation device, characterized in that: The device is used to prepare an interconnected microstructure of a three-dimensional package copper interface, and the device comprises: A laser for generating an ultrashort pulse beam; A beam shaping unit, the beam shaping unit is used to receive and process the ultrashort pulse beam to obtain a shaped laser beam; A motion platform, which is used to control the position of the processed sample; The beam zoom system is used to compress the shaped laser beam into a spot beam and emit it to a specified position above the motion platform.

2. A method for preparing a high-strength microstructure, characterized in that: The method is implemented based on the high-strength microstructure preparation device according to claim 1, and the method comprises: An ultrashort pulse beam is generated by a laser, and a shaped laser beam is obtained by a beam shaping unit. The shaped laser beam is compressed into a spot beam by a beam zoom system, and then emitted and focused on the copper surface interface. Manipulate the motion platform to perform mesh scanning on the copper interface; By adjusting the laser processing parameters, a uniform periodic cone microstructure is formed on the copper interface not covered by the mask. The two cone-shaped microstructures to be interconnected are sintered to obtain an interconnected microstructure.

3. The method for preparing a high-strength microstructure according to claim 2, characterized in that: The method further comprises: The energy, wavelength, power density and pulse width of the ultrashort pulse beam emitted by the laser are set according to the desired interconnected microstructure features.

4. The method for preparing a high-strength microstructure according to claim 2, characterized in that: The laser processing parameters include one or more of repetition frequency, laser energy, scanning speed and scanning interval.

5. The method for preparing a high-strength microstructure according to claim 2, characterized in that: Before sintering the interconnect, the two pyramidal microstructures were cleaned with alcohol in an ultrasonic cleaner.

6. The method for preparing a high-strength microstructure according to claim 2, characterized in that: The sintering interconnection of two conical microstructures to be interconnected specifically comprises: The copper interfaces where the two conical microstructures are located are placed into an alignment mold, the alignment molds are interlocked, and a layer of coated nano-copper slurry is evenly applied between the copper interfaces and then sintered.

Citation Information

Patent Citations

  • Manufacturing method of high-contrast and high-strength high-temperature-resistant grating

    CN105807347A

  • Copper interconnection functional microstructure and preparation method thereof

    CN109473418A

  • Femtosecond laser high-efficiency manufacturing device of infrared anti-reflection microstructure

    CN110014224A

  • Nanometer copper paste for chip pressureless sintering interconnection and preparation method and application thereof

    CN111975011A

  • Microwave assembly pretreatment method based on single-beam laser seal welding

    CN118123236A

Cited By

  • Processing method of maskless tree-shaped silicon nano-structure array and silicon wafer prepared by using maskless tree-shaped silicon nano-structure array

    CN120174379A