Method for recovering iodide in perovskite solar cell

Through ultrasonic oscillation and acid solvent washing combined with sublimator temperature control, the problems of iodide recovery efficiency and crystallization morphology control in perovskite solar cells are solved, high-purity and high-efficiency iodide recovery are achieved, and pertitanium is improved Photoelectric conversion efficiency of mineral solar cells.

CN119019288APending Publication Date: 2024-11-26ZHEJIANG IRIDIUM TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411134725.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently and at low cost to recover high-quality iodides in perovskite solar cells, and it is difficult to control its crystalline form, affecting the photoelectric conversion efficiency.

Method used

Use ultrasonic oscillation to treat waste perovskite solar cells in organic solvents, combine acidic solvent washing and temperature control in sublimator, separate and collect high-purity lead iodide and formicamidine iodide, and accurately control the temperature and collection section settings. Ensure that the crystalline morphology of lead iodide meets the requirements of perovskite films.

Benefits of technology

High efficiency recovery of high-purity iodide is achieved, ensuring high purity and suitable crystalline morphology of lead iodide and formicamidine, and improving the photoelectric conversion efficiency and film stability of perovskite solar cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019288A_ABST
    Figure CN119019288A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of new energy materials, and discloses a method for recovering iodide in a perovskite solar cell, which comprises the following steps: soaking a waste perovskite solar cell in a solvent, and carrying out ultrasonic oscillation for a certain time to obtain slurry 1; taking out the glass substrate from the ultrasonic oscillator, and washing residual substances on the surface with a detergent to obtain slurry 2; mixing and filtering the slurry 1 and the slurry 2 to obtain filter residues, washing and drying the filter residues, putting the filter residues into a sublimation instrument, and pumping the quartz tube to high vacuum by using a vacuum pump; slowly raising the temperature of each temperature zone of the sublimation instrument, keeping the temperature for a certain time, and collecting iodomethylamine or iodoformamidine; after the temperature of each temperature zone is reduced to the room temperature, slowly raising the temperature of the raw material section of the lead iodide, and setting the temperature of each collection section according to a certain gradient to obtain lead iodide with various morphologies; and after vacuum breaking, lead iodide is collected in a partitioned manner according to the collection temperature. And the recovered lead iodide is high in purity, and the crystal form and the grain size can be regulated and controlled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of new energy materials and relates to a method for recovering iodide in perovskite solar cells. Background Art

[0002] Halide perovskite materials (structural formula ABX3, where A is a monovalent cation such as methylamine (MA), formamidine (FA) or Cs, B is a divalent metal cation such as Pb, Sn, and X is a halogen anion such as Cl, I, Br) have been widely used in optoelectronic devices such as solar cells, photodetectors and light-emitting diodes due to their excellent photoelectric properties. At present, the industrialization of halide perovskite materials in the field of photovoltaic power generation has begun to take shape, and GW-level production lines will be built in the next few years, which will inevitably greatly increase the demand for lead and iodine resources. Among them, iodine resources account for most of the raw material costs of the perovskite light-absorbing layer. Therefore, high-efficiency, high-quality and low-cost recycling of halogen materials in perovskite solar cells is an important path for the sustainable development of perovskite solar cells in the future.

[0003] The recovery of iodide from perovskite solar cells is mainly carried out in the form of lead iodide and iodoformamidine respectively; as the most important raw materials for preparing the perovskite light-absorbing layer, they play a decisive role in the photoelectric conversion efficiency of perovskite photovoltaic modules. First, if there are more impurities in lead iodide and iodoformamidine, they will directly enter the perovskite precursor solution, causing defects in the prepared perovskite film. Secondly, the crystal form of the raw materials can directly affect the final morphology of the perovskite film, and its grain size, crystal orientation, crystallinity, etc. all affect the stability and film quality of the perovskite film. Therefore, it is urgent to develop a method that can effectively recover halides in perovskite solar cells. Summary of the invention

[0004] The purpose of the present invention is to provide a method for efficiently recovering iodide from waste perovskite photovoltaics, so as to achieve the purpose of high purity and controllable crystal morphology of the recovered iodide, while meeting the requirement of high efficiency of perovskite solar cells prepared with the recovered iodide.

[0005] The present invention adopts the following technical solution:

[0006] A method for recovering iodide in a perovskite solar cell comprises the following steps:

[0007] (1) soaking the discarded iodide perovskite solar cells in a solvent and subjecting them to ultrasonic vibration for a certain period of time to obtain a slurry 1, wherein the solvent is one or more of chloroform and chlorobenzene;

[0008] (2) taking the glass substrate obtained in step (1) out of the ultrasonic oscillator, washing the residual substances on the surface with a detergent to obtain slurry 2, wherein the detergent is one of dilute sulfuric acid, dilute hydrochloric acid, hydroiodic acid, hydrobromic acid, hydrofluoric acid, and dilute acetic acid;

[0009] (3) Slurry 1 and slurry 2 are mixed and filtered, and the obtained filter residue is washed and dried and placed in a sublimator, and the quartz tube is evacuated to a high vacuum using a vacuum pump;

[0010] (4) slowly raising the temperature of each temperature zone of the sublimator and keeping it warm for a certain period of time, while the temperature of the collecting section is not raised, and iodoformamidine or iodomethylamine is obtained in the collecting section;

[0011] (5) After the temperature of each temperature zone is lowered to room temperature and iodoformamidine or iodomethylamine is taken out, the temperature of the raw material section is slowly increased, and the temperature of each collection section is set according to a certain gradient to obtain lead iodide with various morphologies;

[0012] (6) After breaking the vacuum, collect the lead iodide in different areas according to the collection temperature.

[0013] Preferably, in step (2), the concentration of the detergent is 5% to 35%, the solid content during washing is 0.125 to 0.5 g / ml, and the washing stirring time is 1 to 4 hours.

[0014] Preferably, in step (3), the drying temperature is 70° C. to 100° C., and drying is performed using a blast dryer or a double cone dryer.

[0015] Preferably, in step (4), the heating rate is 1 to 3°C / min, the insulation temperature is 180°C to 230°C, and the insulation time is 1 to 12 hours.

[0016] Preferably, in step (5), the temperature of the raw material section is increased to 370°C to 450°C, the heating rate is 5 to 10°C / min, and the holding time is 8 to 24 hours.

[0017] Preferably, in step (5), 2 to 5 collection sections are set, the collection temperature of the first section is 320°C to 350°C, the collection temperature of the second section is 280°C to 300°C, the collection temperature of the third section is 200°C to 250°C, the collection temperature of the fourth section is 150°C to 180°C, and the collection temperature of the fifth section is 40°C to 70°C.

[0018] Preferably, in step (6), the temperature during vacuum breaking is from room temperature to 40° C., and the gas used for vacuum breaking is one of nitrogen and argon.

[0019] The benefits and technical principles of the present invention are as follows:

[0020] One benefit of the present invention is that it can efficiently recycle lead iodide and iodoformamidine in perovskite solar cells, and its technical principle is: by ultrasonic oscillation in an organic solvent, all except a dense inorganic electron transport layer (such as tin dioxide) can be detached from the glass substrate, and the organic hole transport layer will dissolve in chloroform and chlorobenzene, and iodide is insoluble therein; then by washing the substrate with an acidic solvent, the residual iodide can be completely rinsed, and the hydroxylation reaction of lead iodide during the washing process is prevented, thereby improving the recovery efficiency. Then, by accurately controlling the temperature of the recovered product in the sublimator, ultra-high purity lead iodide and iodoformamidine are finally obtained. It should be noted that at a relatively low temperature (180-230°C), the volatile organic matter (iodoformamidine or iodomethylamine) in the recovered product is collected first; at a relatively high temperature, lead iodide will sublime first (370-410°C), while impurities that are difficult to sublime (such as a small amount of lead sulfate, calcium, silver, gold, etc.) remain in the raw material area of ​​the sublimator and are separated. Finally, lead iodide and iodoformamidine with higher purity are obtained.

[0021] Another benefit of the present invention is that it can accurately control the crystal morphology of lead iodide: the crystallinity and morphology of lead iodide currently produced industrially or prepared by traditional methods may not meet the special requirements of perovskite solar cells; for example, under high humidity conditions, lead iodide is required to have large grains and crystallize in the horizontal direction, which can resist the erosion of water vapor on the film at the microscopic level. However, by controlling the lead iodide deposition temperature during the sublimation process, the present method can effectively control the grain size, crystal growth direction, crystallinity strength, etc. of lead iodide to meet the various requirements of various perovskite film preparation methods. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 : JV curves of perovskite solar cells prepared using the lead iodide and iodoformamidine recovered in Example 1 and purchased iodoformamidine and lead iodide;

[0023] Figure 2 : Microscopic morphology of the lead iodide powder obtained in the collection section 1 of Example 2;

[0024] Figure 3 : Microscopic morphology of the lead iodide powder obtained in collection section 5 of Example 2;

[0025] Figure 4 : Example 2 Collection of X-ray diffraction pattern of lead iodide powder obtained in Section 1;

[0026] Figure 5 : Example 2 Collection section 5 obtained the X-ray diffraction spectrum of the lead iodide powder. DETAILED DESCRIPTION

[0027] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention, rather than to limit the present invention.

[0028] Embodiment 1:

[0029] The discarded carboxamidine iodine-based perovskite solar cell was immersed in chlorobenzene for ultrasonic vibration for 4 hours to obtain slurry 1. The glass substrate was removed from the ultrasonic oscillator and the residual material on the surface was washed with dilute sulfuric acid to obtain slurry 2. Slurry 1 and slurry 2 were added to a beaker, stirred and mixed, and then filtered, and then the filter residue was dried at 100°C for 3 hours with a blower dryer to obtain a recovered crude product. After the recovered crude product was placed in a sublimator and evacuated to high vacuum, the raw material temperature was set to 180°C, the heating rate was 1°C / min, and the temperature was kept for 3 hours. The collection section was not heated; after each temperature section cooled to room temperature, all the products of the collection section were taken out. Then the temperature of the raw material section was set to 400°C, the collection temperature was set to 200°C, and the heating rate was 5°C / min. After the lead iodide in the raw material section was completely sublimated, heating was stopped. After cooling to room temperature, nitrogen was used to break the vacuum and collect the lead iodide.

[0030] A total of 1520 g of iodomethane and 2190 g of lead iodide were collected; a small amount of residue was found in the raw material area, which was detected to be lead sulfate, lead oxide and a small amount of other metal ions.

[0031] The impurity content and purity of the obtained iodoformamidine and lead iodide are shown in Table 1. It can be clearly seen that the purity of the recovered lead iodide and iodoformamidine is very high, reaching the 5N level. Lead iodide and iodoformamidine are prepared into a perovskite precursor solution in a certain ratio using a mixed solvent of N,N-dimethylimidazole and dimethyl sulfoxide (N,N-dimethylimidazole: dimethyl sulfoxide = 9:1, 1.8 mol / L), and then coated into a perovskite film, and a perovskite solar cell is prepared. The obtained perovskite solar cell efficiency and cell performance parameters are shown in Figure 1 As shown, the efficiency of perovskite solar cells reached 23.5%, which is comparable to the efficiency of solar cells prepared with purchased iodoformamidine and lead iodide (23.0%).

[0032] Table 1 Impurity content and purity of iodoformamidine and lead iodide in Example 1

[0033]

[0034] Embodiment 2:

[0035] The present embodiment is an improvement of the embodiment 1. A total of 2200 g of lead iodide obtained in the embodiment 1 is placed in a sublimator. The temperature of the raw material section is set to 450°C, the collection temperature of the first section is 350°C, the collection temperature of the second section is 300°C, the collection temperature of the third section is 250°C, the collection temperature of the fourth section is 150°C, the collection temperature of the fifth section is 40°C, and the heating rate is 5°C / min. When the lead iodide in the raw material section is completely sublimated, the heating is stopped, and after cooling to room temperature, the vacuum is broken with nitrogen, and the lead iodide is collected in sections. 1968 g of lead iodide is obtained in the first section of the collection area, 93 g of lead iodide is obtained in the second section, 50 g of lead iodide is obtained in the third section, 9 g of lead iodide is obtained in the fourth section, and 1 g of lead iodide is obtained in the fifth section. After ICP detection, the purity reaches 99.9992%. The scanning electron microscope images of the powders in the first section and the fifth section of the collection area are shown as follows. Figure 2 , 3, X-ray diffraction peaks as shown Figure 4 As shown in Figure 5, it was found that the morphology and crystallization properties of the obtained lead iodide powder were significantly changed, and it can be used to customize different types of high-purity lead iodide powders.

Claims

1. A method for recovering iodide from perovskite solar cells, characterized in that: The following steps are involved: (1) soaking the discarded iodide perovskite solar cells in a solvent and subjecting them to ultrasonic vibration for a certain period of time to obtain a slurry 1, wherein the solvent is one or more of chloroform and chlorobenzene; (2) taking the glass substrate obtained in step (1) out of the ultrasonic oscillator, washing the residual substances on the surface with a detergent to obtain slurry 2, wherein the detergent is one of dilute sulfuric acid, dilute hydrochloric acid, hydroiodic acid, hydrobromic acid, hydrofluoric acid, and dilute acetic acid; (3) Slurry 1 and slurry 2 are mixed and filtered, and the obtained filter residue is washed and dried and placed in a sublimator, and the quartz tube is evacuated to a high vacuum using a vacuum pump; (4) slowly raising the temperature of each temperature zone of the sublimator and keeping it warm for a certain period of time, while the temperature of the collecting section is not raised, and iodoformamidine or iodomethylamine is obtained in the collecting section; (5) After the temperature of each temperature zone is lowered to room temperature and iodoformamidine or iodomethylamine is taken out, the temperature of the raw material section is slowly increased, and the temperature of each collection section is set according to a certain gradient to obtain lead iodide with various morphologies; (6) After breaking the vacuum, collect the lead iodide in different areas according to the collection temperature.

2. The method for recovering iodide in perovskite solar cells according to claim 1, characterized in that: In step (2), the concentration of the detergent is 5% to 35%, the solid content during washing is 0.125 to 0.5 g / ml, and the washing stirring time is 1 to 4 hours.

3. The method for recovering iodide in perovskite solar cells according to claim 1, characterized in that: In step (3), the drying temperature is 70° C. to 100° C., and the drying is performed using a blast dryer or a double cone dryer.

4. The method for recovering iodide in perovskite solar cells according to claim 1, characterized in that: In step (4), the heating rate is 1 to 3°C / min, the insulation temperature is 180°C to 230°C, and the insulation time is 1 to 12 hours.

5. The method for recovering iodide in perovskite solar cells according to claim 1, characterized in that: In step (5), the temperature of the raw material section is increased to 370°C to 450°C, the heating rate is 5 to 10°C / min, and the insulation time is 8 to 24 hours.

6. The method for recovering iodide in perovskite solar cells according to claim 1, characterized in that: In step (5), 2 to 5 collection sections are set, the collection temperature of the first section is 320°C to 350°C, the collection temperature of the second section is 280°C to 300°C, the collection temperature of the third section is 200°C to 250°C, the collection temperature of the fourth section is 150°C to 180°C, and the collection temperature of the fifth section is 40°C to 70°C.

7. The method for recovering iodide in perovskite solar cells according to claim 1, characterized in that: In step (6), the temperature during vacuum breaking is from room temperature to 40° C., and the gas used for vacuum breaking is one of nitrogen and argon.