Vinasse self-adhesive plate as well as preparation method and application thereof
By crushing the wine lees and adding volatile acids or alkalis for hot pressing, the wine lees are self-adhesive, which solves the problem of adding adhesives to prepare particleboards of wine lees, and environmentally friendly boards that meet national standards are prepared, and solid waste for brewing is realized. Resource utilization.
Patent Information
- Application Number
- CN202411120886.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-15
AI Technical Summary
In the prior art, the preparation of wine lees into particleboard requires adhesives, which leads to unenvironmental problems, and at the same time, winemaking solid waste is difficult to effectively deal with.
The dried lees are crushed and volatile acids or alkalis are added, and the lees are subjected to hot pressing to achieve self-adhesion of the lees, avoiding the use of additional adhesives, and using the viscosity of the remaining protein in the lees for bonding.
A plate with a static curved strength of 12-17.5MPa and an elastic modulus of 1.9-2.5GPa was successfully prepared, which met the national standard requirements and realized the resource utilization of brewing solid waste, without the risk of new waste liquid generation and VOC release.
Smart Images

Figure CN119017500A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of artificial board preparation, and in particular relates to a wine lees self-adhesive board and a preparation method and application thereof. Background Art
[0002] There are three most common ways to process distiller's grains: preparing biogas, feed or fertilizer. However, with the continuous development of brewing technology in recent years, the starch and protein content in distiller's grains after brewing is low, and the use of distiller's grains as raw materials in the fields of biogas, feed or fertilizer has gradually decreased, and the demand for high-value and diversified utilization of distiller's grains has become increasingly prominent.
[0003] Preparing wine lees into boards has become a way to diversify the utilization of wine lees. At present, there are generally two ways to prepare wine lees into boards. One is to wash the wine lees, remove starch sugars, proteins, and inorganic salts, and then stick the remaining materials mainly composed of rice husks together in the way of "Hexiang Board". This method will produce a large amount of wastewater and waste a lot of resources. The second method is to use an additional adhesive to stick all the materials in the wine lees together. For example, patent CN 107116659 A uses adhesive to bond dry wine lees and its solubles to wood shavings, and then paves them to form boards, and then obtains formaldehyde-free composite particleboards through hot pressing. However, the disadvantage of this board is obvious. It is not environmentally friendly due to the use of adhesives. Summary of the invention
[0004] In order to solve the problem that winemaking solid waste lees is difficult to handle, and at the same time solve the problem in the prior art that the lees need to be prepared into particleboard, which is not environmentally friendly and requires the addition of an adhesive, the present invention provides a lees self-adhesive board and a preparation method and application thereof.
[0005] In order to achieve the above application purpose, the technical solution adopted by the present invention is as follows:
[0006] In a first aspect, the present invention provides a method for preparing a wine lees self-adhesive board, comprising the following steps: drying and crushing the wine lees, adding a volatile acid or alkali and mixing, adding or not adding un-crushed wine lees, and hot pressing.
[0007] Wherein, the lees drying temperature is ≤120°C. Preferably, the drying temperature is 80-120°C.
[0008] The moisture content of the dried lees is 0-20%. Preferably, the moisture content of the dried lees is 3-20%.
[0009] Wherein, the particle size of the crushed distiller's grains is ≤800 μm. Preferably, the particle size of the crushed distiller's grains is 100-500 μm.
[0010] Wherein, the total amount of the lees is 100 parts.
[0011] The acid is at least one of formic acid, acetic acid or hydrochloric acid. The base is at least one of triethylamine, dipropylamine, sec-butylamine or pentylamine.
[0012] Wherein, based on 100 parts by weight of the lees, the volatile acid is 5 to 80 parts, and the volatile base is 20 to 150 parts. Preferably, the volatile acid is 5 to 20 parts, and the volatile base is 20 to 50 parts.
[0013] Wherein, the lees is a mixture of crushed and uncrushed lees, and the ratio of crushed and uncrushed lees is 0:10 to 10:0, excluding 0:10. Preferably, the ratio of lees is 3:7 to 10:0. More preferably, the ratio is 5:5 to 7:3.
[0014] Wherein, the hot pressing temperature is 100-190°C. Preferably, the hot pressing temperature is 120-190°C.
[0015] Wherein, the hot pressing pressure is ≥ 0.5 MPa. Preferably, the hot pressing pressure is 2 to 7.5 MPa.
[0016] Wherein, the hot pressing time is 8min to 12h.
[0017] In a second aspect, the present invention provides a wine lees self-adhesive board prepared by the above preparation method.
[0018] In a third aspect, the present invention also provides the use of the above-mentioned wine lees self-adhesive board in the preparation of artificial boards.
[0019] The artificial board is prepared by mixing the above-mentioned wine lees self-adhesive board with traditional particle board and fiberboard.
[0020] Beneficial effects: The present invention utilizes the viscosity of the residual protein in the wine lees to achieve board bonding, combines volatile acid, alkali and hot pressing processes, and successfully prepares boards with a static bending strength of 12 to 17.5 MPa, an elastic modulus of 1.9 to 2.5 GPa, and an internal bonding strength of 0.45 to 0.8 MPa without adding additional adhesives. The board of the present invention fully meets the basic requirements of the national standard GB / T4897.1-7 2015 particleboard P2 type as a particleboard. In addition, the method of the present invention realizes the resource utilization of brewing solid waste, the process of preparing the board does not generate new waste liquid, the board does not introduce new adhesives, and there is no risk of VOC release. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a cross-sectional optical microscope photograph of Example 1;
[0022] Figure 2 This is an optical microscope photograph of the cross section of the blank case. DETAILED DESCRIPTION
[0023] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clear, the present application is further described in detail below in combination with the implementation methods. Unless otherwise defined, all scientific and technological terms used herein have the same meanings as understood by ordinary technicians in the field.
[0024] In a specific embodiment of the present invention, a method for preparing a wine lees self-adhesive board is provided, comprising the following steps: drying and crushing the wine lees, then adding a volatile acid or alkali to mix, then adding or not adding un-crushed wine lees, and hot pressing.
[0025] In the above preparation method, the purpose of drying the lees is to control the moisture content in the lees. Conventional drying equipment including ovens, fluidized bed dryers, rotary dryers, freeze dryers, etc. are used to control the moisture content in the lees to 0-20%, preferably 3-20%, at a temperature not exceeding 120°C. Exceeding 120°C causes some easily decomposable functional groups on the protein to decompose, and the protein no longer has pH responsiveness, which affects subsequent bonding.
[0026] In the above preparation method, the dried vinasse is crushed to increase the bulk density of the vinasse particles. After crushing, the particle size of the vinasse particles is ≤800 μm, preferably 100 to 500 μm.
[0027] In the above preparation method, volatile acid or base is added to the lees for mixed modification in order to give the protein viscosity. The working principle is to use volatile acid or base to adjust the pH of the lees, and under the action of strong ions, the protein is denatured, the molecular chain unfolds, and the viscosity is exhibited. The acid is preferably at least one of formic acid, acetic acid or hydrochloric acid. The base is preferably at least one of triethylamine, dipropylamine, sec-butylamine or pentylamine.
[0028] Wherein, based on 100 parts by weight of the lees, the volatile acid is 5 to 80 parts, and the volatile base is 20 to 150 parts. Preferably, the volatile acid is 5 to 20 parts, and the volatile base is 20 to 50 parts.
[0029] In the above preparation method, after adding the volatile acid or alkali, uncrushed lees can be added. Due to the support of rice husks, the bulk density of the material of uncrushed lees particles is low, and the mechanical properties of the board are not high, but it can also meet the basic requirements. After crushing part of the lees powder, the bulk density of the system can be increased, which is convenient for board forming. However, if the lees powder is completely crushed, there will be problems such as insufficient skeleton structure and reduced strength. Therefore, the ratio of crushed and uncrushed lees is 0:10 to 10:0, excluding 0:10. Preferably, the ratio of lees is 3:7 to 10:0. More preferably, the ratio is 5:5 to 7:3.
[0030] In the above preparation method, the material is put into the mold and shaken before hot pressing to flatten it so as to keep the performance of each part of the board uniform during the subsequent hot pressing. The shaking device used is a flat plate shaker.
[0031] In the above preparation method, the hot pressing parameters are temperature: 100-190°C, pressure ≥0.5MPa, and time 8min-12h. Preferably, the temperature is 120-190°C, and the pressure is 2-7.5MPa.
[0032] In the above preparation method, hot pressing and volatile acid or alkali work together. The working principle is: due to the volatilization of acid and alkali caused by high temperature, protein molecules tend to shrink and entangle, and entangle with other substances such as cellulose, thereby achieving an improvement in the bonding strength between the lees, so that the board has ideal performance. If it is a non-volatile acid or alkali, there will be no contribution to the entanglement, and the strength will deteriorate. Higher temperatures will cause the lees to decompose. The hot pressing time of the present invention is 8min to 12h. In some embodiments of the present invention, the performance of the board is stable at 12h. Continuing to extend the hot pressing time will not improve the performance of the board, and it will waste energy and resources.
[0033] The present invention utilizes the viscosity of the residual protein in the wine lees to achieve board bonding. In this regard, there may be similarities with conventional protein-bonded boards, which affects the innovativeness of the solution. Here, the technical differences between the two solutions are explained in detail.
[0034] The principle of conventional multilayer protein adhesive: the structure of the molecular chain is destroyed under the action of heat, acid, alkali and denaturant, causing the protein to denature and thus produce viscosity. According to the college textbook "Protein Chemistry and Technology" (edited by Mo Chongwen of Chemical Industry Press), the denaturing effect of heat on protein is reflected in the increase of molecular vibration caused by heat, the weakening of various forces within and between protein molecules, the destruction of the original regular and dense protein molecular structure, and the orderly winding and folded polypeptide chains stretching out to form linear molecules. Using strong acid or strong alkali to treat protein is conducive to improving protein viscosity, but strong acid or strong alkali mainly destroys secondary bonds such as salt bonds and ester bonds in proteins, and the secondary structure and tertiary structure of proteins are destroyed and denaturation is caused. Surfactants represented by sodium dodecyl sulfate destroy the hydrophobic interaction within the protein molecules, exposing the hydrophobic side chains originally inside the molecules, weakening the water transport interaction within the molecules, and increasing the water transport interaction between molecules, so that protein molecules aggregate with each other to form larger molecular aggregates. In other words, the traditional single protein adhesive works by opening the folded protein molecular chain, showing stronger viscosity, increasing its contact area with cellulose-based materials (wood, straw, etc.), thereby achieving material bonding. Since there is only a simple van der Waals force between protein adhesives and cellulose-based materials, the bonding effect is not ideal, and it is often necessary to use it in conjunction with substances such as polyacrylamide and zinc oxide.
[0035] For the present invention, in the first step of processing protein (before hot pressing), the technical method used is similar, that is, using acid or alkali to open the folded protein molecular chain and increase its contact with the lees particles. But the difference is that volatile acid or alkali is used. Since the acid or alkali used in the present invention is a volatile acid or alkali, in the second step of hot pressing, these acids or alkalis acting on the protein molecules will volatilize during the processing, so that the secondary structure and tertiary structure of the protein that are destroyed will have a tendency to recover spontaneously (i.e., protein renaturation). During the protein renaturation process, the protein molecular chain will tend to fold regularly. However, since the protein molecules and the lees particles are intertwined at this time, the shrinkage and folding of the protein molecular chain will further strengthen the entanglement between the protein molecules and the lees particles, so that the interaction between the two continues to strengthen, so that the present invention can make the protein molecules have stronger adhesiveness without using other substances, and realize the preparation of lees particle board. That is to say, the purpose of hot pressing in the present invention is not only to bond the lees particles together by high pressure, but also to use high temperature to volatilize the acid or alkali, so that the secondary and tertiary structures of the protein will have a spontaneous recovery trend, so that the protein and the cellulose and other particulate matter in the lees will be further entangled, and the adhesion between molecules will be enhanced, thereby improving the bonding strength of the board. Therefore, the working principle of the self-adhesion of the present invention is completely different from that of the prior art.
[0036] The present invention also provides a wine lees self-adhesive board prepared by the preparation method.
[0037] The above-mentioned board of the present invention as a particleboard fully meets the basic requirements of the national standard GB / T 4897.1-7 2015 particleboard P2 type: static bending strength 12MPa, elastic modulus 1.9GPa, internal bonding strength 0.45MPa.
[0038] Specific examples will be listed below to explain the scheme of the present invention. It will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. Where specific techniques or conditions are not indicated in the examples, the techniques or conditions described in the literature in this area or the product instructions are used. Reagents or instruments used that do not indicate manufacturers are all conventional products that can be obtained commercially.
[0039] The distiller's grains in the embodiment are from Luzhou Laojiao Co., Ltd., and the protein content of the distiller's grains is about 22.88%, the oil content is about 7.88%, the crude fiber content is 47.70%, and the rest is soluble sugar and small and medium molecular esters.
[0040] The thickness of the prepared plates is 6 mm.
[0041] Example 1 Wine lees self-adhesive board
[0042] (1) drying the lees in an oven at 105° C. until the moisture content is 10%;
[0043] (2) crushing the dried lees to a particle size of 100 μm;
[0044] (3) adding 5 parts of acetic acid to 100 parts of crushed vinasse powder, stirring in a blender to mix well, and then pouring into a mold;
[0045] (4) The loaded mold was placed on a flat oscillator to flatten it, and then placed on a hot press at 120°C and 6MPa for 20 minutes to obtain a hot-pressed plate.
[0046] Example 2 Wine lees self-adhesive board
[0047] (1) drying the lees in a fluidized bed dryer at 80° C. until the moisture content is 20%;
[0048] (2) crushing the dried lees to a particle size of 500 μm;
[0049] (3) adding 20 parts of acetic acid to 50 parts of crushed vinasse powder, stirring the mixture with 50 parts of un-crushed vinasse in a blender, and then pouring the mixture into a mold;
[0050] (4) The loaded mold was placed on a flat oscillator to flatten it, and then placed on a hot press at 170°C and 5 MPa for 8 minutes to obtain a hot-pressed plate.
[0051] Example 3 Wine lees self-adhesive board
[0052] (1) drying the lees in an oven at 120° C. until the moisture content is 3%;
[0053] (2) crushing the dried lees to a particle size of 800 μm;
[0054] (3) adding 80 parts of acetic acid to 20 parts of crushed vinasse powder, stirring the mixture with 80 parts of un-crushed vinasse in a blender, and then pouring the mixture into a mold;
[0055] (4) The loaded mold was placed on a flat oscillator to flatten it, and then placed on a hot press at 100°C and 3 MPa for 1 h to obtain a hot-pressed sheet.
[0056] Example 4 Wine lees self-adhesive board
[0057] (1) drying the lees in an oven at 120° C. until the moisture content is 7%;
[0058] (2) crushing the dried lees to a particle size of 300 μm;
[0059] (3) adding 80 parts of triethylamine to 80 parts of crushed vinasse powder, stirring the mixture with 20 parts of un-crushed vinasse in a blender, and then pouring the mixture into a mold;
[0060] (4) The loaded mold was placed on a flat oscillator to flatten it, and then placed on a hot press at 120°C and 0.5 MPa for 12 h to obtain a hot-pressed plate.
[0061] Example 5 Wine lees self-adhesive board
[0062] (1) drying the lees in an oven at 120° C. until the moisture content is 7%;
[0063] (2) crushing the dried lees to a particle size of 300 μm;
[0064] (3) adding 20 parts of triethylamine to 60 parts of crushed vinasse powder, stirring the mixture with 40 parts of uncrushed vinasse in a blender, and then pouring the mixture into a mold;
[0065] (4) The loaded mold was placed on a flat oscillator to flatten it, and then placed on a hot press at 190°C and 7.5 MPa for 1 h to obtain a hot-pressed plate.
[0066] Example 6 Wine lees self-adhesive board
[0067] (1) drying the lees in an oven at 120° C. until the moisture content is 3%;
[0068] (2) crushing the dried lees to a particle size of 300 μm;
[0069] (3) adding 50 parts of triethylamine to 70 parts of crushed vinasse powder, stirring the mixture with 30 parts of uncrushed vinasse in a blender, and then pouring the mixture into a mold;
[0070] (4) The loaded mold was placed on a flat oscillator to flatten it, and then placed on a hot press at 170°C and 4.5 MPa for 3 h to obtain a hot-pressed plate.
[0071] Comparative Example 1
[0072] Compared with Example 1, 100 parts of crushed sake lees were replaced with 100 parts of un-crushed sake lees.
[0073] Comparative Example 2
[0074] Compared with Example 5, the variable is that the hot pressing temperature is increased to 200°C.
[0075] Comparative Example 3
[0076] Compared with Example 6, the variable is that the base used is 5 parts of NaOH.
[0077] Comparative Example 4
[0078] Compared with Example 3, the variable is the use of 100 parts of acetic acid.
[0079] Comparative Example 5
[0080] Compared to Example 1, the variable was that acetic acid was not used.
[0081] Blank example
[0082] Compared with Example 1, the lees were not pulverized and acetic acid was not used.
[0083] Table 1 Materials and parameters of the plates prepared in the examples and comparative examples
[0084]
[0085]
[0086] Experimental Example The mechanical properties of the board were tested according to the method of GB / T 17657-2013, and the results are shown in Table 2. The basic requirements of P2 board are static bending strength 12MPa, elastic modulus 1.9GPa, and internal bonding strength 0.45MPa. Some single properties in the comparative example can meet the standard, but not all three items can be met.
[0087] Table 2 Mechanical properties of the plates prepared in the examples and comparative examples
[0088] sample Static bending strength (MPa) Elastic modulus(GPa) Internal bonding strength (MPa) Example 1 16.30 2.26 0.78 Example 2 14.66 2.13 0.52 Example 3 12.44 1.91 0.48 Example 4 13.45 2.03 0.51 Example 5 17.21 2.33 0.65 Example 6 17.41 2.46 0.76 Comparative Example 1 7.65 1.32 0.37 Comparative Example 2 8.65 3.23 0.28 Comparative Example 3 11.04 1.77 0.46 Comparative Example 4 9.02 1.56 0.42 Comparative Example 5 4.74 0.86 0.22 Blank example 2.11 0.42 ~0.02
Claims
1. A method for preparing a distiller's grains self-adhesive board, characterized in that: The following steps are involved: The lees are dried and crushed, and then a volatile acid or alkali is added and mixed, and un-crushed lees may or may not be added, and hot pressing is performed.
2. The method for preparing the wine lees self-adhesive board according to claim 1, characterized in that: The lees drying temperature is ≤120°C; preferably, the drying temperature is 80-120°C.
3. The method for preparing the wine lees self-adhesive board according to claim 1 or 2, characterized in that: The moisture content of the dried vinasse is 0-20%; preferably, the moisture content of the dried vinasse is 3-20%.
4. The method for preparing the distiller's grains self-adhesive board according to any one of claims 1 to 3, characterized in that: The particle size of the crushed distiller's grains is ≤800 μm; preferably, the particle size of the crushed distiller's grains is 100-500 μm.
5. The method for preparing the distiller's grains self-adhesive board according to any one of claims 1 to 4, characterized in that: The total amount of the lees is 100 parts; the lees is a mixture of crushed and uncrushed lees, and the ratio of crushed and uncrushed lees is 0:10 to 10:0, excluding 0:10; preferably, the ratio of lees is 3:7 to 10:0; more preferably, the ratio is 5:5 to 7:
3.
6. The method for preparing the distiller's grains self-adhesive board according to any one of claims 1 to 5, characterized in that: The acid is at least one of formic acid, acetic acid or hydrochloric acid; the base is at least one of triethylamine, dipropylamine, sec-butylamine or pentylamine.
7. The method for preparing the distiller's grains self-adhesive board according to any one of claims 1 to 6, characterized in that: Based on 100 parts by weight of the lees, the volatile acid is 5 to 80 parts, and the volatile alkali is 20 to 150 parts; preferably, the volatile acid is 5 to 20 parts, and the volatile alkali is 20 to 50 parts.
8. The method for preparing the distiller's grains self-adhesive board according to any one of claims 1 to 7, characterized in that: The hot pressing parameters meet at least one of the following: The hot pressing temperature is 100-190°C; preferably, the hot pressing temperature is 120-190°C; The hot pressing pressure is ≥0.5MPa; preferably, the hot pressing pressure is 2-7.5MPa; The hot pressing time is 8 minutes to 12 hours.
9. Wine lees self-adhesive board prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the wine lees self-adhesive board according to claim 9 in the preparation of artificial boards.
Citation Information
Patent Citations
Method for preparing plant protein / inorganic mineral nano composite material
CN101143965A
Vinasse-based reinforced material for artificial board and vinasse-based non-formaldehyde adhesive prepared from vinasse-based reinforced material
CN103725253A
Technique of manufacturing pressboard from waste distiller's grains
CN1070360A
Formaldehyde-free composite chipboard using DDGS (distillers dried grains with soluble) as core and preparation method thereof
CN107116659A
Preparation method of adhesive-free medium and high density plant fiber board