Ecological concrete for soil slope vegetation restoration and slope protection and greening method thereof

By using ecological concrete and mechanized soil cladding greening methods on soil slopes, the problems of soil erosion and vegetation restoration are solved, the slope stability and ecological landscape are improved, and the ecological environment-friendly engineering protection effect is achieved.

CN119019138APending Publication Date: 2024-11-26CHANGJIANG RIVER SCI RES INST CHANGJIANG WATER RESOURCES COMMISSION
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411169641.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-24
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Soil slopes have problems with soil erosion and vegetation restoration in engineering construction. Traditional protection methods lead to unstable slopes and low vegetation survival rate, which cannot meet the needs of ecological and environmental protection.

Method used

Ecological concrete is used as a restoration material to provide a suitable growth environment by improving the porosity and strength of concrete, and germination and growth of plant grass seeds. Combined with mechanized construction and soil-covered greening methods, slope stability and ecological landscape are improved.

Benefits of technology

It significantly reduces construction costs and technical difficulties, improves the overall stability and ecological landscape of soil slopes, enhances the growth durability of plants, and meets the needs of engineering ecological environment protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019138A_ABST
    Figure CN119019138A_ABST
Patent Text Reader

Abstract

The invention provides ecological concrete for soil slope vegetation recovery and a slope protection and greening method thereof. The ecological concrete is prepared from the following components in parts by weight: 0.35 to 0.45 part by weight of water, 0.4 to 0.7 part by weight of cement, 5.0 to 6.2 parts by weight of coarse aggregate, 0.15 to 0.3 part by weight of fly ash, 0.15 to 0.3 part by weight of blast furnace mineral powder, 0.1 to 0.4 part by weight of ferrous sulfate, 0.02 to 0.045 part by weight of phosphate fertilizer, 0.01 to 0.015 part by weight of bacillus subtilis and 0.007 to 0.015 part by weight of rooting powder. The ecological concrete for soil slope vegetation recovery and the slope protection and greening method thereof can be used for river soil bank slope regulation, river channel desilting and slope treatment, municipal and expressway soil slopes and other projects, the stability and flood discharge capacity of river bank slopes can be improved, the ecological environment can be improved, and the slope protection and greening effects can be improved. And the construction project ecosystem service function is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of soil and water conservation ecological restoration, and in particular to an ecological concrete used for soil slope vegetation restoration and a slope protection and greening method thereof. Background Art

[0002] The ecological protection of soil slopes has long been the focus and difficulty of environmental protection work in construction projects. The mutual constraints between slope stability and ecology are also key scientific issues in the fields of engineering disaster prevention and mitigation, soil and water conservation and ecological restoration. At present, unreasonable protection forms and inadequate vegetation restoration methods for soil slopes in construction projects often lead to serious soil and water loss on the slopes, and even cause geological disasters such as landslides and mud-rock flows. At the same time, soil and water loss takes away the original nutrients of the soil slopes, making vegetation restoration more difficult, which not only affects the final completion acceptance of the project, but also makes the later rectification difficult and the restoration cost high.

[0003] Traditional methods such as artificial grass planting, rigid slope protection, and flexible slope protection have caused serious soil and water loss on the slopes, poor overall stability, high damage rate, and low vegetation survival rate, which can no longer meet the needs of ecological environmental protection for construction projects in the new era. The ecological protection of engineering soil slopes is imminent, and there is an urgent need for an ecological protection technology for engineering soil slopes that can meet the requirements of slope protection stability and have environmentally friendly and ecologically sound characteristics.

[0004] Therefore, the present invention designs an ecological concrete for soil slope vegetation restoration and a slope protection and greening method thereof. This technology will effectively improve the vegetation restoration capacity of soil slopes in construction projects, enhance the ecological landscape, biodiversity, engineering measures and overall stability of soil slopes, effectively ensure project quality, and significantly reduce the construction cost and technical difficulty of project slope protection, which is of great significance to helping the construction of ecological civilization in the new era. Summary of the invention

[0005] The purpose of the present invention is to solve the problems of soil erosion and vegetation restoration on soil slopes during engineering construction, and to propose an ecological protection technology for engineering soil slopes using ecological concrete as a repair material. On the basis of improving the macropores and strength of ecological concrete, the present invention reduces soil erosion on soil slopes, improves the overall stability of the slope, and provides a good living environment for the germination and growth of grass seeds on the slopes, thereby meeting the needs of ecological environmental protection in engineering construction.

[0006] In order to achieve the above-mentioned purpose, the present invention provides an ecological concrete for soil slope vegetation restoration, wherein the components are mixed in the following proportions by weight: 0.35-0.45 weight parts of water, 0.4-0.7 weight parts of cement, 5.0-6.2 weight parts of coarse aggregate, 0.15-0.3 weight parts of fly ash, 0.15-0.3 weight parts of blast furnace slag, 0.1-0.4 weight parts of ferrous sulfate, 0.02-0.045 weight parts of phosphate fertilizer, 0.01-0.015 weight parts of Bacillus subtilis and 0.007-0.015 weight parts of rooting powder.

[0007] Furthermore, the total mass of cement, fly ash and blast furnace slag is 1, and the mass ratio of ferrous sulfate is the ratio of the mass of ferrous sulfate to the total mass of cement, fly ash and blast furnace slag.

[0008] Furthermore, the cement is ordinary Portland cement with grade 425.

[0009] Furthermore, the coarse aggregate is guami stone with a diameter of 5-30 mm.

[0010] Furthermore, the phosphate fertilizer is a general phosphate fertilizer with an effective phosphorus pentoxide content of greater than or equal to 12% and a water-soluble phosphorus content of greater than or equal to 7%.

[0011] A method for slope protection and greening using the above ecological concrete comprises the following steps:

[0012] Step 1: Leveling the soil slope: The original soil slope that needs to be poured with ecological concrete is leveled and rectified by manual or mechanical excavation and filling to form the required plane;

[0013] Step 2, reinforcement of the foot of the earth slope: build a mortar-stone retaining wall at the foot of the earth slope, where part of the retaining wall is buried in the foot of the slope, and a part is reserved for blocking the ecological concrete and covering soil on the slope surface;

[0014] Step 3, mixing of ecological concrete: the mixing of ecological concrete is carried out on site, and the components of ecological concrete are mixed in proportions according to weight: 0.35-0.45 weight parts of water, 0.4-0.7 weight parts of cement, 5.0-6.2 weight parts of coarse aggregate, 0.15-0.3 weight parts of fly ash, 0.15-0.3 weight parts of blast furnace slag, 0.1-0.4 weight parts of ferrous sulfate, 0.02-0.045 weight parts of phosphate fertilizer, 0.01-0.015 weight parts of Bacillus subtilis, 0.007-0.015 weight parts of rooting powder, and the on-site mixing time of ecological concrete is 5-9 minutes;

[0015] Step 4, ecological concrete transportation: the mixed ecological concrete is transported to the construction site;

[0016] Step 5, ecological concrete paving: According to the size of the construction area, ecological concrete paving is carried out manually or mechanically; when paving manually, the surface of the ecological concrete is leveled and compacted with a vibrator; when paving mechanically, an excavator is used for paving and leveling, and the ecological concrete is compacted with an excavator bucket;

[0017] Step 6, ecological concrete curing: ecological concrete is immediately covered and watered for curing after paving;

[0018] Step 7, eco-concrete covering with soil: After the eco-concrete has been covered and watered for 14 days, remove the covering on the eco-concrete and lay 3-5cm of planting soil on the eco-concrete;

[0019] Step 8, sowing grass seeds: sow grass seeds on the ecological concrete planting soil, and the weight of grass seeds per unit area is controlled at 30-50g / m 2 .

[0020] Step 9, covering with soil and greening maintenance: After sowing the grass seeds, cover with 1-2cm thick planting soil, and cover the planting soil with non-woven fabric or sunshade net to retain water and moisture. After covering with non-woven fabric or sunshade net, water in time to ensure sufficient moisture for plant development.

[0021] Furthermore, in step 2, the width×height of the retaining wall is 30×50 cm, wherein 30 cm of the retaining wall is buried in the foot of the slope, and 20 cm is reserved for blocking the ecological concrete and covering soil on the slope surface.

[0022] Furthermore, in step 5, the paving thickness of the ecological concrete is 10-15 cm.

[0023] Furthermore, in step 6, a moisturizing film, geofelt, geotextile or straw mat covering is used to moisturize and maintain the ecological concrete.

[0024] The advantages of the present invention are: the ecological concrete is prepared by water, cement, coarse aggregate, fly ash, blast furnace ore powder, ferrous sulfate, phosphate fertilizer, Bacillus subtilis and rooting powder in a certain proportion, with moderate pH and large porosity, providing a good environment for plant growth and root development. The plant roots freely shuttle in the criss-crossing pores of the ecological concrete, absorb nutrients therein, and after a period of time, the plant roots will penetrate the 10-15cm thick ecological concrete, penetrate into the original soil slope soil to absorb moisture and nutrients in the soil, so that the plant growth is more luxuriant, the plant growth durability is strong, and the ecological concrete layer, the plant root system and the original soil slope are integrated, and the overall stability of the soil slope is enhanced. The on-site paving and soil covering of the ecological concrete can be mechanized, with a short construction period, low labor cost, and a moderate comprehensive unit price of the construction cost. The ecological concrete for soil slope vegetation restoration and the slope protection and greening method provided by the present invention can be used for river soil bank slope improvement, river dredging and slope management, municipal and highway soil slope and other projects, which can improve the stability and flood discharge capacity of river bank slopes, improve the ecological environment, and enhance the ecosystem service function of construction projects. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic diagram of the ecological concrete after mixing in the present invention.

[0026] Figure 2 It is a partial cross-sectional schematic diagram of the ecological concrete slope protection after greening in the present invention.

[0027] Figure 3 This is a diagram of the growth and root development of Bermuda grass plants in the ecological concrete indoor vegetation experiment in Example 1 of the present invention.

[0028] Figure 4 This is a diagram of the growth and root development of Bermuda grass plants in the ecological concrete indoor vegetation test in Example 2 of the present invention.

[0029] Figure 5 This is a diagram of the growth and root development of Bermuda grass plants in the ecological concrete indoor vegetation experiment in Example 3 of the present invention.

[0030] The reference numerals in the figures are described as follows: 1. coarse aggregate; 2. a mixture of water, cement, fly ash, blast furnace slag, ferrous sulfate, phosphate fertilizer, Bacillus subtilis and rooting powder; 3. plants; 4. covered planting soil; 5. ecological concrete; 6. plant roots penetrating the ecological concrete; 7. original soil slope; 8. a mortar-made stone retaining wall reinforced at the toe of the soil slope. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] Embodiment 1:

[0033] An ecological concrete for soil slope vegetation restoration, the preparation process of which is as follows:

[0034] 0.35 parts by weight of water, 0.4 parts by weight of cement, 5.5 parts by weight of coarse aggregate, 0.3 parts by weight of fly ash, 0.3 parts by weight of blast furnace powder, 0.2 parts by weight of ferrous sulfate, 0.02 parts by weight of phosphate fertilizer, 0.012 parts by weight of Bacillus subtilis and 0.008 parts by weight of rooting powder are mixed and stirred evenly to make standard parts of 150mm×150cm×150cm (length×width×height). After 28 days of curing, the unconfined compressive strength reaches 8.8MPa and the permeability coefficient is 0.178m / s. When the ecological concrete blocks are soaked in distilled water for 28 days, the pH value of the aqueous solution is 8.5. Cover with planting soil and sow Cynodon dactylon seeds. After 60 days, the plant departure rate is 56% and the maximum plant height is 43.4cm. Example 1 Ecological concrete indoor vegetation test Cynodon dactylon plant growth and root development as shown Figure 3 shown.

[0035] Embodiment 2:

[0036] An ecological concrete for soil slope vegetation restoration, the preparation process of which is as follows:

[0037] 0.4 weight parts of water, 0.5 weight parts of cement, 6 weight parts of coarse aggregate, 0.2 weight parts of fly ash, 0.3 weight parts of blast furnace powder, 0.3 weight parts of ferrous sulfate, 0.03 weight parts of phosphate fertilizer, 0.01 weight parts of Bacillus subtilis, and 0.01 weight parts of rooting powder were mixed and stirred evenly to make standard parts of 150mm×150cm×150cm (length×width×height). After curing for 28 days, its unconfined compressive strength reached 7.2MPa and permeability coefficient was 0.19m / s. When the ecological concrete block was soaked in distilled water for 28 days, the pH of the aqueous solution was 8.1. Covering with planting soil and sowing Bermuda grass seeds, the plant departure rate was 62% after 60 days, and the maximum plant height was 51.3cm.

[0038] Example 2 Eco-concrete Indoor Planting Test Bermudagrass Plant Growth and Root Development Figure 4 shown.

[0039] Embodiment 3:

[0040] An ecological concrete for soil slope vegetation restoration, the preparation process of which is as follows:

[0041] 0.45 parts by weight of water, 0.6 parts by weight of cement, 6.2 parts by weight of coarse aggregate, 0.2 parts by weight of fly ash, 0.2 parts by weight of blast furnace slag, 0.4 parts by weight of ferrous sulfate, 0.04 parts by weight of phosphate fertilizer, 0.011 parts by weight of Bacillus subtilis and 0.012 parts by weight of rooting powder are mixed and stirred evenly to make standard parts of 150mm×150cm×150cm (length×width×height). After 28 days of curing, the unconfined compressive strength reaches 6.8MPa and the permeability coefficient is 0.206m / s. When the ecological concrete blocks are soaked in distilled water for 28 days, the pH value of the aqueous solution is 7.7. Cover with planting soil and sow Cynodon dactylon seeds. After 60 days, the plant departure rate is 74% and the maximum plant height is 47.5cm. Example 3 Ecological concrete indoor vegetation test Cynodon dactylon plant growth and root development are as follows Figure 5 shown.

[0042] The embodiment of the present invention further provides a method for slope protection and greening using the above-mentioned ecological concrete, comprising the following steps:

[0043] Step 1: Leveling the soil slope. The original soil slope that needs to be poured with ecological concrete is leveled and renovated by manual or mechanical excavation and filling to create the required plane. When leveling the site, it is necessary to consider meeting the requirements of construction technology, transportation and site drainage, and minimize the amount of soil transport and repeated excavation;

[0044] Step 2: Strengthen the foot of the earth slope. Build a mortar-stone retaining wall at the foot of the earth slope. The size of the retaining wall is generally 30×50cm (width×height), of which 30cm of the retaining wall is buried in the foot of the slope, and 20cm is reserved for the ecological concrete and covering soil on the slope surface.

[0045] Step 3, mixing of ecological concrete. The mixing of ecological concrete is carried out on site. The weight proportions of the components of ecological concrete are as follows: 0.35-0.45 weight parts of water, 0.4-0.7 weight parts of cement, 5.0-6.2 weight parts of coarse aggregate, 0.15-0.3 weight parts of fly ash, 0.15-0.3 weight parts of blast furnace slag, 0.1-0.4 weight parts of ferrous sulfate, 0.02-0.045 weight parts of phosphate fertilizer, 0.01-0.015 weight parts of Bacillus subtilis, 0.007-0.015 weight parts of rooting powder. The mixing time of ecological concrete on site is 5-9 minutes. The structure of ecological concrete after mixing is as follows: Figure 1 shown.

[0046] Step 4: Transport of eco-concrete. The mixed eco-concrete should be transported to the construction site in a timely manner. The tank should be kept clean during transportation to avoid bumps and concrete segregation during loading and unloading.

[0047] Step 5: Spreading ecological concrete. Depending on the size of the construction area, ecological concrete can be spread manually or mechanically. When spreading manually, the surface of the ecological concrete needs to be leveled manually, and the ecological concrete needs to be compacted with a vibrator; when spreading mechanically, an excavator can be used for spreading and leveling, and the ecological concrete can be compacted with an excavator bucket. The thickness of the ecological concrete spread is 10-15cm;

[0048] Step 6, ecological concrete curing. Ecological concrete should be covered and watered immediately after paving. Use moisturizing membrane, geofelt, geotextile, straw mat and other covering materials to maintain the ecological concrete. In areas with large temperature differences between day and night, ecological concrete should be maintained with thermal insulation to ensure that the concrete surface is always moist. In the early stage of ecological concrete curing, people, animals and vehicles are strictly prohibited from passing through. If necessary, a temporary bridge can be built. Traffic can be opened only when the strength is sufficient.

[0049] Step 7, ecological concrete covered with soil. After the ecological concrete has been covered and watered for 14 days, the covering on the ecological concrete is removed and 3-5 cm of planting soil is laid on the ecological concrete. This can be done manually or mechanically.

[0050] Step 8: Sowing grass seeds. Sow grass seeds on the planting soil laid on the ecological concrete. The plant species should be selected from local plant species according to the construction environment. Shrubs and grass can be used together. The weight of grass seeds per unit area is generally controlled at 30-50g / m 2 .

[0051] Step 9, cover with soil and maintain greening. After sowing the grass seeds, add 1-2cm of planting soil, and cover the planting soil with non-woven fabric or sunshade net to retain water and moisture. After covering with non-woven fabric or sunshade net, water should be applied in time to ensure sufficient water for plant development. Figure 2 shown.

[0052] Among them, the coarse aggregate used in the ecological concrete provides a large-pore environment for plant germination and growth. Based on the nutrients provided by the upper 1-2cm planting soil and the lower 3-5cm planting soil laid on the ecological concrete, plant grass seeds have the conditions for rooting and germination. When the plant roots pass through the large pores inside the ecological concrete, penetrate the ecological concrete layer, and take root in the original soil slope, the plant has strong durability in the later growth, and the ecological concrete layer, plant roots and original soil slope are integrated, and the overall stability of the soil slope is enhanced.

[0053] Compared with ordinary concrete, the ecological concrete uses less cement. Cement is a strong alkaline material. Reducing the amount of cement can reduce the alkalinity of concrete and provide a weak alkaline environment for plant growth. At the same time, cement is a gelling material that will block pores after reacting with water. Reducing the amount of cement can increase the porosity of concrete.

[0054] The ferrous sulfate used in the ecological concrete is a plant fertilizer, also known as iron fertilizer, which promotes the formation of plant chlorophyll and can prevent and treat chlorosis caused by iron deficiency in flowers and trees. At the same time, the ferrous sulfate can reduce the alkalinity of concrete and react chemically with calcium hydroxide and aluminum hydroxide, the main components of ordinary Portland cement, to generate ferric hydroxide with weaker alkalinity than calcium hydroxide and aluminum hydroxide.

[0055] Among them, the main component of the phosphate fertilizer used in the ecological concrete is phosphorus pentoxide, which generates phosphoric acid after dissolving in water, which can further reduce the alkalinity of the concrete and react chemically with calcium hydroxide and aluminum hydroxide, the main components of ordinary Portland cement, to generate calcium phosphate and aluminum phosphate.

[0056] Among them, the Bacillus subtilis used in the ecological concrete is a microbial agent that can secrete antibacterial substances and inhibit the growth of pathogens, which can activate the soil, improve fertility, and promote plant rooting and germination. At the same time, the rooting powder used in the ecological concrete can further promote plant rooting and germination.

[0057] Among them, the ecological concrete paving and soil covering greening in the soil slope protection and greening construction method can be mechanized in combination with the project area, with a short construction period, low labor cost and moderate comprehensive unit price of construction cost.

[0058] The present invention is based on the characteristics of engineering soil slopes, and ecological concrete is mixed and spread on site. After the ecological concrete is cured to a certain strength, a layer of planting soil is laid, and grass seeds are sown, so that the growth and survival of plants are good. The construction processes such as mixing, spreading, and spreading planting soil of ecological concrete can be mechanized. Therefore, ecological concrete protection not only improves the overall stability of the soil slope, but also provides a plant growth environment, which belongs to the ecological environment friendly slope protection engineering measures.

[0059] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. An ecological concrete for soil slope vegetation restoration, characterized by: The components are mixed in the following proportions by weight: 0.35-0.45 parts by weight of water, 0.4-0.7 parts by weight of cement, 5.0-6.2 parts by weight of coarse aggregate, 0.15-0.3 parts by weight of fly ash, 0.15-0.3 parts by weight of blast furnace slag, 0.1-0.4 parts by weight of ferrous sulfate, 0.02-0.045 parts by weight of phosphate fertilizer, 0.01-0.015 parts by weight of Bacillus subtilis, and 0.007-0.015 parts by weight of rooting powder.

2. The ecological concrete for soil slope vegetation restoration according to claim 1, characterized in that: The cement is ordinary Portland cement with the label number 425.

3. The ecological concrete for soil slope vegetation restoration according to claim 1, characterized in that: The coarse aggregate is 5-30 mm guami stone.

4. The ecological concrete for soil slope vegetation restoration according to claim 1, characterized in that: The phosphate fertilizer is a general phosphate fertilizer with an effective phosphorus pentoxide content of greater than or equal to 12% and a water-soluble phosphorus content of greater than or equal to 7%.

5. A method for slope protection and greening using ecological concrete, characterized in that: The steps include: Step 1: Leveling the soil slope: The original soil slope that needs to be poured with ecological concrete is leveled and rectified by manual or mechanical excavation and filling to form the required plane; Step 2, reinforcement of the foot of the earth slope: build a mortar-stone retaining wall at the foot of the earth slope, where part of the retaining wall is buried in the foot of the slope, and a part is reserved for blocking the ecological concrete and covering soil on the slope surface; Step 3, mixing of ecological concrete: the mixing of ecological concrete is carried out on site, and the components of ecological concrete are mixed in proportions according to weight: 0.35-0.45 weight parts of water, 0.4-0.7 weight parts of cement, 5.0-6.2 weight parts of coarse aggregate, 0.15-0.3 weight parts of fly ash, 0.15-0.3 weight parts of blast furnace slag, 0.1-0.4 weight parts of ferrous sulfate, 0.02-0.045 weight parts of phosphate fertilizer, 0.01-0.015 weight parts of Bacillus subtilis, 0.007-0.015 weight parts of rooting powder, and the on-site mixing time of ecological concrete is 5-9 minutes; Step 4, ecological concrete transportation: the mixed ecological concrete is transported to the construction site; Step 5, ecological concrete paving: According to the size of the construction area, ecological concrete paving is carried out manually or mechanically; when paving manually, the surface of the ecological concrete is leveled and compacted with a vibrator; when paving mechanically, an excavator is used for paving and leveling, and the ecological concrete is compacted with an excavator bucket; Step 6, ecological concrete curing: ecological concrete is immediately covered and watered for curing after paving; Step 7, eco-concrete covering with soil: After the eco-concrete has been covered and watered for 14 days, remove the covering on the eco-concrete and lay 3-5cm of planting soil on the eco-concrete; Step 8, sowing grass seeds: sow grass seeds on the ecological concrete planting soil, and the weight of grass seeds per unit area is controlled at 30-50g / m 2 . Step 9, covering with soil and greening maintenance: After sowing the grass seeds, cover with 1-2cm thick planting soil, and cover the planting soil with non-woven fabric or sunshade net to retain water and moisture. After covering with non-woven fabric or sunshade net, water in time to ensure sufficient moisture for plant development.

6. The method according to claim 5, characterized in that: The width×height of the retaining wall in step 2 is 30×50 cm, wherein 30 cm of the retaining wall is buried in the foot of the slope, and 20 cm is reserved for blocking the ecological concrete and covering soil on the slope surface.

7. The method according to claim 5, characterized in that: The thickness of the ecological concrete paving in step 5 is 10-15 cm.

8. The method according to claim 5, characterized in that: In step 6, a moisturizing film, geofelt, geotextile or straw mat covering is used to moisturize and maintain the ecological concrete.

Citation Information

Patent Citations

  • Construction method of ecological greening concrete cast-in-place protection slope

    CN110258447A

  • Porous ecological concrete and preparation process thereof

    CN115700231A

  • Ecological slope protection construction method

    CN117211305A