Na3V2 (PO4) 3 and nitrogen-doped reduced graphene oxide synergistically enhanced Na2Fe0. 6Mn0. 4PO4F material and preparation method thereof
Through nitrogen doping reduction of graphene oxide and Na3V2 (PO4)3, the Na2Fe0.6Mn0.4PO4F material is enhanced in combination, and the problems of poor electrochemical activity and low operating voltage in sodium ion batteries are solved, achieving high performance The sodium ion battery positive electrode material has high operating voltage, high magnification capability and long life performance.
Patent Information
- Application Number
- CN202411203242.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-26
AI Technical Summary
Na2Fe0.6Mn0.4PO4F material has problems with poor electrochemical activity and low operating voltage in sodium ion batteries, and has failed to achieve the highest theoretical specific capacity.
Nitrogen-doped reducing graphene oxide (N-RGO) and Na3V2 (PO4)3 are used to jointly enhance Na2Fe0.6Mn0.4PO4F material, and improve conductivity and ion diffusion performance through modification, and suppress the Jahn-Teller effect.
The sodium ion battery cathode material that achieves high operating voltage, high rate capability and long life performance improves the electrochemical performance and cycling stability of the material.
Smart Images

Figure CN119018873A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of positive electrode materials for sodium ion batteries, and specifically relates to a Na3V2(PO4)3 nitrogen-doped reduced graphene oxide synergistically enhanced Na2Fe 0.6 Mn 0.4 PO4F material and preparation method thereof. Background Art
[0002] The uneven distribution of lithium resources leads to high costs for lithium-ion batteries, limiting their sustained and long-term large-scale applications. Sodium-ion batteries have abundant raw materials, low prices, and are highly compatible with lithium-ion battery technology. They have become one of the most promising battery technologies for the next generation of large-scale energy storage systems, showing broad application prospects. Polyanionic compounds are often used in positive electrode materials for sodium-ion batteries. In addition to their high theoretical specific capacity and price advantages, Na2MnPO4F and Na2FePO4F also have the advantages of high operating voltage and high electrochemical activity, respectively. However, Na2MnPO4F and Na2FePO4F have the major defects of poor electrochemical activity and low operating voltage, respectively. A compromise solution proposed by predecessors is to design and prepare the solid solution material Na2Fe 0.6 Mn 0.4 PO4F. Although this material is low in cost and easy to design and control in structure and morphology during synthesis, has high operating voltage, good cycle stability, and its comprehensive performance can be flexibly controlled by ion doping or substitution, it is still far from reaching the highest theoretical specific capacity and the solid solution product Na2Fe 0.6 Mn 0.4 Relevant research work such as the sodium storage mechanism of PO4F has not yet been carried out.
[0003] Studies have shown that graphene doped with heteroatoms has a great impact on its capacitance performance when used as an electrode material. Graphene needs to be functionalized to adjust its physical and chemical properties. Nitrogen doping, phosphorus doping and boron doping are the main approaches at present. Since the phosphorus doping rate is very low, the electronegativity of the boron-doped material is very small, and nitrogen atoms are doped into graphene. Nitrogen atoms can transfer more positive charges to the carbon atoms adjacent to them, which can effectively improve the conductivity of the material. Many researchers have conducted in-depth research on nitrogen-doped graphene.
[0004] Na3V2(PO4)3 (NVP) is a typical NASICON material, belonging to the R3c space group. V generally has four valence states. In the normal polyanion material NVP, V is trivalent, which is just right for the introduction of Na2Fe 0.6 Mn 0.4 Replacement of Mn in PO4F 3+ , thereby suppressing the Jahn-Teller effect, and if the two Na+ At the same time, a reversible deintercalation reaction occurs, and the theoretical capacity can be as high as 117.6 mAh / g, which is also the case for solid solution material Na2Fe 0.6 Mn 0.4 PO4F theoretical specific capacity is a good supplement.
[0005] For solid solution material Na2Fe 0.6 Mn 0.4 The problems of PO4F, in order to further improve its electrochemical activity, this patent uses nitrogen-doped reduced graphene oxide N-RGO and Na3V2(PO4)3 to synergistically enhance Na2Fe 0.6 Mn 0.4 PO4F solid solution material, modified by N-RGO to improve the conductivity of the solid solution material, using the characteristics of Na3V2(PO4)3 fast ion conductor and the ability to react with Na2Fe 0.6 Mn 0.4 PO4F are mutually doped to improve the ion diffusion performance. Summary of the invention
[0006] Na2Fe 0.6 Mn 0.4 Although PO4F solid solution material is an ideal substitute for Na2MnPO4F and Na2FePO4F, it can solve the major defects of Na2MnPO4F and Na2FePO4F, which are poor electrochemical activity and low working voltage. 0.6 Mn 0.4 The specific capacity of PO4F is far from its highest theoretical specific capacity. To address this problem, this patent design uses nitrogen-doped reduced graphene oxide N-RGO and Na3V2(PO4)3 to synergistically enhance the Na2Fe 0.6 Mn 0.4 The electrochemical properties of PO4F solid solution materials are expected to obtain a N-RGO / Na3V2(PO4)3-Na2Fe with high working voltage, high rate capability and long life performance. 0.6 Mn 0.4 PO4F sodium-ion battery positive electrode material.
[0007] In order to achieve the above object, the present invention adopts the following technical solution:
[0008] A Na3V2(PO4)3 nitrogen-doped reduced graphene oxide synergistically enhanced Na2Fe 0.6 Mn 0.4 The preparation method of PO4F material comprises the following steps:
[0009] 1. N-RGO enhances Na2Fe 0.6 Mn 0.4PO4F composite material preparation
[0010] (1) Weigh 0.02 g, 0.05 g, and 0.1 g of GO respectively and add them into 50 mL of deionized water for ultrasonic dispersion for 30 min, then stir magnetically for 30 min. Then, add 0.2 g, 0.5 g, and 1.0 g of ascorbic acid respectively to the above graphene oxide GO dispersion according to the proportion, stir magnetically for 2-5 h, then add 0.6 g, 1.5 g, and 3.0 g of urea respectively according to the proportion, stir magnetically for 8-12 h, and obtain three N-RGO dispersions, which are recorded as 0.02, 0.05, and 0.1 samples.
[0011] (2) Weigh 0.98 g of manganese acetate tetrahydrate (Mn(CH3COO)2·4H2O), 2.10 g of citric acid monohydrate (C6H8O7·H2O), and 1.67 g of ferrous sulfate heptahydrate (FeSO4·7H2O), add 100 mL of deionized water, stir at room temperature for 2 h, weigh 0.42 g of sodium fluoride (NaF) and 1.20 g of sodium dihydrogen phosphate (NaH2PO4), add the above solution and continue stirring for 2 h, and then add them to the three N-RGO dispersions obtained in the above step (1) to obtain three mixed solutions respectively.
[0012] (3) The three mixed solutions obtained in step (2) were stirred in a water bath at 80°C for 8-10 h until a colloid was formed, and then vacuum dried for 12 h. The dried black substance was preheated at 300°C for 3 h in a tube furnace and calcined at 625°C for 6 h to obtain three N-RGO-enhanced Na2Fe 0.6 Mn 0.4 PO4F materials are recorded as 1-0.02, 1-0.05, and 1-0.1 samples.
[0013] 2. N-RGO / Na3V2(PO4)3 synergistically enhances Na2Fe 0.6 Mn 0.4 PO4F material preparation:
[0014] 0.525 g of citric acid (C6H8O7·H2O), 0.585 g of ammonium metavanadate (NH4VO3) and 1.17 g of disodium hydrogen phosphate dihydrate (NaH2PO4·2H2O) were weighed and dissolved in 50 mL of deionized water in turn. The mixture was stirred magnetically at room temperature for 30 min until a bright yellow aqueous solution was formed. The mixture was then added to the three mixed solutions obtained in step 1 (2) above, stirred continuously for 8-10 h in a water bath at 80 °C until a colloid was formed, and dried in vacuum for 12 h. The dried black substance was preheated at 300 °C for 3 h in a tube furnace and calcined at 625 °C for 6 h to obtain three Na3V2(PO4)3 nitrogen-doped reduced graphene oxide synergistically enhanced Na2Fe 0.6 Mn 0.4 PO4F materials are recorded as samples 1-1-0.02, 1-1-0.05, and 1-1-0.1.
[0015] The inventors' research work shows that Na3V2(PO4)3 nitrogen-doped reduced graphene oxide synergistically enhances the Na2Fe 0.6 Mn 0.4 The main reasons for the improvement of the electrochemical performance of PO4F materials can be summarized into two points:
[0016] (1) Design and synthesize N-RGO materials, and modify Na2Fe with the fast ion conductor Na3V2(PO4)3 having NASICON structure 0.6 Mn 0.4 PO4F, thereby increasing Na2Fe 0.6 Mn 0.4 Electronic conductivity and ion diffusion rate of PO4F.
[0017] (2) By compounding Na3V2(PO4)3, part of the V in Na3V2(PO4)3 replaces Na2Fe 0.6 Mn 0.4 Mn in PO4F reduces the Mn in the reaction process 3+ concentration, preventing structural distortion and inhibiting Na2Fe 0.6 Mn 0.4 The occurrence of Jahn-Teller effect in PO4F material. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] FIG1 is a SEM image of three material samples in an embodiment of the present invention, wherein a is 1-1-0.02, b is 1-1-0.05, and c is 1-1-0.1.
[0019] Figure 2 The infrared spectra of three material samples (1-1-0.02, 1-1-0.05, and 1-1-0.1) in the embodiments of the present invention are shown in FIG.
[0020] Figure 3 These are the cycle performance diagrams of three material samples (1-1-0.02, 1-1-0.05, and 1-1-0.1) in the embodiments of the present invention.
[0021] Figure 4 It is the rate performance diagram of three material samples (1-1-0.02, 1-1-0.05, 1-1-0.1) in the embodiments of the present invention. DETAILED DESCRIPTION
[0022] The present invention is described in detail below in conjunction with the accompanying drawings and embodiments, but the protection scope of the present invention is not limited thereto.
[0023] Na3V2(PO4)3 and nitrogen-doped reduced graphene oxide synergistically enhance Na2Fe as a positive electrode material for sodium-ion batteries 0.6 Mn 0.4 The preparation method of PO4F material comprises the following steps:
[0024] 1. N-RGO enhances Na2Fe 0.6 Mn 0.4 PO4F composite material preparation
[0025] (1) Weigh 0.05 g of GO and add 50 mL of deionized water for ultrasonic dispersion for 30 min, then stir magnetically for 30 min. Then, add 1.0 g of ascorbic acid to the above graphene oxide GO dispersion according to the proportion. After magnetic stirring for 5 h, add 3.0 g of urea according to the proportion. After magnetic stirring for 12 h, N-RGO dispersion was obtained, which was recorded as 0.05 sample.
[0026] (2) Weigh 0.98 g of manganese acetate tetrahydrate (Mn(CH3COO)2·4H2O), 2.10 g of citric acid monohydrate (C6H8O7·H2O), and 1.67 g of ferrous sulfate heptahydrate (FeSO4·7H2O), add 100 mL of deionized water, stir at room temperature for 2 h, weigh 0.42 g of sodium fluoride (NaF) and 1.20 g of sodium dihydrogen phosphate (NaH2PO4), add the above solution and continue stirring for 2 h, then add them to the N-RGO dispersion obtained in the above step (1) to obtain a mixed solution.
[0027] (3) The mixed solution obtained in step (2) was stirred in a water bath at 80°C for 10 h until a colloid was formed, and then vacuum dried for 12 h. The dried black substance was preheated at 300°C for 3 h in a tube furnace and calcined at 625°C for 6 h to obtain N-RGO enhanced Na2Fe 0.6 Mn 0.4 PO4F material, recorded as 1-0.05 sample.
[0028] 2. Na3V2(PO4)3 and nitrogen-doped reduced graphene oxide synergistically enhance Na2Fe 0.6 Mn 0.4 PO4F material preparation:
[0029] 0.525 g of citric acid (C6H8O7·H2O), 0.585 g of ammonium metavanadate (NH4VO3) and 1.17 g of disodium hydrogen phosphate dihydrate (NaH2PO4·2H2O) were weighed and dissolved in 50 mL of deionized water in sequence. The mixture was stirred magnetically at room temperature for 30 min until a bright yellow aqueous solution was formed. The mixture was then added to the mixed solution obtained in step 1 (2) above and stirred continuously for 10 h in a water bath at 80 °C until a colloid was formed. The mixture was vacuum dried for 12 h. The dried black substance was preheated at 300 °C for 3 h in a tube furnace and calcined at 625 °C for 6 h to obtain Na3V2(PO4)3 and nitrogen-doped reduced graphene oxide synergistically enhanced Na2Fe 0.6 Mn 0.4 PO4F material, recorded as 1-1-0.05 sample.
[0030] Figure 1 (a) 1-1-0.02, (b) 1-1-0.05, (c) 1-1-0.1 are SEM images of three materials in the embodiment of the present invention. Figure 1 It can be seen that the materials all show obvious porous structures with large porosity. There are many microsphere particles attached to them. The block agglomerates in the samples are secondary micron-sized agglomerates formed by stacking tiny primary nanoparticles, and the particle size of the primary nanoparticles is only 10-30 nm. Studies have shown that the size of primary particles has a significant effect on the electrochemical activity of the product, especially the smaller size is conducive to reducing the diffusion and transmission distance of sodium ions and improving the utilization rate of active substances.
[0031] Attached Figure 2 The infrared spectra of three material samples (1-1-0.02, 1-1-0.05, 1-1-0.1) in the embodiment of the present invention are shown in the figure below. Figure 2 It can be seen that 3448 cm -1 is the stretching vibration absorption peak of OH in water molecules, 1650 cm -1 is the C=C double bond stretching vibration absorption peak (this peak is caused by the unoxidized C=C in graphite), 1393 cm -1 The IR spectrum analysis shows that the oxygen-containing functional groups in RGO are decreasing, indicating that GO is reduced to RGO. -1 The peak at 2830 cm-1 belongs to the stretching vibration of the CN bond. -1The peaks on the left and right belong to the stretching vibration of the NH bond, which proves that the N element has been successfully incorporated into the material.
[0032] Attached Figure 3 Attached is the cycle performance diagram of three material samples (1-1-0.02, 1-1-0.05, 1-1-0.1) in the embodiment of the present invention. Figure 3 It shows that at a current density of 0.05 C, the initial discharge capacity of the 1-1-0.05 material is 149.27 mAh g -1 After 100 cycles, the discharge capacity can be maintained at 101.89 mAh g -1 It accounts for 68.26% of its initial discharge capacity. It can be seen that the N-RGO / Na3V2(PO4)3 double-modified Na2Fe 0.6 Mn 0.4 PO4F composites showed higher and better Coulombic efficiency.
[0033] Attached Figure 4 The following are rate performance diagrams of three material samples (1-1-0.02, 1-1-0.05, and 1-1-0.1) in the embodiments of the present invention. Figure 4 It can be seen that the three materials showed excellent rate performance during the continuous change of current density. When tested at current densities of 0.05 C, 0.1 C, 0.2 C, 0.5 C, and 1 C, the three materials provided 135.05 mAh·g -1 、114.73 mAh·g -1 、97.62 mAh g -1 The excellent discharge capacity of the three materials was also shown. Moreover, after the current density was cycled back to 0.05C, the three materials were still able to recover to the initial discharge capacity. This also shows that the Na2Fe 0.6 Mn 0.4 PO4F solid solution material has obvious advantages.
Claims
1. Na3V2(PO4)3 and nitrogen-doped reduced graphene oxide synergistically enhance Na2Fe as a positive electrode material for sodium-ion batteries 0.6 Mn 0.4 The preparation method of PO4F material is characterized in that: The following steps are involved: (1) Weigh 0.05 g of graphene oxide GO, add 50 mL of deionized water, ultrasonically disperse for 30 min, and magnetically stir for 30 min to obtain a graphene oxide GO dispersion. Then, add 0.5 g of ascorbic acid to the above graphene oxide GO dispersion, magnetically stir for 2-5 h, and then add 1.5 g of urea. After magnetic stirring for 8-12 h, a reduced graphene oxide N-RGO dispersion is obtained. (2) Weigh 0.98 g of tetrahydrate manganese acetate Mn(CH3COO)2·4H2O, 2.10 g of monohydrate citric acid C6H8O7·H2O, and 1.67 g of heptahydrate ferrous sulfate FeSO4·7H2O, add 100 mL of deionized water, stir at room temperature for 2 h, then add 0.42 g of sodium fluoride NaF and 1.20 g of sodium dihydrogen phosphate NaH2PO4, continue stirring for 2 h, and then add the solution to the reduced graphene oxide N-RGO dispersion obtained in the above step (1) to obtain a mixed solution; (3) Na3V2(PO4)3 and nitrogen-doped reduced graphene oxide synergistically enhance Na2Fe 0.6 Mn 0.4 Preparation of PO4F material: Weigh 0.525 g of citric acid C6H8O7·H2O, 0.585 g of ammonium metavanadate NH4VO3 and 1.17 g of dihydrated sodium hydrogen phosphate NaH2PO4·2H2O and dissolve them in 50 mL of deionized water in turn. Stir magnetically at room temperature for 30 min to form a bright yellow aqueous solution. Then add the bright yellow aqueous solution to the mixed solution obtained in the above step (2). Stir continuously for 8-10 h in a water bath at 80 °C until a colloid is formed. Vacuum dry for 12 h. The dried black substance is placed in a tube furnace for preheating at 300 °C for 3 h and calcined at 625 °C for 6 h to obtain Na3V2(PO4)3 and nitrogen-doped reduced graphene oxide synergistically enhanced Na2Fe 0.6 Mn 0.4 PO4F material.
Citation Information
Patent Citations
Method for preparing sodium ferric manganese fluorophosphate composite positive electrode material
CN109659525A